Method for preparing multistage micro-nano gradient structure of titanium alloy surface layer in situ through alternating superposition milling

The multi-stage micro-nano gradient structure of the surface of titanium alloy is generated through alternating superposition milling technology, which solves the problem of surface deterioration layer of titanium alloy milling, improves the fatigue and wear resistance of the material, and is suitable for high performance in aerospace and medical fields. manufacture.

CN118977063APending Publication Date: 2024-11-19SHENYANG AEROSPACE UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411082751.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-08
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

Irregular microstructures in the metamorphic layer of the surface of titanium alloy milling lead to insufficient fatigue resistance, corrosion resistance and wear resistance of materials, especially in the fields of aerospace and medical care, and traditional shot peening technology is difficult to effectively solve these problems, especially in large-scale Complex components are being manufactured.

Method used

The alternating superposition milling method is adopted, and the reverse/scheduled alternating motion and axial impact are synchronized by the CNC universal rotary head and the gradient micro-edge impact head during the milling process, to generate a multi-stage micro-nano gradient structure surface layer, combined with electric spark Cutting and ultrasonic cleaning and other steps, adjust the impact parameters to form a gradient structure.

Benefits of technology

The multi-stage micro-nano gradient structure of the surface layer of titanium alloy is realized, which improves the mechanical properties and wear resistance of the material, prevents sudden changes in mechanical properties caused by grain size changes, and improves the service performance of the material through mutual coordinated deformation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118977063A_ABST
    Figure CN118977063A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of metal surface modification, and particularly discloses a method for preparing a multistage micro-nano gradient structure of a titanium alloy surface layer in situ through alternating superposition milling, which comprises the following steps: milling the surface of a titanium alloy workpiece to be processed into a plane; then, the surface of the to-be-machined titanium alloy workpiece is subjected to alternating superposition milling; and finally, cleaning, grinding, polishing and corroding treatment are conducted in sequence. Compared with the prior art, the multi-stage micro-nano gradient structure surface layer is prepared by milling the surface of the to-be-machined titanium alloy workpiece in an alternating superposition manner, and the grain size of the multi-stage micro-nano gradient structure surface layer of the titanium alloy is gradually increased from the surface nanoscale to the matrix micron scale in a gradient continuous change manner, so that matching of strength and toughness is facilitated; on the one hand, mechanical property mutation caused by mutation of grain size or lamellar thickness can be prevented; and on the other hand, action mechanisms corresponding to different grain sizes can simultaneously show to promote the materials to perform mutual coordination deformation, so that the service performance of the materials is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of metal surface modification, in particular to a method for in-situ preparation of a multi-level micro-nano gradient structure on a titanium alloy surface by alternating superposition milling. Background Art

[0002] Titanium alloys have the advantages of high specific strength, good thermal stability, corrosion resistance and biocompatibility, and are widely used in aerospace, marine and medical fields. Among them, aircraft engines serve in a complex environment of high speed, high temperature and high pressure, and have very high requirements for the fatigue resistance of titanium alloy blades. Deep-sea vehicles have continuously improved the corrosion resistance of titanium alloy components. Once the titanium alloy is corroded, it will cause damage and leakage, causing immeasurable consequences. Medical titanium alloy implants are subjected to strong friction during activities such as running, jumping and walking, requiring titanium alloy implants to have excellent wear resistance. Milling is a key link in the manufacture of titanium alloy components, and the milling surface metamorphic layer has become a common problem that restricts the fatigue resistance, corrosion resistance and wear resistance of titanium alloy components. Studies have shown that the irregular microstructure (grain bending, dragging, twisting and fracture, etc.) in the milling surface metamorphic layer of titanium alloy is the fundamental reason that restricts the material's response performance to external loads. In order to solve this problem, researchers usually use a combination of milling and shot peening to compensate for the defects of the surface metamorphic layer. However, for large and complex titanium alloy components such as aircraft frames and deep-sea pressure-resistant cabins, it is difficult to post-process them due to the size limitation of shot peening equipment, which has become a technical bottleneck in the manufacturing of large and high-reliability service components. Therefore, how to solve the irregular microstructure in the surface metamorphic layer in situ during the milling stage has become a frontier hot issue that has attracted much attention and is of great significance for achieving high-performance manufacturing of titanium alloy components from the source.

[0003] In addition, in terms of implementation plans and equipment, the uniformity of traditional shot peening is difficult to control, the roughness of the shot peening surface is difficult to guarantee, and it is difficult to reduce production time and cost by using subsequent shot peening. Therefore, in terms of means and implementation equipment, innovative design of tool structure and working actuator is proposed to meet the cutting and impact compound functions, and realize alternating superposition milling to create a multi-level micro-nano gradient structure surface in situ. Summary of the invention

[0004] In order to solve the above technical problems, the present invention provides a method for in-situ preparation of a multi-level micro-nano gradient structure on the surface of a titanium alloy by alternating superposition milling.

[0005] To achieve the above object, the present invention is implemented according to the following technical solutions:

[0006] A method for in-situ preparation of a multi-level micro-nano gradient structure on the surface of a titanium alloy by alternating superposition milling, comprising the following steps:

[0007] S1, milling the surface of the titanium alloy workpiece to be processed into a smooth surface;

[0008] S2. Fix the titanium alloy workpiece to be processed after milling on a CNC universal rotary head milling machine, wherein a gradient micro-blade impact head is installed on the tool handle of the CNC universal rotary head milling machine, and the contact end between the impact head and the titanium alloy workpiece to be processed is designed to be hemispherical, and the diameter of the hemispherical shape is 10 mm or 12 mm, respectively, and then perform alternating superposition milling on the surface of the titanium alloy workpiece to be processed:

[0009] S21, controlling the impact head to perform reciprocating forward / reverse alternating milling motion in coordination with the axial impact synchronous motion to process the surface of the titanium alloy workpiece, so that the titanium alloy surface microstructure generates a multi-level micro-nano gradient structure under the combined action of multiple stresses;

[0010] S3. Use an electric spark cutting machine to slice the processed workpiece, put the cut samples into an ultrasonic cleaner and clean them with anhydrous ethanol to ensure that there are no other attachments on the surface, and then observe the cross-sectional microstructure of the samples.

[0011] Furthermore, the reciprocating forward / reverse alternating milling motion of the impact head and the axial impact synchronous motion are coordinated to process the surface of the titanium alloy workpiece, and the reversing times, reciprocating passes, and impact parameters are regulated. The specific settings are: feed speed is 40-60mm / min, punching depth is 0.1-0.15mm; impact interval is 1-2mm; reverse / forward reversing times is 1 time; reciprocating passes are 1-3 times; impact frequency is 70Hz.

[0012] Furthermore, the Kroll reagent is composed of a volume ratio of HF:HNO3:H2O=2:1:17.

[0013] Furthermore, in step S3, the cross-sectional microstructure observation of the sample is performed by preparing the sample using a metallographic insert machine, setting the temperature to 150° C. and maintaining the pressure for 10 minutes, then taking out the sample after cooling, and grinding and polishing the sample; then, the polished sample surface is corroded using a Kroll reagent for 45 seconds.

[0014] Furthermore, in step S3, 400 mesh, 800 mesh, 1000 mesh, 1500 mesh and 3000 mesh sandpaper are used in sequence to grind and polish the sample.

[0015] Compared with the prior art, the present invention obtains a multi-level micro-nano gradient structure surface layer by alternating and superimposed milling on the surface of the titanium alloy workpiece to be processed. The grain size of the multi-level micro-nano gradient structure surface layer of the titanium alloy changes continuously and gradually from the surface nanoscale to the matrix micrometer scale, which is beneficial to the matching of strength and toughness and improves the intrinsic mechanical properties: on the one hand, it can prevent the sudden change of mechanical properties caused by the sudden change of grain size or layer thickness; on the other hand, it can make the action mechanisms corresponding to different grain sizes manifest at the same time to promote the coordinated deformation of the materials, thereby improving the service performance of the materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 This is the working principle of alternating superposition milling.

[0017] Figure 2 Surface morphologies under different alternating superposition milling parameters: (a) sample #1; (b) sample #2; (c) sample #3; (d) sample #4; (e) sample #5; (f) sample #6; (g) sample #7; (h) sample #8.

[0018] Figure 3 It is an alternating superposition milling method to produce a multi-level micro-nano gradient structure on the surface. DETAILED DESCRIPTION

[0019] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with embodiments. The specific embodiments described herein are only used to explain the present invention and are not used to limit the invention.

[0020] The following embodiment uses TA2 titanium alloy as the workpiece to be processed, and the specific operations are as follows:

[0021] S1. Milling the surfaces of eight titanium alloy workpieces to be processed into smooth surfaces; the eight titanium alloy workpieces to be processed are respectively recorded as specimen #1, specimen #2, specimen #3, specimen #4, specimen #5, specimen #6, specimen #7, and specimen #8;

[0022] S2. Fix the titanium alloy workpiece to be processed after milling on a CNC universal rotary head milling machine, wherein an impact head is installed on the tool handle of the CNC universal rotary head milling machine, and the contact end between the impact head and the titanium alloy workpiece to be processed is designed to be hemispherical, and the diameter of the hemispherical shape is 10mm or 12mm respectively. The material of the impact head is selected from high-hardness and high-stability SKD11 cold-working die steel; then perform alternating superposition milling on the surface of the titanium alloy workpiece to be processed:

[0023] S21, such as Figure 1 As shown, the reciprocating reverse / forward alternating milling motion of the impact head is controlled to cooperate with the axial impact synchronous motion to process the surface of the titanium alloy workpiece; the number of reversing times, the number of reciprocating passes, and the impact parameters are regulated, and the specific settings are: feed speed is 40-60mm / min, punching depth is 0.1-0.15mm; impact interval is 1-2mm; reverse / forward reversing times is 1 time; reciprocating passes are 1-3 times; impact frequency is 70Hz, and the alternating superposition milling process parameter design for eight specimens is shown in Table 1.

[0024] Table 1

[0025]

[0026] Surface morphology under different alternating superposition milling parameters Figure 2 As shown, Figure 2 (a) is sample #1; (b) is sample #2; (c) is sample #3; (d) is sample #4; (e) is sample #5; (f) is sample #6; (g) is sample #7; and (h) is sample #8.

[0027] S3. Use an electric spark cutting machine to slice the processed workpiece, put the cut samples into an ultrasonic cleaner and clean them with anhydrous ethanol to ensure that there is no other attachment on the surface; then complete the preparation of the sample through a metallographic embedding machine, set the temperature to 150℃ and hold the pressure for 10 minutes, then take it out after cooling, and use 400 mesh, 800 mesh, 1000 mesh, 1500 mesh and 3000 mesh sandpaper to grind and polish the sample in turn; then, use Kroll reagent (volume ratio HF:HNO3:H2O=2:1:17) to corrode the surface of the polished sample for 45 seconds.

[0028] Surface mechanical properties are tested:

[0029] Firstly, the load-displacement curves at different depths of the surface section were measured by nanoindentation experiment to obtain the elastic modulus, nanohardness and yield stress indicators.

[0030] The nanoindentation experiment was carried out on a Nano Indenter G200 nanometer. The experiment was carried out at room temperature of 20°C. A triangular pyramid-shaped Bosch diamond indenter was selected for the nanoindentation experiment. The angle from the edge to the vertical axis of the indenter top was 77.05°, and the arc radius of the indenter top was 150nm. In order to avoid the interference of the indenter size effect on the results, the maximum load was selected as 100mN, the maximum indentation depth was 1000nm, and the holding time was 20s.

[0031] The residual stress at different depths of the surface layer of the multi-level micro-nano gradient structure of titanium alloy was detected by Empyrean intelligent grazing incidence X-ray diffractometer without peeling and damage. The power of the ceramic X-ray tube was 2.2kW, the X-ray wavelength λ corresponding to the copper target was 0.154nm, the working tube voltage was 40kV, and the current was 40mA. During the detection, the deflection angle was 4.37°, the offset angle was -1.0932°, the fixed mask width was 20mm, and the divergence slit was set to a fixed slit. The grazing incidence X-ray diffraction data was analyzed using Jade software to obtain the nature and size of the residual stress.

[0032] The friction and wear characteristics of the multi-level micro-nano gradient structure surface of titanium alloy were microscopically tested on a pin-disc wear tester, with a speed range of 0-3000r / min and a load range of 0-3000N. The friction coefficient and friction torque were measured and recorded online by a computer connected to the tester, and the wear micromorphology was characterized and analyzed using SEM. The nano scratch test was also conducted on a Nano Indenter G200 nanometer. The normal force in the constant loading mode was selected as 500μN, 1000μN, 2000μN and 4000μN, and the normal force in the continuous loading mode increased linearly from 0 to 2000μN during the scratching process.

[0033] Figure 2 Surface morphology under different alternating superposition milling parameters, comparison Figure 2 (a) and Figure 2 In (b), the surface impact indentation and texture are obvious when the impact head has a diameter of 12 mm. This shows that within the experimental parameter range, as the impact head increases, the contact area between the impact head and the workpiece increases, which in turn increases the degree of plastic deformation on the material surface, leaving obvious impact marks. Figure 2 (c) shows the surface morphology when the feed rate is increased to 60 mm / min, and the surface impact marks do not change significantly. Therefore, the feed rate has little effect on the surface morphology. Figure 2 (d) is the surface morphology when the punching depth increases to 0.15 mm. It can be seen that the indentation on the surface of the material is obvious, and there is obvious local deformation. This shows that within the experimental parameters, a larger punching depth can cause more severe plastic deformation of the surface layer of the material, but it will also have an adverse effect on the surface morphology. Figure 2 (e) and Fig. Figure 2 (f) in the figure respectively represents the surface morphology of the same direction forward rotation and reverse reversal with an impact interval of 2mm. It can be observed from the figure that the first indentation is eliminated, and there is an obvious bulge in the first impact area in both figures. This shows that in the alternating superposition milling of TA2 pure titanium, the secondary impact can effectively promote the plastic deformation of the material and eliminate the indentation left by the previous impact, but at the same time, it is also necessary to consider how to avoid the formation of new bulges in the previous impact area. In addition, similar deformation effects can be observed regardless of the same direction forward rotation or reverse reversal, which shows that although the processing direction affects the plastic flow inside the material, it has little effect on the surface morphology. Figure 2(g) in the figure is the surface morphology with an impact pass interval of 1 mm. Although the formation of bulges can still be observed, the protrusions are less obvious. In the simulation results of different indentation overlap intervals, stress concentration is generated at the local indentation edge. Comparing the surface morphology in the experiment, it can be explained that the stress concentration is caused by the formation of bulges. A smaller impact interval means an increase in the overlapping area, which leads to more dispersed material flow and effectively improves the degree of bulges. When the impact passes are increased to 3 times, there is no obvious improvement on the surface, as shown in Figure 1. Figure 2 As shown in (h) in the figure, therefore, the impact pass has little effect on the surface morphology.

[0034] Compared with the surface roughness of the original workpiece (0.910μm), the surface roughness of the TA2 pure titanium workpiece can be effectively reduced by using the alternating superposition milling process. The surface roughness of the #1 sample is 0.376μm, which is the lowest value under all parameters. The surface roughness of the #4 sample is the largest under all processing parameters, which is consistent with the Figure 2 The surface morphology results in (d) are consistent. As the punching depth increases, the surface indentation and texture are obvious, which leads to an increase in surface roughness. It is worth noting that in the samples of alternating superposition milling, the #3, #4, #5, #6, #7 and #8 samples are larger than the milling surface. This is because during the rotation process, the friction between the tool and the material surface causes wear on the impact head surface, which increases the surface roughness of the material. At the same time, in the surface morphology of the #5, #6, #7 and #8 samples, the secondary impact improves the bulge formed by the previous impact.

[0035] Figure 3 (a) is the electron backscatter diffraction (EBSD) observation result of the titanium alloy surface and matrix. Compared with the matrix structure, the surface titanium alloy grains have obvious gradient refinement phenomenon. Figure 3 The KAM results of (b) show that the dislocation density of the surface layer increases in a gradient. These results indicate that a multi-level micro-nano gradient structure is generated on the surface of the titanium alloy under the action of alternating superposition milling.

[0036] In order to verify that alternating superposition milling can improve the mechanical properties of the material surface, the average hardness of the surface plastic deformation area was measured by an ultrasonic hardness tester, as shown in Table 2.

[0037] Table 2 Surface hardness of original specimen, milling and alternating superposition milling process

[0038]

[0039] It can be seen from Table 2 that the alternating superposition milling process can effectively improve the microhardness of the surface layer, with the highest being 553.33 HV. The grain refinement in the plastic deformation layer will increase the hardness of the workpiece surface, so this process has a good surface strengthening effect.

[0040] The technical solution of the present invention is not limited to the above-mentioned specific embodiments. All technical variations made according to the technical solution of the present invention fall within the protection scope of the present invention.

Claims

1. A method for in-situ preparation of multi-level micro-nano gradient structure on the surface of titanium alloy by alternating superposition milling, characterized in that: The following steps are involved: S1, milling the surface of the titanium alloy workpiece to be processed into a smooth surface; S2. Fix the titanium alloy workpiece to be processed after milling on a CNC universal rotary head milling machine, wherein an impact head is installed on the tool handle of the CNC universal rotary head milling machine, and the contact end between the impact head and the titanium alloy workpiece to be processed is designed to be hemispherical, and the diameter of the hemispherical shape is 10 mm or 12 mm respectively; then perform alternating superposition milling on the surface of the titanium alloy workpiece to be processed: S21, controlling the impact head to perform reciprocating forward / forward alternating milling motion in coordination with the axial impact synchronous motion to process the surface of the titanium alloy workpiece, so that the surface microstructure of the titanium alloy generates a multi-level micro-nano gradient structure under the action of multiple composite stresses; S3. Use an electric spark cutting machine to slice the processed workpiece, put the cut samples into an ultrasonic cleaner and clean them with anhydrous ethanol to ensure that there are no other attachments on the surface; then observe the cross-sectional microstructure of the samples.

2. The method for in-situ preparation of multi-level micro-nano gradient structure on the surface of titanium alloy by alternating superposition milling according to claim 1 is characterized in that: The control of the reciprocating reverse / forward alternating milling motion of the impact head and the axial impact synchronous motion to coordinate the reversing times, reciprocating passes, and impact parameters when processing the surface of the titanium alloy workpiece is performed. The specific settings are: feed speed 40-60mm / min; punching depth 0.1-0.15mm; impact interval 1-2mm; reverse / forward reversing times 1 time; reciprocating passes 1-3 times; impact frequency 70Hz.

3. The method for in-situ preparation of multi-level micro-nano gradient structure on the surface of titanium alloy by alternating superposition milling according to claim 1, characterized in that: The Kroll reagent is composed of a volume ratio of HF:HNO3:H2O=2:1:

17.

4. The method for in-situ preparation of multi-level micro-nano gradient structure on the surface of titanium alloy by alternating superposition milling according to claim 1, characterized in that: In step S3, the cross-section observation of the sample is completed by preparing the sample through a metallographic insert machine, setting the temperature to 150° C. and maintaining the pressure for 10 minutes, then taking out the sample after cooling, and grinding and polishing the sample; then, the surface of the polished sample is corroded using a Kroll reagent for 45 seconds.

5. The method for in-situ preparation of multi-level micro-nano gradient structure on the surface of titanium alloy by alternating superposition milling according to claim 4, characterized in that: In step S3, 400 mesh, 800 mesh, 1000 mesh, 1500 mesh and 3000 mesh sandpaper are used to grind and polish the sample in sequence.