Application of platinum nanowire catalyst in electrochemical hydrogenation of soybean oil
By growing platinum nanowire catalysts on carbon powder, used for electrochemical hydrogenation of soybean oils and fats in proton exchange membranes, the problem of insufficient mechanical strength and durability of traditional catalysts is solved, and the hydrogenation effect of efficient and low trans fatty acids is achieved.
Patent Information
- Application Number
- CN202410763257.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-13
- Publication Date
- 2024-11-26
AI Technical Summary
The high content of trans fats in hydrogenated soybean oil produced by traditional hydrogenation processes leads to human health hazards. The lack of mechanical strength and durability of commercial carbon-loaded platinum catalysts leads to poor hydrogenation efficiency and stability.
Platinum nanowire catalyst is used to mix with carbon powder and Nafion solution through ultrasonic method, spray it on the PTFE membrane, and the growth temperature is controlled to 10-40℃ to form a platinum nanowire/carbon matrix catalyst, which is used for electrochemical hydrogenation of soybean oil and fat in proton exchange membrane. .
The catalytic efficiency of hydrogenated soybean oil is improved, the formation of trans fatty acids is reduced, the stability and electrochemical activity of the catalyst are enhanced, and the hydrogenation efficiency of oil and fat is improved.
Smart Images

Figure BDA0004891656460000041 
Figure BDA0004891656460000111 
Figure BDA0004891656460000121
Abstract
Description
Technical Field
[0001] The invention relates to a Pt-based catalyst, in particular to a platinum nanowire catalyst and application thereof in electrochemical hydrogenation of soybean oil. Background Art
[0002] Soybean hydrogenated oil is widely used in candy, shortening, margarine and other food fields, but the trans fatty acid (TFAs) content in hydrogenated soybean oil produced by traditional hydrogenation process is as high as 20%-60%, which is very harmful to human health, such as obesity, cardiovascular and cerebrovascular diseases, diabetes, breast cancer and Alzheimer's disease, and has a serious impact on the growth and development of infants and young children. Therefore, the demand for developing new technologies for soybean oil without trans fatty acids is becoming increasingly urgent. The proton exchange membrane electrochemical hydrogenation method uses electrolyte solution or aqueous solution as hydrogen source, overcomes the defect of low adhesion of gaseous hydrogen atoms on the surface of solid catalyst in a multiphase dispersed system with hydrogen as hydrogen source, realizes hydrogenation addition at low temperature, normal pressure and low current density, greatly reduces the formation of trans fatty acids, and becomes the most potential method to reduce trans fatty acids instead of traditional gas hydrogenation.
[0003] The core component of the SPE reactor is the membrane electrode assembly (MEA) composed of a proton exchange membrane and carbon paper sprayed with a catalyst. It is the main place for the hydrogenation reaction. The catalyst used in the MEA is closely related to the hydrogenation effect of the reactor. At present, the most commonly used commercial carbon-supported platinum (Pt / C) catalyst in oil hydrogenation is a Pt-based catalyst, using amorphous carbon black as a catalyst carrier. However, due to the irregular structure of amorphous carbon, limited mechanical strength and loading capacity, the amount of catalyst loaded on it is limited, and as the reaction proceeds, the amorphous carbon is gradually destroyed, and the Pt loaded on it also falls off and agglomerates, resulting in poor hydrogenation efficiency and catalytic stability. The zero-dimensional (0D) morphology of commercial Pt / C catalyst nanoparticles has high surface energy and low surface coordination atoms, with many defect sites and character boundaries, which often leads to Ostwald ripening and agglomeration of nanoparticles; and due to the corrosion of carbon, the Pt particles loaded on carbon are prone to migrate during the operation of the fuel cell, so these commercial catalysts have low activity and poor durability. Compared with nanoparticles, the one-dimensional (1D) structure of platinum nanowires (Pt-NWs) has intrinsic structural features such as anisotropy of highly active crystal faces and preferential exposure to <111> Therefore, the nanowire structure possesses a more accessible electron transfer pathway and has a more effective surface exposure as an active catalytic site in the electrode-electrolyte interface. Summary of the invention
[0004] The purpose of the present invention is to solve the problems existing in the prior art, disclose a preparation method of a platinum nanowire catalyst and its application in electrochemical hydrogenation of soybean oil. The specific preparation method of the present invention can improve the catalytic efficiency of electrochemical hydrogenation of soybean oil, and prepare hydrogenated soybean oil with low trans fatty acids. The specific preparation method comprises the following steps:
[0005] 1. Weigh 0.5-3 mg of carbon powder, place it in a centrifuge tube, add isopropanol and Nafion solution, and ultrasonicate for 1-2 hours to prepare catalyst slurry;
[0006] 2. Spray the catalyst slurry onto the PTFE membrane using a spray gun to obtain a carbon powder matrix layer;
[0007] 3. Fix the substrate layer in a culture dish, add 1-2 mg of chloroplatinic acid and 0.2%-0.6% formic acid aqueous solution to obtain a carbon substrate attached to platinum nanowires;
[0008] 4. The growth temperature of platinum nanowires is controlled at 10-40°C.
[0009] The volume of the isopropanol is 0.5 to 2 times the mass of the carbon powder, and the mass concentration of the Nafion solution is 5 to 30%;
[0010] The dimensions of the PTFE membrane were 2.3×2.3 cm.
[0011] The Pt-NWs / C catalyst prepared by the above method can be used as a cathode catalyst in a SPE electrochemical hydrogenation reactor.
[0012] The Pt-NWs / C catalyst prepared by the above method can be used as a hydrogenation reaction catalyst.
[0013] The Pt-NWs / C catalyst prepared by the above method can be used as an SPE cathode catalyst in the electrochemical hydrogenation of soybean oil. The reaction conditions are: reaction temperature 30-80°C, oil phase flow rate 20-90 mL / min, water phase flow rate 20-90 mL / min, and the anode catalyst is Pt / C.
[0014] Compared with the prior art, the present invention has the following advantages:
[0015] Soybean oil was hydrogenated using an SPE hydrogenation reactor, and the oil hydrogenation process was optimized by preparing platinum nanowires. Platinum nanowires, as a one-dimensional precious metal catalyst, have highly active crystal face anisotropy and preferential exposure. <111> The surface has high electrocatalytic activity and stability, giving full play to the catalytic performance of Pt particles and improving the efficiency of oil hydrogenation. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1CVs (left) and ECSA values (right) corresponding to Pt-NWs grown at different formic acid concentrations
[0017] Figure 2 CVs (left) and ECSA values (right) of Pt-NWs at different growth temperatures
[0018] Figure 3 CVs (left) and ECSA values (right) of Pt-NWs grown on substrates with different Nafion contents
[0019] Figure 4 SEM images of the Pt-NWs catalytic layer grown at different formic acid concentrations, 5:600 (a, b), 7:600 (c, d) and 9:600 (e, f)
[0020] Figure 5 SEM images of the catalytic layer surface of Pt-NWs at different growth temperatures, (a, b) 10°C, (c, d) 20°C, and (e, f) 40°C.
[0021] Figure 6 SEM images of the surface of the carbon matrix catalyst layer with different Nafion contents, Nafion is (a) 5, (b) 10, (c) 15, (d) 20wt% respectively.
[0022] Figure 7 TEM images of the Pt-NWs catalytic layer grown at different formic acid concentrations: 5:600 (A), 7:600 (B), and 9:600 (C).
[0023] Figure 8 TEM images of the Pt-NWs catalytic layer surface at different growth temperatures: (a, b) 10°C, (c, d) 20°C, and (e, f) 40°C.
[0024] Fig. 9 XRD patterns of Pt-NWs grown at 20℃ with formic acid concentration of 7:600 and commercial Pt / C
[0025] Fig.10 Comparison of water contact angles for commercial Pt / C and Pt-NWs / C catalyst layers
[0026] Fig.11 The influence of thermal pressure factors on membrane electrode resistance
[0027] Fig.12 The voltage change during hydrogenation at different reaction temperatures and its effect on iodine value and resistance
[0028] Fig.13The voltage change during hydrogenation at different oil phase flow rates and its effect on iodine value and resistance
[0029] Fig.14 Comparison chart of soybean oil and hydrogenated oil catalyzed by different catalysts
[0030] Fig.15 Analysis of aroma and flavor components of hydrogenated soybean oil (A), Pt / C (B) and Pt-NWs / C (C)
[0031] Fig.16 The principal component analysis diagram of soybean oil, Pt / C and Pt-NWs / C hydrogenated oil
[0032] Fig.17 Melting and crystallization curves of soybean oil, Pt / C hydrogenated oil and Pt-NWs / C hydrogenated oil
[0033] Fig.18 Crystallization of hydrogenated soybean oil (a), Pt / C (b) and Pt-NWs / C (c) DETAILED DESCRIPTION
[0034] The technical solution of the present invention is further described below in conjunction with the accompanying drawings, but is not limited thereto. Any modification or equivalent replacement of the technical solution of the present invention without departing from the spirit and scope of the technical solution of the present invention should be included in the protection scope of the present invention.
[0035] This experiment provides a method for preparing a Pt-NWs / C catalyst, the method comprising the following steps:
[0036] Step 1: Weigh 11.556 mg of carbon powder, place in a centrifuge tube, add 2 ml of isopropanol and 10% Nafion solution of the carbon powder mass, and ultrasonicate for 1 h to prepare catalyst slurry;
[0037] Step 2: The catalyst slurry is sprayed on a 2.3×2.3 cm PTFE membrane using a spray gun to obtain a carbon powder matrix layer;
[0038] Step 3: Fix the substrate layer in a culture dish, add 1-2 mg of chloroplatinic acid and 0.2%-0.6% formic acid aqueous solution to obtain a carbon substrate attached to the platinum nanowires; the growth temperature of the platinum nanowires is controlled at 20°C.
[0039] Results and analysis:
[0040] 1. Preparation of platinum nanowires and study of their properties
[0041] Pt-NWs were successfully grown on a sprayed carbon substrate (carbon powder) by a simple wet chemical method, namely chemical reduction. The catalyst morphology was characterized by scanning electron microscopy and transmission electron microscopy, and the electrochemical performance of the catalyst was characterized by CV curves by controlling the single-factor variable reducing agent concentration, reaction temperature, and Nafion content in the carbon matrix. Finally, the Pt-NWs / C with the optimal reaction conditions was compared with the commercial catalyst Pt / C.
[0042] 1. Electrochemical activity analysis
[0043] (1) Cyclic voltammetry curve test
[0044] The cyclic voltammetry (CV) tests were carried out in 0.1 M HClO4 electrolyte, with the main purpose of studying the redox properties of the catalyst.
[0045] (2) Electrochemical Active Surface Area (ECSA, m 2 / g) is the area that reflects the actual catalytic effect of the catalyst during the reaction process. It is an important parameter for evaluating the intrinsic activity of the catalyst. By analyzing the adsorption / desorption peak area in the cyclic voltammetry (CV) diagram, the electrochemically active surface area of the catalyst can be calculated. ECSA is an important indicator for evaluating the electrocatalytic activity of platinum catalysts. The larger the ECSA, the more catalytic active sites are provided to the electrode reaction, that is, the higher the electrochemical activity of the catalyst. The ECSA calculation formula is as follows:
[0046]
[0047] Note: SH is the peak area, V is the scanning rate (its ratio is the number of electron transfers in the selected peak area, C); m is the mass of Pt, g; qH is a constant: 0.21mC.cm -2 SH is calculated using the integration function in Origin Pro 2021 software.
[0048] from Figure 1 It can be seen that at 20 ° C, with the increase of formic acid concentration, the electrochemical performance of Pt-NWs first increases and then decreases, and the shape is similar to that of a volcano. At a concentration of 7:600, the ECSA value reaches a maximum of 27.40 m 2 g -1 However, when the formic acid concentration increased to 13:600, the ECSA value dropped significantly to 17.05m 2 g -1, the electrochemical performance is the worst. This may be because the high concentration of formic acid causes Pt to agglomerate, reducing the exposure of the active surface. Therefore, a formic acid concentration of 7:600 is the optimal condition for preparing the cathode platinum nanowire catalytic layer.
[0049] from Figure 2 It can be seen that the reaction temperature has a significant effect on the structure of the Pt-NWs cathode and its battery performance. When the growth temperature was raised to 40°C, the reaction solution in the culture dish was observed and its color was gradually deepening. The reason for this change is that although part of the Pt underwent a reduction reaction in the solution, it was not completely attached to or grown on the carbon support, which resulted in the active sites on the carbon support not being fully utilized, which in turn caused a decrease in battery performance. In order to more comprehensively evaluate the effect of reaction temperature on the performance of Pt-NWs, the researchers measured the CV curves of single cells prepared with Pt-NWs catalyst layers grown in the temperature range of 10 to 40°C, and calculated the corresponding ECSA values based on this. Figure 2 As shown in Figure 2, the ECSA values of Pt-NWs at different growth temperatures show significant differences. Specifically, at reaction temperatures of 10, 20, 30, and 40 °C, the ECSA values of Pt-NWs are 21.46, 27.40, 23.93, and 17.98 m 2 g -1 . From these data, it can be seen that when the reaction temperature is 20°C, the ECSA value of Pt-NWs reaches the best state. This means that at this temperature, the distribution of Pt-NWs on the carbon spheres is more uniform, and the agglomeration phenomenon is reduced, thereby exposing a larger active area. This uniform distribution and less agglomerated structure help improve the utilization rate and electrochemical performance of the catalyst.
[0050] from Figure 3 It can be seen that the content of Nafion solution added to the carbon matrix has a significant effect on the ECSA value of the catalyst. When the Nafion content is 10wt%, the ECSA value reaches a peak value, i.e., 27.4m 2 g -1 When the Nafion content is 5wt%, the three-phase reaction interface is relatively insufficient, resulting in a low ECSA value. When the Nafion content is too high, reaching 20wt%, the ECSA value drops significantly to only 18.82m 2 g -1 .
[0051] 2. Scanning electron microscopy analysis
[0052] In order to further analyze the effects of formic acid concentration, growth temperature, and Nafion content on the growth and performance of Pt-NWs, scanning electron microscopy (SEM) was used to reveal the growth mechanism of Pt-NWs under different conditions and its correlation with performance.
[0053] Figure 4 Figure 2 is the SEM image of the surface of the Pt-NWs catalyst layer under different formic acid concentrations. It can be observed from the figure that the distribution of Pt in the catalyst layer and the length of Pt-NWs change with the change of formic acid concentration. When the formic acid concentration is low (such as 5:600), the length of Pt-NWs is relatively short and the distribution on the surface of the catalyst layer is uneven. This phenomenon may be due to insufficient reducing agent, which limits the reduction and growth process of Pt. The SEM images show that the distribution and morphology of Pt-NWs on the carbon spheres are different under different formic acid concentrations. At low concentrations, Pt-NWs form small clusters, which may affect the exposure of active crystal faces and platinum utilization. As the formic acid concentration increases to 7:600, the length of Pt-NWs increases and the distribution becomes more uniform, which is due to the increase in the reducing agent concentration that promotes the reduction and growth of Pt. Moderate Pt aggregation can form a wider conductive path and improve the catalytic performance. However, when the formic acid concentration is too high (e.g., 9:600), Pt-NWs agglomerate severely, affecting the gas transmission from GDL to the catalyst and increasing the mass transfer resistance.
[0054] Figure 5 The growth morphology of Pt-NWs on the carbon substrate at different temperatures is clearly shown. At a lower temperature of 10°C, Pt mainly aggregates on the surface of the carbon matrix layer and aggregates to form larger spherical nanoclusters ( Figure 5 a and b). This agglomeration phenomenon is likely due to the slow reaction rate under low temperature conditions, where Pt atoms are locally concentrated on the surface of the carbon sphere to form nanoscale atomic clusters, but fail to diffuse widely and grow into nanowires. As the temperature rises, it is observed that the number of nanoclusters gradually decreases, and the distribution of Pt-NWs on the carbon sphere gradually tends to be uniform. Especially at 20°C, the distribution of Pt-NWs is relatively uniform, and the number of nanoclusters is significantly reduced ( Figure 5 b and c). This indicates that the appropriate temperature helps the uniform diffusion and growth of Pt atoms on the surface of carbon spheres, resulting in a more uniform distribution of Pt-NWs. However, when the temperature rises to 40 °C, although the SEM images show that the nanoclusters are no longer obvious, the distribution of Pt-NWs on the carbon spheres is more dispersed ( Figure 5 e and f), but such over-dispersion may lead to reduced connectivity between Pt-NWs, which in turn has an adverse effect on electron transport and catalytic performance.
[0055] From the SEM images of the catalyst layer with different Nafion contents ( Figure 6) observed that the Nafion content had a significant effect on the microstructure of the Pt nanowire catalyst. Specifically, when the Nafion content was 5wt%, the number of Pt nanowires on the surface of the catalyst layer was relatively small, and the agglomeration phenomenon was not obvious. This is mainly because the lower Nafion content allows the reaction solution of chloroplatinic acid and formic acid to penetrate into the carbon matrix more easily, thereby reducing the possibility of forming Pt nanowires on the surface. At the same time, since there are a large number of carbon surfaces in the carbon matrix that are not covered by Nafion, this provides more active sites for the growth of Pt, thereby reducing the agglomeration of Pt nanowires. However, it should be pointed out that a lower Nafion content also means that there are fewer three-phase interfaces in the catalyst layer, resulting in poor proton conduction performance, which to a certain extent restricts the performance of the electrode. In contrast, when the Nafion content increases to 10wt%, the catalyst layer reaches a balance point in terms of expanding the three-phase interface, reducing Pt nanowire agglomeration, and increasing the porosity of the catalyst layer. This equilibrium state enables the catalytic layer to exhibit optimal performance, ensuring smooth proton conduction and reducing the agglomeration of Pt nanowires, thereby improving the utilization of the catalyst. Therefore, from the perspective of microstructure, 10wt% Nafion content is a better choice for preparing Pt nanowire electrodes.
[0056] 3. Transmission electron microscopy analysis
[0057] Transmission electron microscopy is an important tool for observing the microstructure of catalysts. Its magnification is larger than that of scanning electron microscopy (SEM). In order to more deeply analyze the effects of formic acid concentration and growth temperature on the growth and performance of Pt-NWs, TEM was used to characterize the morphology of Pt-NWs catalysts under different growth conditions.
[0058] Figure 7 The TEM images of Pt-NWs at different formic acid concentrations are shown. As the formic acid concentration increases, the agglomeration of Pt on the carbon spheres becomes more and more obvious. In particular, when the formic acid concentration is 9:600, dense platinum nanoclusters are formed on the surface of some carbon spheres. This observation is consistent with Figure 4 The SEM images in the figure are consistent with those in the figure, further verifying that high concentrations of formic acid will aggravate the agglomeration of Pt. Comparing TEM images at different concentrations, it was found that at a formic acid concentration of 7:600, the Pt nanowires had a longer length. This result is consistent with the previous electrochemical performance analysis, indicating that platinum nanowires of appropriate length help improve catalytic performance, because longer nanowires mean more surface atoms, thereby increasing the contact opportunities with reactants. At a formic acid concentration of 7:600, the increase in ECSA can be attributed to the increase in the length of the platinum nanowires and more exposure of the active crystal faces. However, excessively high formic acid concentrations cause platinum nanowires to agglomerate, which not only shortens the length of the nanowires, but may also block part of the active crystal faces, thereby reducing the catalytic performance.
[0059] By observation Figure 8 The TEM images of the Pt-NWs catalyst layer surface in the figure clearly show the growth of Pt-NWs on carbon particles at different temperatures, which is consistent with the previous discussion and Figure 5 The SEM observations in the results are consistent. At 10 ° C, due to the low temperature, the reduction rate of Pt is slow, resulting in the agglomeration of Pt atoms mainly on the surface layer of carbon particles to form large platinum nanoclusters. This agglomeration phenomenon makes the distribution of Pt-NWs uneven and the active surface area is reduced, so the electrochemical performance is poor and the ECSA value is small. As the temperature variable increases to 20 ° C, the reduction rate of Pt is moderate, and small-volume nanoclusters are aggregated on more carbon particles, indicating that Pt atoms begin to diffuse and grow more evenly on carbon particles. This uniform distribution helps to increase the active surface area and electron transport properties, thereby improving the electrochemical performance of Pt-NWs. It can be seen that the Pt-NWs catalytic layer prepared at a growth temperature of 20 ° C obtains the best electrochemical performance. However, when the temperature is further increased to 40 ° C, although the nanocluster phenomenon is reduced, the Pt-NWs begin to become short and dispersed. This morphological change may be due to the fact that the diffusion rate of Pt atoms is too fast at high temperature, which prevents the nanowires from forming an elongated shape during growth. At the same time, too high a temperature may also cause the Pt atoms to fail to grow completely onto the carbon support, thus affecting the electrochemical performance. Thick and short nanowires mean a reduction in active surface area, so the electrochemical performance will also be reduced accordingly.
[0060] 4. X-ray diffraction analysis
[0061] According to the analysis and characterization results of CV curves, scanning electron microscopy, and transmission electron microscopy, the Pt nanowire catalyst exhibited the best performance when the ratio of formic acid to water was 7:600, the Nafion content was 10wt%, and the reaction temperature was 20°C. XRD technology was used to analyze the crystallinity of Pt-NWs under different preparation conditions. Pt-NWs / C was compared with commercial Pt / C. The results are as follows Fig. 9 shown.
[0062] The diffraction peaks observed at 39.4°, 46.6° and 67.4° for the catalyst Pt-NWs / C correspond to the <111>, <200> and <220> planes of the face-centered cubic (fcc) structure of Pt. At the same time, the Pt-NWs / C catalyst sample shows sharper and more intense diffraction peaks in the <111> plane direction than commercial Pt / C. Sharp and intense diffraction peaks usually mean that the material has a higher degree of crystallinity, that is, its crystal structure is more ordered and perfect. The <111> crystal plane is generally considered to be a more active crystal plane in Pt catalysis, so Pt-NWs has a more excellent catalytic performance.
[0063] 5. Water contact angle analysis
[0064] The water contact angle, as a key indicator to measure the contact state between the liquid and the surface of the solid material, specifically refers to the angle between the tangent line of the solid-liquid interface and the liquid side and the solid-liquid boundary line at the intersection of the liquid and the solid. Accurate measurement of this angle can reveal the wetting characteristics of the liquid on the solid surface. If the water contact angle of the catalytic layer is greater than 90°, it means that the surface of the catalytic layer is hydrophobic, that is, the liquid is difficult to effectively wet the solid surface and is easier to move freely on it. Such characteristics help to reduce the accumulation of water in the catalytic layer, thereby reducing the probability of "flooding". Pt-NWs / C was compared with commercial Pt / C, and the results are as follows Fig.10 shown.
[0065] By comparing the contact angles of different types of nanoparticles in the cathode catalyst layer, it was found that the catalyst layer prepared by Pt-NWs / C has better hydrophobicity. This is because the one-dimensional structure of Pt-NWs makes its contact angle larger than that of the catalyst layer after spraying Pt / C. This larger contact angle means that the Pt-NWs / C catalyst layer is more repellent to liquid water, thus reducing the occurrence of "flooding".
[0066] 2. Process research on hydrogenated soybean oil with carbon-supported platinum nanowires
[0067] Through single factor experiments, the amount of Pt-NWs / C catalyst in MEA, the core component of the SPE electrochemical hydrogenation reaction device, the hydrogenation temperature in the soybean oil hydrogenation process, and the process conditions of oil phase flow rate were optimized according to the changes in resistance and iodine value, and the changes in fatty acid composition over time under this process were analyzed. The external electric field was applied by the BTS high-precision battery detection system, with a constant current of 500mA and a maximum voltage of 5000mV.
[0068] 1. Effect of hot pressing temperature on hydrogenated oil and hydrogenation process
[0069] In the hot pressing process of membrane electrode, hot pressing pressure and hot pressing temperature have a significant impact on its performance and life. The selection of hot pressing temperature should ensure that the bonding force between the membrane and the electrode is enhanced and certain internal stress is eliminated to improve the performance of the battery. Appropriate hot pressing pressure can make the membrane and the electrode tightly bonded and improve battery performance.
[0070] Fig.11It is clearly shown that although the resistance value of the membrane electrode reaches the lowest under the hot pressing condition of 115°C, the membrane has not been fully softened because this temperature has not reached the limit of the glass transition temperature of the proton exchange membrane (i.e., 120°C), resulting in insufficient bonding with the catalyst layer. This insufficient bonding may increase the possibility of damage to the membrane electrode during the hydrogenation reaction, thereby adversely affecting the stability of the reaction. As the hot pressing temperature gradually increases, the overall resistance value of the membrane electrode shows an upward trend. In particular, when the temperature climbs to 145°C, the resistance value of the membrane electrode shows a significant drop to a relatively low level (2.98Ω, excluding the abnormal data points at 110°C). This may be due to the fact that in this temperature range, the fluidity of the perfluorosulfonic acid resin is enhanced, making the proton exchange membrane and the catalyst layer more closely bonded, thereby forming a more efficient proton transport channel. As the hot pressing pressure increases, the resistance of the membrane electrode first drops significantly and then rises sharply. At a pressure of 0.4MPa, the resistance of the membrane electrode reaches its lowest value (2.62Ω). This is because the hot pressing pressure directly affects the thickness of the membrane electrode. Moderate pressure can make the membrane electrode thinner, thereby improving its conductivity. However, too much hot pressing pressure will cause the carbon paper to deform, thereby destroying the microporous structure of the catalyst layer, thereby hindering the smooth flow of gas channels, and ultimately increasing the resistance of the membrane electrode. On the contrary, if the applied pressure is too small, the bond between the catalyst layer and the proton exchange membrane will not be strong enough, which will also cause the membrane electrode resistance to increase, and it will be more prone to breakage during the hydrogenation reaction. Taking all the above factors into consideration, this study selected a hot pressing pressure of 0.4MPa to ensure the conductivity of the membrane electrode while avoiding damage due to excessive pressure. This choice takes into account both the structural integrity of the membrane electrode and its performance in the hydrogenation reaction.
[0071] 2. Effect of hydrogenation temperature on hydrogenated oil and hydrogenation process
[0072] Since oil hydrogenation is a type of addition reaction, the effect of temperature on the SPE electrochemical hydrogenation process cannot be ignored. The following experimental conditions were set, i.e., constant current charging at 500 mA under normal pressure, oil phase flow rate of 50 mL / min, water phase flow rate of 35 mL / min, anode catalyst of 20 wt% Pt / C, cathode catalyst of Pt-NWs / C, to explore the effect of different hydrogenation temperatures (30-80 ° C) on the hydrogenation process. The experimental results are shown in Figure 2. Fig.12As shown in the figure, as the reaction temperature increases, the resistance of the membrane electrode gradually decreases. This trend is consistent with the results of Li Xuan et al., that is, the resistance of carbon-based materials decreases linearly with increasing temperature. Therefore, the reduction in membrane electrode resistance is mainly attributed to the change in the resistance of the carbon paper layer. However, it is worth noting that when the reaction temperature reaches 70 and 80 ° C, although the resistance of MEA is small in the initial stage, the resistance increases rapidly as the reaction proceeds. After 500 seconds, its resistance is even greater than that of the 60 ° C group. This may be due to the rapid increase in the electrolysis efficiency of the anode at higher temperatures, while the increase in the addition reaction rate of the cathode is relatively small, resulting in a large amount of H+ accumulated in the reaction chamber. These accumulated H+ may corrode the surface of the carbon paper layer, thereby increasing the resistance. In addition, the experiment also observed that in the range of 30-60 ° C, the iodine value of hydrogenated soybean oil showed a downward trend with increasing temperature, indicating that the increase in temperature helps to promote the hydrogenation addition reaction. However, when the temperature exceeds 60 ° C, the iodine value of the hydrogenation product increases slightly. This is also due to the fact that the membrane electrode is prone to damage at higher temperatures, resulting in a sharp increase in resistance. When the resistance reaches a maximum value of 5000mV at 2800 seconds, the current density decreases, which in turn leads to a decrease in the hydrogenation rate. Considering the change in membrane electrode resistance and the change trend of the iodine value of hydrogenated soybean oil, this study chose to hydrogenate soybean oil at 60°C. This temperature can not only ensure a high hydrogenation efficiency, but also avoid membrane electrode damage caused by excessively high temperature.
[0073] 3. Effect of oil phase flow rate on hydrogenated oil and hydrogenation process
[0074] The SPE electrochemical hydrogenation reaction process involves two parts: water electrolysis at the anode and addition reaction at the cathode. Since the two reactions have different energy barriers, their reaction rates will also be different. Various conditions need to be carefully controlled in the experiment to optimize the reaction effect. Under normal pressure at 60°C, the experiment changed the oil phase flow rate (20-70mL / min) while maintaining the water phase flow rate at 35mL / min, the anode catalyst was Pt / C, the cathode catalyst was Pt-NWs / C, and the constant current charge was 500mA to explore the effect of the oil phase flow rate on the hydrogenation results. The results are shown in Fig.12 shown.
[0075] The experimental results show that at the initial stage of the reaction, the resistance of the membrane electrode is similar at different flow rates. This is because when the reaction just starts, the generation and flow of H protons are not significantly affected by the oil phase flow rate. However, as the reaction proceeds, the effect of the oil phase flow rate on the membrane electrode resistance gradually becomes apparent. When the oil phase flow rate increases, the resistance of the membrane electrode decreases. This observation is consistent with the experimental hypothesis that high concentrations of H protons may corrode the carbon paper layer. When the oil phase flow rate is high, the flow velocity in the reaction chamber increases, which helps the H protons flow out with the oil phase, thereby reducing the erosion of the carbon paper layer and reducing the resistance of the MEA.
[0076] The experiment also found that when the oil phase flow rate was 20 and 30 mL / min, the iodine value of the hydrogenated product was large. This may be due to the fact that in the later stage of the reaction, the lower oil phase flow rate caused the MEA resistance to increase, causing the current density to decrease to less than 500 mA, resulting in a decrease in hydrogenation efficiency. A larger iodine value means incomplete hydrogenation, that is, the unsaturated bonds in the oil phase are not fully hydrogenated. Therefore, a lower oil phase flow rate is not conducive to obtaining high-quality hydrogenated products. On the other hand, when the oil phase flow rate is too high, the iodine value of the hydrogenated product also increases slightly. This may be because the excessively high flow rate takes away the H protons that pass through the Nafion membrane, resulting in a decrease in the H proton concentration in the cathode chamber. The lack of H proton concentration will directly affect the rate and efficiency of the hydrogenation reaction, so that the hydrogenated product still contains more unsaturated bonds, which is manifested as an increase in the iodine value. In addition, according to the theoretical model of semi-hydrogenated intermediates, insufficient H proton concentration may also trigger the occurrence of isomerization reactions, further affecting the quality and properties of the hydrogenated products. Taking into account the changes in MEA resistance and iodine value of hydrogenated products, the optimal oil phase flow rate was determined to be 50 mL / min. At this flow rate, sufficient H proton supply in the cathode chamber can be guaranteed to maintain efficient hydrogenation reaction, while the problem of H proton loss and carbon paper layer erosion caused by excessive flow rate can be avoided.
[0077] 4. Effect of hydrogenation time on hydrogenated oil and hydrogenation process
[0078] Under the optimized experimental conditions, i.e. constant current charging at 500mA and 50°C under normal pressure; the water phase flow rate and oil phase flow rate were set to 35mL / min and 50mL / min respectively; the anode and cathode catalysts were 20wt% Pt / C and Pt-NWs / C respectively to further explore the effect of time on the hydrogenation process and products.
[0079] Table 1 Fatty acid composition and iodine value of soybean oil selectively hydrogenated at different times
[0080]
[0081] Note: Different capital letters (AF) indicate significant differences within the treatment groups (p<0.05), and different lowercase letters (ae) indicate significant differences between the treatment groups (p<0.05)
[0082] Based on the above optimization scheme, the hydrogenation process and products were studied over time. Under normal pressure at 50°C, the water phase flow rate was set to 35 mL / min, the oil phase flow rate was set to 40 mL / min, the anode catalyst was Pt / C, the cathode catalyst was Pt-NWs / C, and the constant current charge was 500 mA. Fig.16 Shown is the influence of different hydrogenation times on the iodine value of hydrogenated oil. It can be clearly seen that along with the extension of hydrogenation time, the iodine value of corresponding soybean hydrogenated oil is in a gradually declining trend. In the experiment, when the hydrogenation reaction just began to be carried out, the amount of unsaturated fatty acids contained in soybean oil was higher, and the reaction substrate in the reaction system was sufficient, and the hydrogenation reaction could be carried out smoothly and quickly. When the reaction finished, the iodine value of hydrogenated oil was about 109g I2 / 100g, which was slightly hydrogenated, indicating that it still contained some unsaturated fatty acids, and the carrying out of the hydrogenation reaction was not affected. So in the whole hydrogenation process, the iodine value of hydrogenated oil was in a straight line downward trend.
[0083] 3. Molecular composition and quality analysis of hydrogenated soybean oil supported by carbon-supported platinum nanowires
[0084] Soybean oil was hydrogenated using an SPE electrochemical hydrogenation reactor at atmospheric pressure and 50°C. During this process, the flow rate of the oil phase was set to 50mL / min, while the flow rate of the water phase was set to 35mL / min. The anode catalyst selected was a 20wt% Pt / C catalyst, while the cathode catalyst used two materials, Pt-NWs / C and Pt / C, respectively. After 2 hours of reaction, the fatty acid composition, trans fatty acid content, melting and crystallization characteristics and crystal morphology of the hydrogenated oil, and flavor of the hydrogenated soybean oil were comprehensively evaluated. This study aims to further explore the comparison of the catalytic performance of the two catalysts in the hydrogenation process and their impact on the quality of the hydrogenated products.
[0085] 1. Analysis of basic indicators of SPE hydrogenated soybean oil
[0086] Table 2 Quality analysis of soybean oil and hydrogenated oil catalyzed by different catalysts
[0087]
[0088] Depend on Fig.14It can be seen that the original soybean oil is golden yellow, and the liquid is clear and transparent. However, the two hydrogenated oils after hydrogenation, whether prepared with Pt-NWs / C or Pt / C as catalyst, are uniformly milky white and have an opaque texture. The flavor of the hydrogenated oil is still similar to that of soybean oil, retaining its unique bean flavor, which to a certain extent guarantees the edible acceptability of the hydrogenated product. Regarding the basic quality analysis of the hydrogenated products, the detailed data are shown in Table 2. The iodine value of the original soybean oil is as high as 131g I2 / 100g, showing its high degree of unsaturation. After Pt-NWs / C catalytic hydrogenation, the iodine value of the product is reduced to 109g I2 / 100g, while the iodine value of the product after Pt / C catalytic hydrogenation is 110g I2 / 100g. This change shows that the hydrogenation reaction effectively reduces the unsaturation of the oil and improves its stability. At the same time, the peroxide value and refractive index of the two hydrogenated oils decreased, while the acid value increased. These changes are common phenomena in hydrogenation reactions and are in line with the expected effects of oil hydrogenation. This shows that the hydrogenated product prepared by Pt-NWs / C as a catalyst in the SPE reactor has good quality, not only retaining the unique flavor of the original soybean oil, but also effectively improving the physical properties of the oil through the hydrogenation reaction, improving its stability and edible safety.
[0089] 2. Analysis of fatty acid composition of SPE hydrogenated soybean oil
[0090] Table 3 shows the analysis of the fatty acid composition of soybean oil and hydrogenated oils electrochemically hydrogenated with two different catalysts by gas chromatography. The results show that soybean oil mainly contains C16:0 (palmitic acid), C18:1n9c (oleic acid), C18:2n6c (linoleic acid) and C18:3n3 (α-linolenic acid), which is consistent with the research results of Chen Xia et al. After soybean oil was hydrogenated in an SPE reactor, it was observed that the content of dienoic acid and trienoic acid in the two hydrogenated oils decreased, while the content of monoenoic acid and saturated acid increased. This change is consistent with the results of hydrogenated soybean oil prepared by Wang et al. by electrochemical hydrogenation under high pressure H2 environment. This shows that in the hydrogenation process, it is mainly the unsaturated double bonds in octadecanoic acid that participate in the addition reaction. Since the content of C18:2n6c (linoleic acid) in soybean oil is the highest (54.59%), its unsaturated double bonds are more vulnerable to attack during the hydrogenation process, resulting in a decrease in content. At the same time, the changes in fatty acids also reflect the hydrogenation rules in the SPE hydrogenation reactor, which is consistent with the hydrogen atom collision theory model proposed by Ai Hongtao and others. This model points out that dienoic acid is more likely to collide with the active center due to its high content, resulting in a higher degree of reaction. Compared with the Pt / C catalyst, the changes in C18:2n6c (linoleic acid) in the hydrogenated oil obtained using Pt-NWs / C as a catalyst are more significant. This shows that the Pt-NWs / C catalyst has a higher catalytic activity in the reaction of catalyzing the hydrogenation of linoleic acid to produce oleic acid. This increase in catalytic activity may be related to the higher SLo (linoleic acid hydrogenation selectivity) of Pt-NWs, which enables it to more effectively promote the conversion of unsaturated fatty acids during the hydrogenation process.
[0091] Table 3 Fatty acid composition of soybean oil and hydrogenated oils with two different catalysts
[0092]
[0093] 3. Analysis of trans fatty acid content in hydrogenated soybean oil by SPE
[0094] Table 4 shows the data of trans fatty acid content of soybean oil measured by gas chromatography and hydrogenated oil obtained by SPE hydrogenation treatment with two different catalysts. After SPE hydrogenation treatment, the content of short-chain trans fatty acids such as C16:19t and C18:1n9t in soybean oil is low. However, in the hydrogenated oil, the content of these short-chain trans fatty acids has increased. For long-chain trans fatty acids, such as C18:2n6t, C18:2n9c,12t, C18:2n9t,12c, etc., the content in soybean oil is relatively low, but it increases significantly in hydrogenated oil. This result reflects that isomerization reaction occurs during the hydrogenation process. Monoenoic acid and trienoic acid are the main ones in the newly generated TFAs. The TFAs content in the hydrogenated oil prepared by Pt-NWs / C catalyst was only 1.47% (109g I2 / 100g), and the TFAs content in the hydrogenated oil prepared by Pt / C was 1.69% (110g I2 / 100g). This result is close to the hydrogenated soybean oil prepared by Wang et al. using MEH electrochemical process under high pressure H2 environment (TFAs 3.32%, 90.6g I2 / 100g). However. In contrast, the TFAs content of hydrogenated soybean oil prepared by Hastert et al. using traditional stirred high-pressure reactor at 140°C and 44psi was as high as 20% (110g I2 / 100g), and the TFAs content of hydrogenated soybean oil prepared by Heldal et al. using fluidized bed hydrogenation process at 170°C and 50psi was 17% (112g I2 / 100g). The low generation of TFAs in hydrogenated oil prepared by SPE hydrogenation process is due to the relatively mild reaction conditions (normal pressure, 60℃) and the high H proton transfer efficiency. Li An used Gussian software and density functional theory to conduct in-depth simulation calculations on the isomerization reaction path of soybean oil. The study found that ambient temperature is one of the core factors affecting the formation of unsaturated fatty acids. The isomerization process of a single cis double bond requires a higher activation energy (more than 200kJ / mol) to form an intermediate state, and a higher ambient temperature helps to reduce this energy barrier, thereby promoting the occurrence of the reaction. In addition, the research of Dijkstra et al. also showed that the transmission and dispersion effect of H protons has a direct impact on their utilization. When the supply of H protons is insufficient, the generation of TFAs will increase. Due to its large specific surface area, the Pt-NWs / C catalyst can provide more active sites for adsorbing H protons, thereby increasing the H concentration in the catalytic layer. This is consistent with the result that Pt-NWs / C has a smaller SLn (linolenic acid hydrogenation selectivity) value in the hydrogenation selectivity analysis, further confirming its excellent performance in the hydrogenation process.
[0095] Table 5 Trans fatty acid content in soybean oil and two different catalyst hydrogenated oils
[0096]
[0097] 4. Selective analysis of hydrogenated soybean oil by SPE
[0098] Table 5 shows in detail the hydrogenation selectivity results of Pt / C hydrogenated oil and Pt-NWs / C hydrogenated oil calculated under Matlab. From these results, it can be seen that different catalysts have a significant effect on the hydrogenation selectivity of different fatty acids. The Pt / C catalyst showed higher selectivity in the hydrogenation of linolenic acid and stearic acid, while the Pt-NWs / C catalyst showed higher selectivity in the hydrogenation of linolenic acid. These differences may be due to the different structures of the catalysts, the distribution of active sites, and the interaction modes with different fatty acid molecules. Both catalysts showed good linolenic acid hydrogenation selectivity in the hydrogenation reaction, indicating that they can effectively promote the conversion of linolenic acid to linoleic acid. Previous studies by Sun et al. pointed out that an increase in C18:3 content may be detrimental to the flavor stability of hydrogenated products. Therefore, catalysts with higher SLn values (linolenic acid hydrogenation selectivity), such as the Pt-NWs / C catalyst in this study, have a stronger ability to promote the hydrogenation of linolenic acid, providing broader prospects for commercial applications and helping to improve the flavor stability of hydrogenated products. At the same time, the SLn value can also reflect the change of hydrogen concentration in the electrochemical hydrogenation reaction system. When the hydrogen concentration increases, the SLn value will also decrease accordingly, which further verifies the advantage of Pt-NWs / C catalyst in adsorbing H protons, which not only improves the catalytic efficiency, but also helps to reduce the generation of TFAs. In addition, it is worth noting that the SLo (linoleic acid hydrogenation selectivity) of soybean oil electrochemically hydrogenated by two different catalysts is at a low level in each group. This may be because in the process of C18:3 converting to C18:2, the newly generated C18:2 and the original C18:2 are further converted into C18:1, resulting in no obvious change in the content of C18:2 in the overall composition. The hydrogenation rates of linolenic acid, linoleic acid, and oleic acid in soybean oil are faster under SPE hydrogenation conditions, but SLn and SLo are lower under conventional industrial hydrogenation conditions, and good selectivity is shown under electrochemical hydrogenation conditions.
[0099] Table 5 Fatty acid hydrogenation selectivity of two hydrogenated oils
[0100]
[0101] 5. SPE hydrogenated soybean oil flavor analysis
[0102] pass Fig.15Electronic nose radar chart analysis shows that the main components of soybean oil aroma are concentrated in sensor No. 2, which is associated with ammonia oxides. In addition, sensors No. 3 to No. 9 respond to a variety of compounds such as ammonia aromatic substances, hydrides, and alkane aromatic components, which together affect the overall flavor of soybean oil. In the two hydrogenated oils after hydrogenation, sensors No. 2, 5, and 10 showed higher responses to the main flavor components. The hydrogenated oils catalyzed by Pt-NWs / C and Pt / C showed similar trends in flavor. Compared with the original soybean oil, hydrogenation treatment increased the response value of sensor No. 2, while other response values decreased, reflecting the changes in flavor components during the hydrogenation process, especially the increase in the content of ammonia oxides. It is worth noting that the response value of Pt-NWs / C hydrogenated oil on hydrogen sulfide components is higher than that of Pt / C hydrogenated oil, but the response value on aromatic alkanes is slightly lower. These subtle differences may indicate that the two hydrogenated oils are different in flavor.
[0103] like Fig.16 As shown, by processing the electronic nose sensor data with Airsense software, PCA simplifies the multivariate data into two principal components (PC-1 and PC-2), which efficiently reflects the original information. If the cumulative variance of the principal component accounts for more than 85%, it can represent the characteristics of the original data. PCA analysis results show that the two principal components together contribute up to 99.72% of the flavor information, which fully verifies the representativeness and accuracy of the PCA analysis results. In-depth observation of the PCA analysis results shows that the three samples show clear distinction in the figure, and there is no overlap between them, which further confirms the difference in flavor between the three samples.
[0104] 6. Analysis of melting and crystallization curve of SPE hydrogenated soybean oil
[0105] Fig.17The melting and crystallization curves shown were measured in a DSC (differential scanning calorimeter) test at a heating rate of 20°C / min and a cooling rate of 10°C / min. This figure intuitively reflects the changes in thermal behavior of soybean oil and its two hydrogenated products (Pt / C hydrogenated oil and Pt-NWs / C hydrogenated oil) during heating and cooling. From the melting curve part, it can be seen that compared with the original soybean oil, the melting peaks of the two oils after hydrogenation are shifted to the left and become wider. This shift and broadening phenomenon indicates that the hydrogenation process changes the melting point range of the oil and fat, making it wider. This may be because hydrogenation increases the content of saturated fatty acids in the oil and fat, thereby affecting its melting characteristics. Further observation shows that the melting peak of the Pt-NWs / C hydrogenated oil is broader than that of the Pt / C hydrogenated oil. This shows that under the same hydrogenation conditions, the hydrogenated oil obtained using the Pt-NWs / C catalyst has a higher degree of hydrogenation. This high degree of hydrogenation may have led to a wider melting point distribution, causing the Pt-NWs / C hydrogenated oil to show a larger temperature range during the melting process. As for the crystallization curve, it also shows a similar pattern. The crystallization peak of the hydrogenated oil is also wider than that of soybean oil, which shows that hydrogenation not only affects the melting characteristics of the oil, but also has a significant effect on its crystallization characteristics. The widening of the crystallization peak may mean that the hydrogenated oil has a wider temperature adaptability during the crystallization process, which helps to improve the storage stability and processing performance of the oil.
[0106] Table 6 lists in detail the phase transition temperatures and enthalpy data of the melting and crystallization of the three oils. The melting enthalpy of the hydrogenated oils increased compared with the original soybean oil, which may mean that after hydrogenation, the hydrogenated oil requires more energy to melt, causing the hydrogenated oil to exhibit different physical properties during melting and crystallization. The melting peak temperature of the Pt-NWs / C hydrogenated oil is lower than that of the Pt / C hydrogenated oil, and the melting enthalpy also shows an increasing trend, which may mean that the Pt-NWs / C hydrogenated oil reaches the maximum melting rate at a lower temperature. The three oils differ in crystallization enthalpy, among which the Pt-NWs / C hydrogenated oil has the lowest crystallization enthalpy, which may mean that it releases less energy during the crystallization process. The increase in the crystallization point may mean that its melting point is slightly higher than that of the Pt / C hydrogenated oil, and more energy is required for the melting process.
[0107] Table 6 Melting-crystallization parameters of soybean oil and two different catalysts for electrochemical hydrogenation of oils
[0108]
[0109] 7. SPE hydrogenated soybean oil crystal morphology analysis
[0110] After hydrogenation, the double bonds in the unsaturated fatty acid molecules of vegetable oils are combined with hydrogen atoms, and the degree of unsaturation is reduced, which leads to a change in the melting point and causes these fats to crystallize at room temperature. These crystallized fats present a unique crystal shape and microstructure, and the crystal size is mainly in the range of 1-140 nanometers. The crystallization of oils and fats is a complex process that includes two stages: crystal nucleation and growth. When the ambient temperature is lower than the melting point of the oil, the triglyceride molecules will change from the original disordered state to an ordered arrangement in a supercooled state, thereby forming a crystal nucleus.
[0111] Polarized light microscopy can be used to observe the crystal state of oils in detail, such as Fig.18 As shown. Microscopic observation results show that the oil crystallization in hydrogenated soybean oil is significantly increased, while no crystallization is observed in unhydrogenated soybean oil. This indicates that the saturation degree of soybean oil is improved through the hydrogenation process, and its melting point is also increased, so that crystallization occurs at room temperature. In addition, the hydrogenated oils prepared by different catalysts also show certain differences in the crystallization state: the crystals in the oils catalyzed by Pt-NWs / C are smaller (about 20nm) and the crystal shape is more uniform. In contrast, in the products prepared by Pt / C as a catalyst, the fat crystal size is larger (about 49nm), and the size difference is more significant. This difference may be attributed to the fact that there are more active sites in the Pt-NWs / C catalyst, which can adsorb more fatty acids for reaction at the same time, making the crystallization in its product more uniform and consistent. The study of Minato et al. further pointed out that the delicate and uniform crystal morphology can form a more dense network structure. This network structure can not only encapsulate more liquid oil or gas, but also give the product a more delicate and soft texture, so it is considered to be an ideal food base oil.
[0112] IV. Conclusion
[0113] In this study, Pt-NWs were grown in situ on carbon powder by chemical reduction, and Pt-NWs / C catalyst was successfully prepared. The SPE electrochemical hydrogenation reactor was used to study the hydrogenation process of soybean oil under low temperature and normal pressure conditions, and the quality, flavor and physical properties of hydrogenated soybean oil were explored. The main conclusions are as follows:
[0114] The optimal process conditions for preparing Pt-NWs were explored by characterizing the catalyst morphology and electrochemistry by scanning electron microscopy, transmission electron microscopy, and CV curves: formic acid was used as a reducing agent, and its ratio to water was set at 7:600; the growth temperature was controlled at 20°C; the content of Nafion in the carbon matrix was 10wt%. SEM and TEM observations showed that as the reducing agent concentration increased from 0.075M to 0.590M, the length of Pt-NWs first increased and then decreased; at the same time, as the temperature increased, the diameter of Pt-NWs gradually increased, and its diameter ranged from 2-3nm at 10°C to 4-5nm at 40°C.
[0115] Through XRD analysis, it was found that the Pt-NWs / C sample showed better crystallinity and main <111> When the two were sprayed on the PTFE membrane, Pt-NWs / C showed better hydrophobicity than commercial Pt / C, thus more effectively preventing the occurrence of "flooding".
[0116] When Pt-NWs / C was used as the SPE cathode catalyst for soybean oil hydrogenation, the optimal reaction conditions were: the pressure of the membrane electrode prepared by thermal transfer method was 0.4 MPa, the temperature was 145°C, the reaction temperature was 50°C, the oil phase flow rate was 50 mL / min, and the optimal hydrogenation time was 1 h.
[0117] Fatty acid composition analysis showed that octadecanoic acid was the main reaction target in the SPE hydrogenation reactor, and different catalysts had different effects on the fatty acid composition of hydrogenated oil. After soybean oil was hydrogenated in the SPE reactor, it was observed that the contents of dienoic acid and trienoic acid in the two hydrogenated oils decreased, while the contents of monoenoic acid and saturated acid increased. Compared with the Pt / C catalyst, the change of C18:2n6c (linoleic acid) in the hydrogenated oil obtained using Pt-NWs / C as a catalyst was more significant. This shows that in the reaction of catalyzing the hydrogenation of linoleic acid to produce oleic acid, the Pt-NWs / C catalyst has a higher catalytic activity, and the TFAs in the hydrogenated oil prepared by the Pt-NWs / C catalyst are only 1.47% (109g I2 / 100g), which is lower than the TFAs content in the Pt / C hydrogenated oil. Pt-NWs / C has a higher SLo (linoleic acid hydrogenation selectivity), indicating that Pt-NWs / C can more effectively promote the conversion of unsaturated fatty acids during the hydrogenation process.
[0118] After SPE electrochemical hydrogenation, soybean oil changed from golden yellow transparent to slightly yellow opaque, and the milky white part of the product catalyzed by Pt-NWs / C was more viscous. Flavor analysis showed that the response values of amino oxides and hydrogen sulfide substances in soybean oil increased after hydrogenation, and the flavor changed. The response of Pt-NWs / C hydrogenated oil was slightly lower in amino oxides, and the response of alkane aromatic substances was slightly higher. PCA analysis confirmed that the flavors of the two were well differentiated and there was no crossover. Further analysis of the crystal morphology of hydrogenated oil and soybean oil showed that the oil crystals of soybean oil electrochemically hydrogenated by Pt-NWs / C as a catalyst were more uniform and smaller, and its crystal size (20nm) was smaller than that of Pt / C hydrogenated oil (49nm).
Claims
1. A method for preparing platinum nanowires, characterized in that The method comprises the following steps: 1) Weigh 0.5-3 mg of carbon powder, place it in a centrifuge tube, add isopropanol and Nafion solution, and ultrasonicate for 1-2 hours to prepare a catalyst slurry; 2) spraying the catalyst slurry onto the PTFE membrane using a spray gun to obtain a carbon powder matrix layer; 3) Fixing the substrate layer in a culture dish, adding 1-2 mg of chloroplatinic acid and 0.2%-0.6% formic acid aqueous solution to obtain a carbon substrate attached to the platinum nanowires; 4) The growth temperature of the platinum nanowires is controlled at 10-40°C.
2. The method for preparing platinum nanowires according to claim 1, characterized in that The volume of the isopropanol is 0.5 to 2 times the mass of the carbon powder, the mass concentration of the Nafion solution is 5 to 30%; and the size of the PTFE membrane is 2.3×2.3 cm.
3. The method for preparing platinum nanowires according to claim 1, characterized in that The preparation method of the platinum nanowire catalyst is as follows: (1) Preparation and fixation of carbon matrix layer Mix carbon powder and platinum carbon in a predetermined ratio and add isopropanol to blend. Then, add an appropriate amount of Nafion solution, put it in a centrifuge tube and put it in an ultrasonic cleaner for 1 hour to form a uniform "ink". Finally, under the irradiation of infrared light, use a pneumatic spray gun to evenly spray the "ink" on the cleaned polytetrafluoroethylene transfer membrane to form a matrix layer. Fix the finished matrix layer in the center of the culture dish and use nano glue to ensure its stability. (2) Wet chemical in situ growth of Pt-NWs / C catalyst An appropriate amount of a mixed solution of chloroplatinic acid and formic acid was added to the culture dish with the fixed matrix layer, and the mixture was left to stand at room temperature for 72 hours. The mixture was rinsed and soaked with deionized water several times to completely remove residual formic acid and other impurities. Next, the polytetrafluoroethylene transfer membrane with the catalytic layer was placed under an infrared lamp and sprayed with a uniform solution mixed with Nafion solution and isopropanol. Finally, the mixture was dried at 50°C for 30 minutes to obtain a platinum nanowire catalyst.
4. The method for preparing platinum nanowires according to claim 3, characterized in that The loading of platinum nanowires in the carbon matrix was 20%.
5. Use of the platinum nanowire catalyst prepared by the method according to any one of claims 1 to 4 as a SPE cathode catalyst in electrochemical hydrogenation of soybean oil.
6. Use of the platinum nanowire catalyst prepared by the method according to any one of claims 1 to 4 in a hydrogenation reaction catalyst.
7. Use of the platinum nanowire catalyst prepared by the method according to any one of claims 1 to 4 as a SPE cathode catalyst in electrochemical hydrogenation of oils and fats.
8. Use of the platinum nanowire catalyst prepared by the method according to any one of claims 1 to 4 in electrochemical hydrogenation of soybean oil.
9. Use of the platinum nanowire catalyst according to claim 8 as a SPE cathode catalyst in electrochemical hydrogenation of soybean oil, characterized in that The reaction conditions of the electrochemical hydrogenation of soybean oil are: reaction temperature 30-80° C., oil phase flow rate 20-90 mL / min, water phase flow rate 20-90 mL / min, and the anode catalyst is commercial Pt / C.
10. Use of the platinum nanowire catalyst according to claim 9 as a SPE cathode catalyst in electrochemical hydrogenation of soybean oil, characterized in that The reaction conditions of the electrochemical hydrogenation of soybean oil are: reaction temperature 50° C., oil phase flow rate 50 mL / min, water phase flow rate 35 mL / min, and the anode catalyst is commercial Pt / C.