Catalyst for electrochemical hydrogenation of aromatic compound and preparation method thereof

By loading Pt2+ and Ru2+ metal ions onto a carbon support and adjusting the pH for high-temperature reduction, a uniformly distributed alloy particle catalyst was prepared. This solved the problem of uneven agglomeration of existing catalyst particles, improved the electrochemical hydrogenation efficiency of aromatic compounds, and reduced costs.

CN118976485APending Publication Date: 2024-11-19SHAANXI HYDROGEN ENERGY TECH CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411058759.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-02
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

Existing aromatic compound electrochemical hydrogenation catalysts suffer from problems such as large particle size, difficulty in controlling particle size, uneven distribution, and easy agglomeration and accumulation, resulting in low hydrogenation efficiency and high cost.

Method used

By loading Pt2+ and Ru2+ metal ions onto a carbon support, adjusting the pH to 9–11.5, and carrying out a high-temperature reduction reaction, uniformly distributed alloy particles are formed, avoiding agglomeration. This simplifies the preparation method and shortens the preparation time.

Benefits of technology

This technology enables highly efficient electrochemical hydrogenation of catalysts, improves the hydrogenation efficiency of aromatic compounds, reduces the loading of precious metals, lowers costs, and expands the range of applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118976485A_ABST
    Figure CN118976485A_ABST
Patent Text Reader

Abstract

The invention provides a catalyst for electrochemical hydrogenation of aromatic compounds and a preparation method thereof, and the preparation method comprises the following steps: adding a carbon carrier into a proper amount of a reducing agent, carrying out ultrasonic dispersion, and continuously adding a salt solution containing Pt < 2 + > and Ru < 2 + > metal ions to form a dispersion system; after the pH of the dispersion system is adjusted to 9-11.5, the dispersion system is transferred to an oil bath pan at 140-220 DEG C for a high-temperature reduction reaction, metal ions in the dispersion system are reduced by a reducing agent, and formed alloy particles are uniformly loaded on the carbon carrier; and adding a reduction solution obtained by the reduction reaction into excessive deionized water, stirring for 1-2 hours, and filtering to obtain the catalyst for electrochemical hydrogenation of the aromatic compound. By simplifying the preparation steps and accurately controlling the preparation parameters, the preparation time is effectively shortened, the prepared catalyst nanoparticles are uniform in distribution and controllable in size, the problems of agglomeration and accumulation are avoided, and the intrinsic activity of the catalyst and the electrochemical hydrogenation efficiency of aromatic compounds are greatly improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of electrochemical technology, and in particular to a catalyst for electrochemical hydrogenation of aromatic compounds and a preparation method thereof. Background Art

[0002] Hydrogen energy, as a green and low-carbon energy source, has attracted widespread attention. Among various hydrogen storage methods, organic liquid hydrogen storage (LOHC) technology is considered to be an effective technology for long-distance and large-scale hydrogen storage due to its advantages such as high hydrogen storage density, long storage time, and safe transportation process. The principle of organic liquid hydrogen storage is to reversibly react olefins, alkynes, carbocyclic aromatic hydrocarbons, and aromatic compounds with conjugated structures with hydrogen under the action of a catalyst. On the one hand, hydrogen is stored in unsaturated aromatic compounds, and on the other hand, hydrogen in hydrogen-rich organic liquids can be released through dehydrogenation reactions, while producing unsaturated aromatic compounds, and the aromatic compounds can be recycled. At present, conventional unsaturated aromatic compounds are hydrogenated by thermochemical methods, but their energy consumption is high. Since electrochemical hydrogenation has a lower reaction energy barrier and milder reaction conditions (room temperature and normal pressure), electrochemical hydrogenation is more concerned.

[0003] At present, the catalysts used for electrochemical hydrogenation mainly include nickel-based catalysts, palladium and platinum-based catalysts, ruthenium-based catalysts, etc. However, the catalysts currently prepared have large particle sizes and the particle size is difficult to control, resulting in uneven distribution of precious metals on the carrier, and even agglomeration and accumulation problems, which reduces the electrochemical hydrogenation efficiency of aromatic compounds. Summary of the invention

[0004] To solve the above problems, the present application provides a catalyst for electrochemical hydrogenation of aromatic compounds and a preparation method thereof. By simplifying the preparation steps and accurately controlling the preparation parameters, the preparation time is effectively shortened, and the prepared catalyst nanoparticles are evenly distributed and have controllable sizes, avoiding the problems of agglomeration and accumulation, greatly improving the intrinsic activity of the catalyst, and thus improving the efficiency of electrochemical hydrogenation of aromatic compounds.

[0005] In a first aspect, the present application provides a method for preparing a catalyst for electrochemical hydrogenation of aromatic compounds, the preparation method comprising:

[0006] Step S1: add a carbon carrier to an appropriate amount of reducing agent, disperse it by ultrasonic, and then add a 2+ And Ru 2+ A salt solution of metal ions forms a dispersed system;

[0007] Step S2, after adjusting the pH of the dispersed system to 9-11.5, transferring to an oil bath at 140°C-220°C for high-temperature reduction reaction, the metal ions in the dispersed system are reduced by the reducing agent, and the formed alloy particles are uniformly loaded on the carbon carrier;

[0008] Step S3, adding the reducing solution obtained by the reduction reaction into excess deionized water, stirring for 1 h to 2 h and then filtering to obtain the catalyst for electrochemical hydrogenation of aromatic compounds.

[0009] Optionally, adjusting the pH value of the dispersed system to 9-11.5 comprises: slowly adding a NaOH solution having a concentration of 1 mol / L to 5 mol / L into the dispersed system, and stirring at 400 rpm to 600 rpm for 0.5 h to 1.5 h until the pH value of the dispersed system reaches 9-11.5.

[0010] Optionally, a peristaltic pump is used to control the NaOH solution to be slowly added into the dispersion system;

[0011] The peristaltic pump pumps 0.01% to 0.1% of the total volume of the dispersed system per minute.

[0012] Optionally, the reducing agent includes: one of ethylene glycol, propylene glycol, triethylene glycol, oleylamine or oleic acid.

[0013] Optionally, in the dispersed system, the Pt 2+ Metal ions and the Ru 2+ The mass ratio of metal ions is 1:6 to 4:1.

[0014] Optionally, the reduction reaction is carried out for 0.5 h to 1.5 h; and the volume of the deionized water is greater than or equal to 10 times the volume of the reducing solution.

[0015] In a second aspect, the present application provides a catalyst obtained by the preparation method provided in the first aspect, wherein the particle size of the alloy particles is 2 nm to 3 nm.

[0016] Optionally, in the catalyst, the alloy particles account for 35% to 45% of the total mass of the catalyst.

[0017] In a third aspect, the present application provides an application of the catalyst provided in the second aspect, wherein the catalyst is used in an electrochemical hydrogenation reaction of aromatic compounds.

[0018] Optionally, the aromatic compound includes one or more of toluene, dibenzyltoluene, N-ethylcarbazole, benzyltoluene, 3-methylindole, 7-methylindole, cyclopentylpyrazine, carbazole, N-methylindole, N-ethylindole, pyrazine, 2,3-dimethylpyrazine, 2,5-dimethylpyrazine, 2-methylpyrazine, pyridazine, pyridine and 3-methylpyridine.

[0019] In summary, the present application includes at least one of the following beneficial technical effects:

[0020] 1. The present application provides a method for preparing a catalyst for electrochemical hydrogenation of aromatic compounds, wherein a carbon carrier is added to a reducing agent, and then a salt solution of two noble metal ions is added, and the noble metal ions are loaded on the carbon carrier by high-temperature reduction to prepare a catalyst for electrochemical hydrogenation of aromatic compounds. The preparation method is simple, the reaction conditions are mild, and the gas phase reduction-calcination operation is omitted, effectively shortening the preparation time. And by controlling the pH of the reduction process, the reducing agent reduces the noble metal ions in an alkaline environment, achieving controllable alloy particle size, avoiding agglomeration or accumulation, and further improving the catalytic effect of the catalyst, thereby improving the hydrogenation efficiency during catalytic hydrogenation of aromatic compounds.

[0021] 2. The catalyst obtained by the preparation method provided in the present application has a low precious metal loading; the catalyst provided in the present application is used in the electrochemical hydrogenation reaction of aromatic compounds, and can achieve a high electrochemical hydrogenation effect, and has good performance in both H-type electrolyzers and PEM electrolyzers, and the catalyst provided in the present application can be applied to the electrochemical hydrogenation of various liquid unsaturated aromatic compounds, indicating that the catalyst provided in the present application has a wide range of applications. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the description of the embodiments of the present application will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0023] Figure 1 It is a process flow chart of a method for preparing a catalyst for electrochemical hydrogenation of aromatic compounds proposed in an embodiment of the present application;

[0024] Figure 2 is the X-ray diffraction pattern of the catalyst in Example 4 of the present application;

[0025] Figure 3 is a transmission electron microscope image (a) of the catalyst in Example 4 of the present application;

[0026] Figure 4 is a transmission electron microscope image of the catalyst in Example 4 of the present application (b);

[0027] Figure 5 This is a gas chromatogram of toluene hydrogenation products tested in a three-electrode H-type electrolyzer using the catalyst proposed in Example 3 of the present application;

[0028] Figure 6 This is a gas chromatogram of toluene hydrogenation products tested in a three-electrode H-type electrolyzer using the catalyst proposed in Example 4 of the present application;

[0029] Figure 7 This is a gas chromatogram of toluene hydrogenation products tested in a three-electrode H-type electrolyzer using a commercial PtRu / C-60% catalyst proposed in Comparative Example 3 of the present application;

[0030] Figure 8 This is a gas chromatogram of toluene hydrogenation products tested in a three-electrode H-type electrolyzer using the catalyst proposed in Comparative Example 1 of the present application;

[0031] Fig. 9 This is a gas chromatogram of toluene hydrogenation products tested in a three-electrode H-type electrolyzer using the catalyst proposed in Comparative Example 4 of the present application;

[0032] Fig.10 This is a gas chromatogram of toluene hydrogenation products tested in a PEM electrolyzer using the catalyst proposed in Example 4 of the present application.

[0033] Fig.11 This is a gas chromatogram of toluene hydrogenation products of the commercial PtRu / C-60% catalyst proposed in Comparative Example 3 of the present application tested in a PEM electrolyzer. DETAILED DESCRIPTION

[0034] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.

[0035] In the drawings, the size of the constituent elements, the thickness of the layer or the area may be exaggerated for the sake of clarity. Therefore, any implementation of the present disclosure is not necessarily limited to the size shown in the drawings, and the shapes and sizes of the components in the drawings do not reflect the true proportions. In addition, the drawings schematically show ideal examples, and any implementation of the present disclosure is not limited to the shapes or values ​​shown in the drawings.

[0036] In the related technologies, hydrogen energy as a green and low-carbon energy has attracted widespread attention, but the development of its safe and efficient storage and transportation technology still faces huge challenges. Therefore, how to achieve efficient hydrogen storage has become one of the main research hotspots. Organic liquid hydrogen storage (LOHC) technology uses organic matter containing unsaturated bonds as hydrogen storage carriers. Under the action of catalysts, unsaturated aromatic compounds react reversibly with hydrogen to achieve hydrogen storage and transportation. At present, conventional unsaturated aromatic compounds are hydrogenated by thermochemical methods, but their energy consumption is high. Since electrochemical hydrogenation has a lower reaction energy barrier and milder reaction conditions, electrochemical hydrogenation has attracted more attention. The hydrogenation catalyst is the most important factor affecting the efficiency of electrochemical hydrogenation, so it is of great significance to develop an efficient and energy-saving electrochemical precious metal hydrogenation catalyst.

[0037] At present, hydrogenation catalysts mainly include nickel catalysts, palladium and platinum catalysts, ruthenium catalysts and rhodium catalysts. Conventional hydrogenation catalysts are nickel metal catalysts with aluminum as carriers. For deep aromatic catalysis, precious metals are the first choice due to their high activity and good stability. They can greatly improve the hydrogenation efficiency of organic liquid hydrogen storage materials and are suitable for large-scale industrial applications.

[0038] However, the existing catalysts and their preparation methods still have some defects and deficiencies:

[0039] 1. The noble metal catalysts prepared by the existing impregnation-gas phase reduction method usually have large particle sizes, and the particle size is difficult to control, the distribution is uneven, and it is easy to agglomerate and accumulate;

[0040] 2. The existing impregnation-gas phase reduction method for preparing precious metal catalysts is usually complicated and time-consuming;

[0041] 3. Currently commercialized precious metal catalysts have a high loading, usually more than 50%, resulting in high catalyst costs and low atomic utilization.

[0042] Based on the above problems, the present application provides a catalyst for electrochemical hydrogenation of aromatic compounds and a preparation method thereof, see Figure 1 , the specific preparation method comprises:

[0043] Step S1: Add the carbon carrier to an appropriate amount of reducing agent, disperse it by ultrasonic, and then add 2+ And Ru 2+ A salt solution of metal ions forms a dispersed system;

[0044] Step S2: After adjusting the pH of the dispersed system to 9-11.5, the dispersed system is transferred to an oil bath at 140°C-220°C for high-temperature reduction reaction, wherein the metal ions in the dispersed system are reduced by the reducing agent, and the formed alloy particles are uniformly loaded on the carbon carrier;

[0045] Step S3: adding the reducing solution obtained by the reduction reaction into excess deionized water, stirring for 1 h to 2 h and then filtering to obtain a catalyst for electrochemical hydrogenation of aromatic compounds.

[0046] It should be noted that the carbon carrier may be any one of Vulcan XC-72, acetylene black, Ketjen black EC300J, EC600JD, carbon nanotubes, carbon fibers, graphene and graphite.

[0047] The reducing agent includes: ethylene glycol, glycerol, triethylene glycol, oleylamine or oleic acid. The reducing agent used in the present application has mild reducing ability and moderate viscosity, which is conducive to controlling the size of the alloy nanoparticles.

[0048] Preferably, the reducing agent is ethylene glycol, and the following embodiments are discussed using ethylene glycol as an example.

[0049] During the preparation, a carbon carrier is used as a carrier, which is added to ethylene glycol to form a uniformly dispersed carbon carrier solution, and then a salt solution of two metal ions is added. After high-temperature reduction, the two metal ions form alloy particles and are uniformly loaded on the carbon carrier to form a catalyst for electrochemical hydrogenation of aromatic compounds with uniform texture. By setting the pH of the dispersion system to 9-11.5, ethylene glycol reduces metal ions in an alkaline environment. In this environment, ethylene glycol has the mildest reducing ability, so that the size of the formed alloy particles can be controlled to avoid agglomeration or accumulation of alloy particles. Alloy particles with smaller size and no agglomeration or accumulation can expose a larger active specific surface area, increase the number of active sites, greatly improve the reaction rate of the catalyst, and thus make the hydrogenation efficiency of aromatic compounds higher when the catalyst catalyzes hydrogenation.

[0050] At the same time, compared with the impregnation-gas phase reduction method, the above preparation method omits the gas phase reduction-calcination operation step, which not only reduces the preparation difficulty, but also shortens the preparation time and improves the economic benefits of the preparation scheme.

[0051] In some embodiments, in step S1, a proper amount of carbon carrier is first weighed and added to ethylene glycol, and ultrasonically dispersed for 10 min to 30 min to obtain a uniformly dispersed carbon carrier solution.

[0052] After ultrasonic dispersion, the carbon carrier can be more evenly dispersed in ethylene glycol, providing a uniform loading environment for the subsequent reduction of metal ions.

[0053] It should be noted that the carbon carrier has good adsorption properties and can improve the 2+ And Ru 2+ The metal ion catalyst is active in hydrogenation catalytic reactions; and the carbon carrier has a rich pore structure, a large specific surface area, and a wide pore distribution, and the dispersion and loading effect of the metal is better than other metal oxide carriers.

[0054] In some embodiments, in step S1, stirring is first started, and the stirring speed is set to 400 rpm to 600 rpm; then an appropriate amount of Pt 2+ And Ru 2+ The salt solution of metal ions is stirred for 20 to 40 minutes until a uniform dispersion system is formed. Stirring helps in the subsequent reduction reaction. 2+ And Ru 2+ Metal ions can be uniformly loaded on the carbon carrier.

[0055] In some embodiments, in step S2, adjusting the pH of the dispersed system to 9 to 11.5 comprises:

[0056] Slowly add a NaOH solution with a concentration of 1 mol / L to 5 mol / L into the dispersion system, and stir at 400 rpm to 600 rpm for 0.5 h to 1.5 h until the pH of the dispersion system reaches 9 to 11.5.

[0057] In the pH range of 9 to 11.5, ethylene glycol has a mild reducing ability, which can achieve controllable size of alloy particles; if the pH exceeds this range, ethylene glycol has a strong reducing ability in this environment, resulting in uncontrollable size of alloy particles, prone to agglomeration and accumulation; if the pH is lower than this range, ethylene glycol has a weak reducing ability in this environment, which will result in insufficient reduction of precious metals, resulting in waste of precious metals. In step S2, ethylene glycol has a moderate viscosity, and the NaOH solution is slowly added to the dispersion system, which helps to accurately adjust the pH of the dispersion system and control the size of alloy particles.

[0058] In some embodiments, when a NaOH solution with a concentration of 1 mol / L to 5 mol / L is slowly added to the dispersion system, it is stirred at 400 rpm to 600 rpm for 0.5 h to 1.5 h to make the alkalinity and viscosity uniform throughout the dispersion system, thus constructing a stable alkaline reducing environment.

[0059] By using a NaOH solution with a relatively high concentration, the pH of the reaction dispersion system can be efficiently regulated to ensure that the solution system quickly reaches the target pH range. A large number of tiny metal hydroxide crystallites can be better dispersed and adsorbed on the surface of the carrier, making the metal particles more dispersed, more uniform in particle size, and smaller in size after reduction, thereby preventing metal ions from staying in the slightly alkaline range for too long, causing a large number of metal hydroxide crystallites to agglomerate, nucleate and grow, resulting in the metal particles being too large in particle size and having poor dispersion.

[0060] In some embodiments, a peristaltic pump is used to control the NaOH solution to be slowly added to the dispersion system; the peristaltic pump pumps 0.01% to 0.1% of the total volume of the dispersion system per minute. The peristaltic pump flow rate can accurately control the amount of NaOH solution added, stably and quickly regulate the pH of the dispersion system, and improve the consistency of the catalyst.

[0061] The synthesis method of the present application enables metal ions to be better dispersed and adsorbed on the surface of the carrier, and after reduction, the metal particles have a higher dispersion, a more uniform particle size, and a smaller size.

[0062] In some embodiments, in the dispersed system, Pt 2+ Metal ions and Ru 2+ The mass ratio of metal ions is 1:6 to 4:1.

[0063] During preparation, platinum and ruthenium are loaded on the same carbon carrier in the form of alloy particles. The two can produce a synergistic effect and jointly promote the hydrogenation catalytic reaction.

[0064] It should be noted that Pt 2+ Metal ions and Ru 2+ The amount of metal ions added can be adjusted appropriately according to the ratio, but whether it is Pt 2+ The metal ion is more Ru 2+ More metal ions can achieve efficient catalysis within a suitable mass ratio range. In addition, the mass ratio of the total mass of metal ions to ethylene glycol must be controlled to ensure that the metal ions in the salt solution are reduced to the maximum, which helps to ensure the loading amount of metal ions on the carbon carrier.

[0065] In some embodiments, in step S1, Pt 2+ The metal ion salt solution can be a platinum chloride salt solution, a sodium hexachloroplatinate salt solution, a platinum nitrate salt solution, a platinum acetylacetonate salt solution, and a platinum sulfate salt solution;

[0066] Ru 2+ The salt solution of metal ions can be ruthenium acetylacetonate salt solution, ruthenium acetate salt solution, triruthenium hexafluorophosphate salt solution and ruthenium chloride salt solution.

[0067] In some embodiments, in step S2, when the dispersed system with a pH of 9 to 11.5 is transferred to an oil bath pot for high-temperature reduction reaction, the oil bath temperature is 140° C. to 220° C., and the reduction reaction time is 0.5 h to 1.5 h.

[0068] The above oil bath temperature helps to promote the reduction of metal ions by ethylene glycol, accelerate the reaction rate and shorten the preparation time.

[0069] In some embodiments, in step S3, after the reducing liquid after high-temperature reduction is cooled to room temperature, the reducing liquid is added into deionized water and stirred for 1 h to 2 h, and the stirring speed is set to 600 rpm.

[0070] Through the above steps, the alloy particles on the carbon carrier are loaded more evenly.

[0071] In some embodiments, the volume of the deionized water is greater than or equal to 10 times the volume of the reducing solution.

[0072] An appropriate amount of deionized water can dilute the reducing liquid with high viscosity, making it easy to separate the catalyst. The reducing liquid obtained by the reduction reaction also contains a large amount of impurity anions (for example, chloride ions, nitrate ions, sulfate ions, etc.). Adding water with a volume greater than or equal to 10 times the volume of the reducing liquid will replace the anions in the catalyst into the diluted reducing liquid, release the space between the alloy particles of the catalyst, remove the unstable metal ions and anions in the carbon carrier of the catalyst, reduce the impurity content in the catalyst product, and facilitate the adsorption and activation of the reactants on the catalyst surface. When the electrochemical hydrogenation reaction is carried out on the electrode, the anions can be prevented from poisoning the electrode / aromatic compound under the action of current / voltage, affecting the effect of catalytic hydrogenation of aromatic compounds.

[0073] In some embodiments, in step S3, the reducing liquid stirred in deionized water is filtered to take out the solid product in the reducing liquid, and the solid product is washed with deionized water and then dried in a vacuum oven, wherein the temperature is set at 60°C to 80°C and the drying time is 6h to 10h. The dried solid product is ground into powder to obtain a catalyst for electrochemical hydrogenation of aromatic compounds.

[0074] After the above treatment, other impurities on the solid product can be removed to obtain a high-purity catalyst.

[0075] In a second aspect, the present application provides a catalyst obtained by the above preparation method. Under the action of the catalyst, the hydrogenation conversion rate of aromatic compounds can reach more than 90% within 2 hours, greatly improving the hydrogenation efficiency.

[0076] In some embodiments, in the catalyst, the particle size of the alloy particles is 2 nm to 3 nm.

[0077] The embodiment of the present application achieves controllability of the size of nanoparticles by adjusting the pH, and the size of the alloy particles formed is 2nm to 3nm, which greatly improves the intrinsic activity of the catalyst.

[0078] In some embodiments, the alloy particles account for 35% to 45% of the total mass of the catalyst.

[0079] Although the loading amount of alloy particles in the catalyst prepared in the embodiment of the present application is less than 50% to 60%, the active sites and active specific surface area on the alloy particles are increased, and the atomic utilization rate is improved. Therefore, the corresponding catalytic efficiency is higher and the hydrogenation effect is better.

[0080] In a third aspect, an embodiment of the present application provides an application of the above-mentioned catalyst, where the catalyst is used in the electrochemical hydrogenation reaction of aromatic compounds.

[0081] In order to enable those skilled in the art to better understand the present invention, a method for preparing a catalyst for electrochemical hydrogenation of aromatic compounds provided by the present invention is described below through a number of specific embodiments.

[0082] Example 1

[0083] A method for preparing a catalyst for electrochemical hydrogenation of aromatic compounds:

[0084] 1. Add 120 mg of Ketjen Black EC300J powder into a three-necked flask containing 30 mL of ethylene glycol, and ultrasonicate for 15 min to obtain a uniformly dispersed carbon support solution;

[0085] 2. Set the stirring speed to 400 rpm, slowly add a platinum chloride solution with a concentration of 41.5 mg / ml and a volume of 0.386 ml, and a ruthenium chloride solution with a concentration of 21.9 mg / ml and a volume of 2.92 ml to the above carbon support solution, and continue stirring for 30 minutes to form a uniform dispersion system (in the dispersion system, Pt 2+ The mass of the ion is 16 mg, Ru 2+ The mass of the ion is 64 mg);

[0086] 3. Slowly and evenly add 5 mol / L NaOH solution into the above dispersion system by controlling the flow rate of the peristaltic pump to 5 μL / min, adjust the pH to 9, and then move to an oil bath for high-temperature reduction reaction. The heating temperature is set to 150°C and the heating time is 1h.

[0087] 4. When the reduced solution after the reaction has finished cools to room temperature, pour the reduced solution into a beaker, add 450 mL of deionized water and stir thoroughly for 1 hour;

[0088] 5. Filter the reducing liquid in the beaker and wash it with deionized water. Collect the product and dry it in a vacuum drying oven. The temperature of the drying oven is set to 60°C and the drying time is 10 hours. After drying, grind the product into powder to obtain a catalyst. In the catalyst, the total loading of PtRu alloy particles on the carbon carrier is 40%.

[0089] Example 2

[0090] The only difference between Example 2 and Example 1 is the pH of the dispersed system. In Example 2, the pH of the dispersed system is 11.5.

[0091] Example 3

[0092] The only difference between Example 3 and Example 1 is the pH of the dispersed system. In Example 3, the pH of the dispersed system is 10.5.

[0093] Example 4

[0094] The difference between Example 4 and Example 3 is that Pt 2+ With Ru 2+ The mass ratio of Pt 2+ The mass of Ru is 53.2 mg. 2+ The mass is 26.6 mg.

[0095] See also Figure 2 , Figure 2 This is the X-ray diffraction pattern of the catalyst in Example 4.

[0096] Among them, Pt has obvious diffraction peaks at 39°, 46° and 67°, which are attributed to the (111), (200) and (220) crystal planes of Pt, respectively. According to the standard PDF card information (JCPDS: 06-0663), the characteristic peaks of metallic Ru are located at 38.4°, 42.2° and 44°. Due to the overlap with the Pt signal, the accurate identification of the Ru diffraction peak is hindered. In addition, it can be seen from the spectrum that the peak type of the diffraction peak is relatively wide, indicating that Ru may have been incorporated into the Pt lattice to form a PtRu alloy in an amorphous form.

[0097] See also Figure 3 and Figure 4 , Figure 3 Transmission electron microscope image (a) of the catalyst in Example 4, Figure 4 (b) is a transmission electron microscope image of the catalyst in Example 4.

[0098] It can be seen from the figure that the catalyst morphology is in the form of nanoparticles, and the particles are evenly distributed without obvious agglomeration, and the particle size is between 2nm and 3nm.

[0099] The catalyst prepared in Example 4 was further subjected to ICP-OES test. The test results are shown in Table 1.

[0100] Table 1. Catalyst ICP-OES test results

[0101] element Theoretical element content of sample w(%) Actual element content of sample w(%) Pt 26.7% 26.3% Ru 13.3% 13.0%

[0102] According to Table 1, the actual content of precious metal elements in the catalyst sample is very close to the theoretical value. This proves that the preparation method of Example 4 of the present application is reasonable, and the total amount of alloy particles loaded in the prepared catalyst is about 40%.

[0103] Example 5

[0104] The difference between Example 5 and Example 3 is that Pt 2+ With Ru 2+ The mass ratio of Pt is different. In Example 5, 2+ The mass of Ru is 11.4 mg. 2+ The mass is 68.6 mg.

[0105] Example 6

[0106] The difference between Example 6 and Example 3 is that Pt 2+ With Ru 2+ The mass ratio of Pt is different. In Example 6, 2+ The mass of Ru is 64 mg. 2+ The mass is 16 mg.

[0107] Example 7

[0108] The only difference between Example 7 and Example 3 is the oil bath temperature. In Example 7, the oil bath temperature is 140°C.

[0109] Example 8

[0110] The only difference between Example 8 and Example 3 is the oil bath temperature. In Example 8, the oil bath temperature is 190°C.

[0111] Example 9

[0112] The difference between Example 9 and Example 3 is only that the reducing agent is different. In Example 9, the reducing agent is propylene glycol and the oil bath temperature is 150°C.

[0113] Example 10

[0114] The difference between Example 10 and Example 3 lies in the different reducing agents and the different oil bath temperatures. In Example 10, the reducing agent is oleylamine and the oil bath temperature is 220°C.

[0115] Embodiment 11

[0116] The difference between Example 11 and Example 3 lies in the different reducing agents and the different oil bath temperatures. In Example 11, the reducing agent is oleic acid and the oil bath temperature is 220°C.

[0117] Example 12

[0118] The only difference between Example 12 and Example 3 is the reducing agent. In Example 12, the reducing agent is triethylene glycol and the oil bath temperature is 150°C.

[0119] Comparative Examples 1-6 were set based on the above-mentioned Examples 1-12.

[0120] Comparative Example 1

[0121] A method for preparing a catalyst for electrochemical hydrogenation of aromatic compounds:

[0122] 1. Dissolve 120 mg of Ketjen Black EC300J powder in a three-necked flask containing 30 mL of ethylene glycol, and ultrasonicate for 15 min to obtain a uniformly dispersed carbon support solution;

[0123] 2. Set the stirring speed to 400 rpm, slowly add a platinum chloride solution with a concentration of 37 mg / ml and a volume of 1.44 ml, and a ruthenium chloride solution with a concentration of 23.63 mg / ml and a volume of 1.13 ml to the above carbon support solution, and continue stirring for 30 min to form a uniform dispersion system (in the dispersion system, Pt 2+ The mass of the ion is 53.2 mg, Ru 2+ The mass of the ion is 26.6 mg);

[0124] 3. Slowly and evenly add 5 mol / L NaOH solution into the above dispersion system by controlling the flow rate of the peristaltic pump to 5 μL / min, adjust the pH to 11.8, and then move to an oil bath for high-temperature reduction reaction. The heating temperature is set to 150°C and the heating time is 1h.

[0125] 4. When the reduced solution after the reaction has finished cools to room temperature, pour the reduced solution into a beaker, add 450 mL of deionized water and stir thoroughly for 1 hour;

[0126] 5. Filter the reducing liquid in the beaker and wash it with deionized water. Collect the product and dry it in a vacuum drying oven. The temperature of the drying oven is set to 60°C and the drying time is 10 hours. After drying, grind the product into powder to obtain a catalyst. In the catalyst, the alloy loading on the carbon carrier is 40%.

[0127] Comparative Example 2

[0128] The difference between Comparative Example 2 and Comparative Example 1 lies in the different pH values ​​of the dispersion system and the different oil bath temperatures. In Comparative Example 2, the pH value of the dispersion system is 10.5, and the oil bath temperature is 120°C.

[0129] Comparative Example 3

[0130] The only difference between Comparative Example 3 and Comparative Example 1 is that a commercial PtRu / C-60%-2:1 catalyst is used in Comparative Example 3. In PtRu / C-60%-2:1, "60%" represents the total loading amount of the PtRu alloy particles on the carbon support; "2:1" represents the mass ratio of Pt to Ru in the alloy particles.

[0131] Comparative Example 4

[0132] The difference between Comparative Example 4 and Comparative Example 1 is that the pH of the dispersed system is different and the metal ions are different. In Comparative Example 4, the pH of the dispersed system is 10.5, and the metal ions are only Pt 2+ .

[0133] Comparative Example 5

[0134] The difference between Comparative Example 5 and Comparative Example 1 is that the pH of the dispersed system is different and the metal ions are different. In Comparative Example 5, the pH of the dispersed system is 10.5, and the metal ions are only Ru 2+ .

[0135] It should be noted that in the above embodiments and comparative examples, the volume of water introduced into the reaction system is not greater than 12% of the volume of the reducing agent, so as to avoid excessive water affecting the viscosity of the dispersion system, resulting in weak adsorption and poor dispersion of metal ions on the carbon carrier; water and the reducing agent form a miscible substance, which easily leads to a low reduction temperature of the dispersion system, which is not conducive to the reduction of metal ions on the carrier.

[0136] Comparative Example 6

[0137] The difference between Comparative Example 6 and Comparative Example 1 is that the pH of the dispersion system is different and the solvent is different. In Comparative Example 6, the pH of the dispersion system is 10.5, the solvent is 25 mL of ethylene glycol and 5 mL of water, and the volume of water introduced into the reaction system is 40% of the volume of the reducing agent.

[0138] The catalytic hydrogenation performance of the catalysts prepared in Examples 1-12 and Comparative Examples 1-6 was tested. The aromatic compound was toluene, and the test was performed using an H-type electrolyzer in a three-electrode manner. During the test, the cathode electrolyte was a phosphate buffer solution and a small amount of toluene, and the catalyst-loaded nickel foam was used as the working electrode, with a loading of 1 mg / cm 2 The saturated Ag / AgCl electrode was used as the reference electrode; the anode used an acidic electrolyte, and the platinum wire was used as the counter electrode. The test temperature was room temperature 25°C. The electrochemical hydrogenation performance of the catalyst was evaluated by the amount of hydrogen added after the catalyst was tested for 1 hour at a constant current. The test results are shown in Figure 5-10 And Table 1 below.

[0139] Table 1. Hydrogenation performance results of examples and comparative examples (a)

[0140]

[0141]

[0142] Figure 5 The gas chromatogram of the toluene hydrogenation product tested in a three-electrode H-type electrolyzer by the catalyst proposed in Example 3 of the present application. Combining the test results of the catalysts prepared in Comparative Example 1, Example 1, Example 2 and Example 3, it can be found that the catalyst prepared in the pH range of 9 to 11.5 has a better catalytic effect than that in Comparative Example 1, wherein the catalyst prepared at a pH of 10.5 has the best effect. The hydrogenation effect of the catalyst prepared at a pH of 11.8 in Comparative Example 1 is much lower than that of the catalyst prepared in Example 3, indicating that the pH during reduction needs to be strictly controlled, and the best pH is 10.5.

[0143] The reduction temperature has a great influence on the performance of the prepared catalyst. If the temperature is too low, the reduction efficiency of ethylene glycol will be reduced, and even the metal ions loaded on the carbon carrier will be less than 35%. When the metal loading on the carbon carrier is too low, the active sites that can catalyze hydrogenation are reduced, resulting in poor catalytic hydrogenation effect. Therefore, the reduction temperature is best controlled at 150°C.

[0144] Figure 6 This is a gas chromatogram of toluene hydrogenation products tested in a three-electrode H-type electrolyzer using the catalyst proposed in Example 4 of the present application. Combined with Table 1, it can be seen that the electrochemical hydrogenation amount of the catalyst in the three-electrode H-type electrolyzer reaches 19.2%. Figure 7 , the commercial PtRu / C-60%-2:1 catalyst can only achieve 8.6% electrochemical hydrogenation in a three-electrode H-type electrolyzer. Figure 8 The catalyst proposed in Comparative Example 1 can only achieve 8.2% electrochemical hydrogenation when toluene is used as a substrate in a three-electrode H-type electrolyzer. Fig. 9 The catalyst proposed in Comparative Example 4 can only achieve 4.5% of electrochemical hydrogenation when toluene is used as a substrate in a three-electrode H-type electrolyzer.

[0145] For the above examples and comparative examples, toluene can also be used as a substrate, and a PEM electrolyzer is used to perform an electrochemical hydrogenation performance test in a two-electrode manner. During the test, the catalyst is used as a cathode catalyst, and the anode catalyst is IrO 2 , the hydrogenation substrate is pure toluene, the test time is 2h, and the test temperature is room temperature 25℃.

[0146] refer to Fig.10This is the gas chromatogram of the toluene hydrogenation product tested in a PEM electrolyzer using the catalyst proposed in Example 4 of the present application. The signal peak at 2.9 min corresponds to the signal peak of methylcyclohexane, and the signal peak at 3.8 min corresponds to the signal peak of toluene. The electrochemical hydrogenation amount can reach 96.25%, showing excellent hydrogenation performance. Fig.11 , the commercial PtRu / C-60%-2:1 catalyst was tested for hydrogenation in a PEM electrolyzer, and its electrochemical hydrogenation capacity could only reach 56.37%. This indicates that the catalytic hydrogenation effect of the catalyst prepared in Example 4 of the present application is much higher than that of the commercial PtRu / C-60%-2:1 catalyst.

[0147] In summary, the present application can control the smaller alloy particle size to allow the metal particles to be evenly distributed on the carbon carrier, which is beneficial to exposing a larger active specific surface area of ​​the alloy nanoparticles and increasing the number of active sites of the alloy nanoparticles, thereby greatly improving the reaction rate of the catalyst and accelerating the hydrogenation conversion rate.

[0148] The catalyst prepared in Example 3 was used with different aromatic compounds as substrates, and the hydrogenation results are shown in Table 2.

[0149] Table 2. Hydrogenation performance results (b)

[0150]

[0151] When different aromatic compounds are used as hydrogen storage carriers, the catalytic hydrogenation effect of the catalyst prepared in Example 3 of the present application remains stable, and can promote the reaction to achieve a higher hydrogenation conversion rate. Taking only N-methylindole and 2-methylpyrazine as examples in Table 2, replacing the substrate with one or more of dibenzyltoluene, N-ethylcarbazole, benzyltoluene, 3-methylindole, 7-methylindole, cyclopentylpyrazine, carbazole, N-ethylindole, pyrazine, 2,3-dimethylpyrazine, 2,5-dimethylpyrazine, pyridazine, pyridine and 3-methylpyridine can also achieve a higher hydrogenation effect, and this application will not repeat it in detail.

[0152] In summary, the catalyst and preparation method thereof for electrochemical hydrogenation of aromatic compounds provided in the present application not only have a simple preparation process and shorten the time cost, but also the nanoparticles prepared by the method have uniform particle size distribution, small size, large active specific surface area, large number of active sites, faster catalytic reaction rate, and higher hydrogenation conversion rate. The size of the alloy particles in the prepared catalyst is 2nm to 3nm, which further improves the intrinsic activity of the catalyst. The loading amount of precious metals in the catalyst is only 40%, which not only reduces the catalyst cost but also improves the atomic utilization rate.

[0153] The various embodiments in this specification are described in a progressive manner, and each embodiment focuses on the differences from other embodiments. The same or similar parts between the various embodiments can be referenced to each other.

[0154] Although the preferred embodiments of the present application have been described, those skilled in the art may make additional changes and modifications to these embodiments once they have learned the basic creative concept. Therefore, the appended claims are intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of the embodiments of the present application.

[0155] Finally, it should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or terminal device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or terminal device. In the absence of further restrictions, the elements defined by the sentence "including one..." do not exclude the existence of other identical elements in the process, method, article or terminal device including the elements.

[0156] The above is a detailed introduction to a catalyst for electrochemical hydrogenation of aromatic compounds and a preparation method thereof provided in the present application. Specific examples are used herein to illustrate the principles and implementation methods of the present application. The description of the above embodiments is only used to help understand the method of the present application and its core idea; at the same time, for a person skilled in the art, according to the idea of ​​the present application, there will be changes in the specific implementation method and application scope. In summary, the content of this specification should not be understood as a limitation on the present application.

Claims

1. A method for preparing a catalyst for electrochemical hydrogenation of aromatic compounds, characterized in that: The preparation method comprises: Step S1: add a carbon carrier to an appropriate amount of reducing agent, disperse it by ultrasonic, and then add a 2+ And Ru 2+ A salt solution of metal ions forms a dispersed system; Step S2, after adjusting the pH of the dispersed system to 9-11.5, transferring to an oil bath at 140°C-220°C for high-temperature reduction reaction, the metal ions in the dispersed system are reduced by the reducing agent, and the formed alloy particles are uniformly loaded on the carbon carrier; Step S3, adding the reducing solution obtained by the reduction reaction into excess deionized water, stirring for 1 h to 2 h and then filtering to obtain the catalyst for electrochemical hydrogenation of aromatic compounds.

2. The method for preparing a catalyst for electrochemical hydrogenation of aromatic compounds according to claim 1, characterized in that: Adjusting the pH value of the dispersed system to 9-11.5 comprises: slowly adding a NaOH solution with a concentration of 1 mol / L-5 mol / L into the dispersed system, and stirring at 400 rpm-600 rpm for 0.5 h-1.5 h until the pH value of the dispersed system reaches 9-11.

5.

3. The method for preparing a catalyst for electrochemical hydrogenation of aromatic compounds according to claim 2, characterized in that: A peristaltic pump is used to control the NaOH solution to be slowly added into the dispersion system; The peristaltic pump pumps 0.01% to 0.1% of the total volume of the dispersed system per minute.

4. The method for preparing a catalyst for electrochemical hydrogenation of aromatic compounds according to claim 1, characterized in that: The reducing agent includes: one of ethylene glycol, glycerol, triethylene glycol, oleylamine or oleic acid.

5. The method for preparing a catalyst for electrochemical hydrogenation of aromatic compounds according to claim 1, characterized in that: In the dispersed system, the Pt 2+ Metal ions and the Ru 2+ The mass ratio of metal ions is 1:6 to 4:

1.

6. The method for preparing a catalyst for electrochemical hydrogenation of aromatic compounds according to claim 1, characterized in that: The reduction reaction time is 0.5h to 1.5h; the volume of the deionized water is greater than or equal to 10 times the volume of the reducing solution.

7. The catalyst obtained by the method for preparing a catalyst for electrochemical hydrogenation of aromatic compounds according to any one of claims 1 to 6, wherein the particle size of the alloy particles is 2 nm to 3 nm.

8. The catalyst according to claim 7, characterized in that In the catalyst, the alloy particles account for 35% to 45% of the total mass of the catalyst.

9. Use of the catalyst according to claim 7, characterized in that: The catalyst is used in the electrochemical hydrogenation reaction of aromatic compounds.

10. Use of the catalyst according to claim 9, characterized in that: The aromatic compound includes: one or more of toluene, dibenzyltoluene, N-ethylcarbazole, benzyltoluene, 3-methylindole, 7-methylindole, cyclopentylpyrazine, carbazole, N-methylindole, N-ethylindole, pyrazine, 2,3-dimethylpyrazine, 2,5-dimethylpyrazine, 2-methylpyrazine, pyridazine, pyridine and 3-methylpyridine.

Citation Information

Patent Citations

  • Preparation method and application of aromatic compound hydrogenation rhodium / activated carbon catalyst

    CN106732564A

  • Catalyst with high metal loading capacity as well as preparation and application thereof

    CN112823880A

  • Preparation method of platinum-carbon catalyst, platinum-carbon catalyst and catalyst coating film

    CN115458755A

  • Preparation and application of carbon-based bimetallic nanocluster catalyst