Processing method of axial hollow-wall polyethylene pipe
Through step-by-step processing and infrared heating technology, the problem of shrinking and collapse of large-diameter axial hollow wall polyethylene pipes during cooling is solved, and efficient molding and quality assurance are achieved.
Patent Information
- Application Number
- CN202411380826.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-30
- Publication Date
- 2024-11-19
AI Technical Summary
When manufacturing large-diameter axial hollow wall polyethylene pipes, the pipes are prone to shrink and collapse due to the long cooling time of the polyethylene material, and the reinforcement ribs are located inside and are not easily cooled, resulting in increased molding difficulty.
The step-by-step processing method is adopted, first forming the inner pipe body and cooling and shaping, then covering the outer pipe body and secondary cooling and shaping, and the top of the reinforcement rib is melted and softened by infrared heating to composite the outer pipe body to avoid shrinkage and collapse.
It improves cooling efficiency, ensures the quality of reinforcement ribs and pipe forming quality, avoids shrinkage and collapse, and is suitable for pipe processing with a diameter of more than 300mm.
Smart Images

Figure CN118977388A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for processing an axial hollow-wall polyethylene pipe, belonging to the technical field of pipe processing. Background Art
[0002] Pipes are widely used in municipal engineering construction, urban construction and other aspects, and there are various types. However, with the improvement of construction quality requirements and pipe quality requirements in municipal engineering, the strength requirements of pipes are also getting higher and higher. In the existing pipe processing process, in order to improve the strength performance index of pipes, the structure of pipes is usually designed. For example, axial hollow wall pipes are currently used more and more, so that they have good support strength performance. Axial hollow wall pipes refer to pipes with hollow structures in the pipe wall, and a number of hollow gaps distributed in an annular shape are arranged between the inner wall and the outer wall. Compared with ordinary solid wall pipes, they have the advantages of light weight, high ring stiffness and low cost. At the same time, since polyethylene is a widely used raw material with good chemical stability, corrosion resistance, electrical insulation and processing performance, it is also widely used in pipe processing materials. The existing pipe processing is usually to melt and soften polyethylene plastic particles through an extruder and extrude them through an extrusion die to shape them into pipes at one time, and then cool and shape the pipe blanks through a vacuum shaping cooling water tank to form pipes. This method can effectively manufacture polyethylene pipes.
[0003] However, the above processing technology is mainly for the processing of solid-wall polyethylene plastic pipes or small-caliber axial hollow-wall polyethylene pipes. When manufacturing large-caliber (diameter 300mm or more) axial hollow-wall polyethylene pipes, there are the following problems. On the one hand, most of the existing axial hollow-wall pipes are made by one-piece molding. However, since the polyethylene material will shrink, deform and collapse when the cooling time is long, when making large-caliber axial hollow-wall pipes, the hollow wall and axial reinforcement ribs of the axial hollow-wall pipe are located inside, making it difficult to cool during the cooling and shaping process, which will cause the cooling time to become longer, and shrinkage, deformation and collapse will occur, making the final pipe molding difficult. On the other hand, since the cooling speed of the polyethylene material itself is also slow, the time for one-time processing and molding is long, which further increases the difficulty of molding. Therefore, the existing one-piece molding method is usually suitable for processing polyethylene axial hollow wall pipes with smaller nominal diameters. For the manufacture of large-diameter polyethylene axial hollow wall pipes, since the middle part is hollow and the axial reinforcement ribs are located inside the pipe, it is difficult to cool during the processing and the cooling time is too long, resulting in shrinkage, collapse and deformation problems. Summary of the invention
[0004] In view of the defects in the above prior art, the present invention provides a method for processing a large-diameter axial hollow-wall polyethylene pipe, which solves the problem of how to avoid shrinkage, collapse and deformation of the hollow-wall pipe during processing.
[0005] The object of the present invention is achieved through the following technical scheme: a method for processing an axial hollow wall polyethylene pipe, wherein the axial hollow wall polyethylene pipe comprises an outer pipe body and an inner pipe body with axial reinforcing ribs distributed circumferentially at intervals, characterized in that the method comprises the following steps:
[0006] A. Plasticizing and melting the raw polyethylene plastic and then extruding it to form the inner tube body, and then cooling and shaping it for the first time through a vacuum shaping cooling system to obtain the inner tube body;
[0007] B. reheating the top ends of the axial reinforcing ribs spaced circumferentially on the outer side of the inner tube body to melt and soften all the top ends of the axial reinforcing ribs;
[0008] C. The polyethylene plastic required as the raw material of the outer tube body is plasticized and melted, and then extruded and coated on the outer side of the inner tube body, so that the top of the axial reinforcing rib is composited with the inner wall of the coated outer tube body; and then the vacuum cooling and shaping system is used for the second cooling and shaping, and the corresponding axial hollow wall polyethylene pipe is obtained through cutting.
[0009] The axially hollow-walled polyethylene pipe is divided into an inner pipe body and an outer pipe body with axial reinforcing ribs in the circumferential direction by a step-by-step processing method. Specifically, the plasticized molten polyethylene material is first extruded to form an inner pipe body with an inner wall and axial reinforcing ribs. The inner pipe body is first cooled and shaped, which is equivalent to directly cooling and shaping the inner pipe body with reinforcing ribs distributed at intervals in the circumferential direction, thereby improving the cooling efficiency and enabling the axial reinforcing ribs of the inner pipe body to be cooled and hardened quickly and effectively. This solves the problem that the pipe processed with polyethylene material is not easy to cool in the hollow interior of the pipe and the reinforcing ribs during the existing one-time molding. The above-mentioned processing method of the present invention effectively avoids the phenomena of shrinkage, collapse and deformation, ensures the quality of the formed reinforcing ribs, and improves the molding quality. Then, the top of the axial reinforcing ribs is selectively heated, melted and softened, which can ensure It is composited with the inner side of the subsequent outer tube body (or outer wall) to effectively ensure the fastness of fusion, and can effectively ensure that the rest of the axial reinforcement ribs will not be melted and softened, avoid being softened by secondary heating, ensure its hardness and strength performance, and also ensure the overall quality of the pipe, so that there will be no shrinkage, collapse and deformation. Then, the polyethylene material of the outer tube body is melt-softened and extruded through secondary molding and covered on the outer surface, and the inner side of the outer tube body is composited with the top of the circumferential reinforcement rib of the inner tube as a whole. After secondary cooling and shaping, the corresponding hollow wall pipe can be obtained, which is equivalent to basically only needing to cool and shape the outer tube body (outer wall) during the second cooling and shaping, so that the cooling efficiency and the molding quality of the outer tube body can be guaranteed, and the shrinkage, collapse and deformation during the cooling process can be effectively avoided, and the quality of cooling and shaping can be improved. Then, the required length of the pipe can be obtained through further post-processing such as cutting. The present invention uses the above-mentioned secondary molding method and secondary heating to melt the top end of the axial reinforcement rib and then composite it with the outer tube body, which can effectively avoid the shrinkage, collapse and deformation caused by the axial reinforcement rib located inside being difficult to cool in the existing primary molding process, thereby improving the molding quality of the pipe. The present invention can effectively avoid the problems of shrinkage, collapse and deformation in the processing of large-diameter (diameter above 300mm) axial hollow wall polyethylene pipes, and has the advantage of good pipe quality.
[0010] In the above-mentioned processing method of axial hollow wall polyethylene pipe, as a preferred method, the secondary heating in step B adopts an infrared heating device to melt and soften the top of the axial reinforcing rib by infrared radiation. By heating by infrared radiation, the phenomenon of sticking caused by direct contact can be avoided. More importantly, heating by infrared radiation makes it possible to have a spacing and no contact between the top surface of the top of the axial reinforcing rib and the inner tube body during heating, so that the heating, melting and softening of the vicinity of the top surface of the top of the axial reinforcing rib can be better achieved. By controlling the spacing and the principle of radiation heating, it is ensured that the axial reinforcing rib will not be softened by the entire heating, so that it can be compounded with the polyethylene material of the outer tube body during subsequent processing while ensuring its overall strength performance and hardness quality, and effectively avoiding deformation, shrinkage and collapse after secondary heating.
[0011] In the above-mentioned processing method of the axial hollow wall polyethylene pipe, preferably, the secondary heating in step B is specifically:
[0012] The inner tube body is heated by passing through the heating port of the infrared heating device, and the spacing between the circumferential heating element of the heating port and the top surface of the circumferential axial reinforcing ribs of the inner tube body along the radial direction of the inner tube body is 3cm to 6cm. The circumferential heating element of the heating port of the infrared heating device and the top surface of the top of the circumferential axial reinforcing rib are kept at a certain spacing, which can more accurately control the heating of the top part of the axial reinforcing rib during infrared heating, and as the radial distance between the infrared heating device and the axial reinforcing rib increases, its heating capacity will weaken. In this way, the entire axial reinforcing rib will not be heated by controlling the spacing and the principle of radiation, ensuring that the end is heated, melted and softened while the other parts have good strength quality, avoiding shrinkage, collapse and deformation during secondary heating.
[0013] In the above-mentioned processing method of axial hollow wall polyethylene pipe, preferably, the melted and softened part of the top of the axial reinforcing rib is located at more than 2 / 3 of the height of the axial reinforcing rib along the diameter direction of the inner tube body. The height here refers to the distance from the top surface to the bottom of the axial reinforcing rib along the radial direction (diameter direction) of the inner tube body, which can more accurately control the melted and softened part of the top of the reinforcing rib after infrared heating, achieve better composite with the outer tube body, and avoid the shrinkage and collapse process during secondary heating, thereby improving the molding quality. As a further preference, the melt-softened depth of the top of the reinforcing rib from the top surface along the diameter direction of the large-diameter inner tube body is 2mm to 5mm.
[0014] In the above-mentioned processing method of the axial hollow wall polyethylene pipe, preferably, the temperature of the secondary heating in step B is 150° C. to 180° C., so as to effectively achieve the purpose of melting and softening the top end of the axial reinforcing rib.
[0015] In the above-mentioned processing method of axial hollow wall polyethylene pipe, as a preference, the heating temperature of the plasticizing and melting in step C is 185°C to 200°C. When processing the outer tube body, the temperature of the plasticizing and melting of the polyethylene plastic material is slightly higher than the temperature of the secondary heating, which is equivalent to making the degree of melting and softening of the material of the outer tube body higher than the degree of melting and cooking of the reinforcing ribs during the secondary heating, so that the material of the outer tube body can be better melted and compounded with the material of the outer tube body and combined together, which is beneficial to the integrity and fastness of the compound; and it is also beneficial to the molding quality of the reinforcing ribs, ensuring that there will be no shrinkage, collapse and deformation problems, and has the advantage of good molding quality.
[0016] In the above-mentioned processing method of axial hollow wall polyethylene pipe, preferably, the temperature of the first cooling and shaping in step A is controlled at 15° C. to 25° C. This can effectively cool and shape the inner pipe body and ensure the shaping quality of the outer reinforcing ribs.
[0017] In the above-mentioned processing method of axial hollow wall polyethylene pipe, as a preference, the temperature of the second cooling and shaping in step C is controlled at 15° C. to 25° C. This can effectively cool the inner pipe and also enable the axial reinforcing ribs to achieve the purpose of cooling and shaping, with good molding quality and no shrinkage, collapse or deformation problems.
[0018] In the above-mentioned processing method of axial hollow wall polyethylene pipe, preferably, the diameter of the axial hollow wall polyethylene pipe is greater than 300 mm. Due to the defect that the reinforcing ribs inside the large-diameter axial hollow wall pipe made of polyethylene material are not easy to cool during the one-piece molding process, the processing method of the present invention can be used to facilitate the processing of large-diameter pipes, effectively prevent shrinkage and collapse during the processing and cooling process, and has the advantage of good molding quality.
[0019] In summary, compared with the prior art, the present invention has the following advantages:
[0020] 1. Through the step-by-step processing method, it is equivalent to directly cooling and shaping the inner tube body of the axial reinforcing ribs distributed at intervals in the circumferential direction, thereby improving the cooling efficiency, effectively avoiding shrinkage, collapse and deformation, ensuring the quality of the formed axial reinforcing ribs, and improving the quality of molding; and then selectively heating and melting the top of the axial reinforcing ribs to soften, which can effectively ensure that the bottom of the reinforcing ribs will not be melted and softened, avoid secondary softening, and also ensure the overall quality of the tube material, so that there will be no shrinkage and collapse.
[0021] 2. By using infrared radiation for heating, the phenomenon of direct contact with the sticky material can be avoided, and there is a gap between the end face of the reinforcing rib of the inner tube body and no contact during heating, which can better achieve heating and softening of the end face of the reinforcing rib, while ensuring that the reinforcing rib will not be heated as a whole, avoiding the phenomenon of complete softening by secondary heating, and ensuring its strength quality. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 It is a schematic diagram of the cross-sectional structure of the axial hollow wall polyethylene pipe.
[0023] Figure 2 It is a schematic diagram of the cross-sectional structure of the inner tube body of the axial hollow wall polyethylene tube.
[0024] Figure 3 This is a schematic diagram of the production line process structure for processing axial hollow wall polyethylene pipes.
[0025] Figure 4 It is a front view structural schematic diagram of the inner tube body passing through the heating port of the infrared heating device during the processing of the axial hollow wall polyethylene pipe.
[0026] Figure 5 It is a three-dimensional structural schematic diagram of the inner tube body of the axial hollow wall polyethylene tube passing through the infrared heating device.
[0027] Figure 6 It is a schematic diagram of the spacing between the circumferential direction of the heating port of the infrared heating device and the top surface of the axial reinforcement rib of the inner tube body.
[0028] In the figure, 1. axial hollow wall polyethylene pipe; 101. outer pipe body; 102. inner pipe body; 103. axial reinforcement rib; 2. extruder 1; 3. extrusion die 1; 4. vacuum shaping cooling system 1; 5. infrared heating device; 51. heating port; 6. extruder 2; 7. extrusion die 2; 8. vacuum shaping cooling system 2; 9. inkjet printer; 10. pipe traction machine; 11. pipe cutting machine; 12. pipe bracket. DETAILED DESCRIPTION
[0029] The technical solution of the present invention is further specifically described below through specific embodiments and drawings, but the present invention is not limited to these embodiments.
[0030] Combination Figure 1 and Figure 2The structure of the axial hollow wall polyethylene pipe 1 includes an outer pipe body 101 and an inner pipe body 102 with axial reinforcing ribs 103 spaced apart in the circumferential direction. The inner pipe body 102 and the outer pipe body 101 are integrated to form the above-mentioned axial hollow wall polyethylene pipe 1. The inner pipe body 102 and the outer pipe body 101 are both made of polyethylene plastic material. More importantly, the inner pipe body 102 and the outer pipe body 101 are combined to form the above-mentioned axial hollow wall polyethylene pipe 1. Figure 1 , Figure 2 , Figure 3 , Figure 4 and Figure 5 As shown, the processing method of the axial hollow wall polyethylene pipe 1 includes the following steps:
[0031] The raw polyethylene plastic is plasticized and melted, and then extruded to form an inner tube body 102, and then cooled and shaped for the first time by a vacuum shaping cooling system 4 to obtain the inner tube body 102;
[0032] Then, the top ends of the axial reinforcing ribs 103 circumferentially spaced on the outer side of the inner tube body 102 are heated for a second time to melt and soften the top ends of all the axial reinforcing ribs 103; the second heating is preferably performed by infrared heating device 5 through infrared radiation;
[0033] The polyethylene plastic required as the raw material of the outer tube body 101 is plasticized and melted, and then extruded and coated on the outer side of the inner tube body 102, so that the top of the axial reinforcement rib 103 is composited with the inner wall of the coated outer tube body 101; and then the vacuum cooling and shaping system 28 is used for the second cooling and shaping, and after cutting, the corresponding axial hollow wall polyethylene pipe is obtained.
[0034] Combination Figure 4 and Figure 5 As shown, the above-mentioned infrared heating device 5 is used for heating. Specifically, the inner tube body 102 with the circumferentially spaced axial reinforcing ribs 103 is passed through the heating port 51 of the infrared heating device 5 on the production line, and the heating temperature is set to 175°C to 185°C, so that the top of the axial reinforcing ribs 103 is heated, melted and softened; it is best to make the circumferentially distributed heating elements of the heating port 51 of the infrared heating device 5 and the top surface of the circumferential axial reinforcing ribs 103 of the inner tube body 102 have a spacing along the radial direction of the inner tube body 102, which is equivalent to a gap between the two, combined with Figure 6 As shown in the figure, the spacing d between the two is such that the inner tube body 102 does not directly contact the circumferential side walls of the heating port 51 of the infrared heating device 5 and the heating elements (not shown in the figure) distributed circumferentially at the heating port 51. The heating elements here can be infrared heating lamps, which use infrared lamps for radiation heating. This is conducive to better heating the top end and can also avoid the phenomenon of contact with sticky materials. A more preferred solution is to make the spacing 3cm to 6cm, preferably 4cm to 5cm.
[0035] Further specific implementation plan, combined with Figure 3 As shown, the process structure diagram of the processing production line adopted above includes extruder 1 2, extrusion die 1 3, vacuum shaping cooling system 1 4, infrared heating device 5, heating port 51, extruder 2 6, extrusion die 2 7, vacuum shaping cooling system 2 8, inkjet printer 9, pipe traction machine 10, pipe cutting machine 11 and pipe bracket 12 in sequence. Figure 3 The figure is only a schematic diagram of the production line flow chart, in order to better illustrate the various processes of the production line, and does not limit the size of the scale. Figure 1 , Figure 2 and Figure 3 When processing the above-mentioned axial hollow wall polyethylene pipe 1, first, polyethylene plastic particles are put into the extruder 2, and the temperature of the extruder 2 is set to 180°C to 190°C, so that the put-in polyethylene plastic particles are plasticized and melted, and then the plasticized and melted polyethylene plastic is extruded through the die head of the extrusion die 3 to form the required inner tube body 102 with axial reinforcing ribs 103 distributed at intervals in the circumference. Here, each axial reinforcing rib 103 is distributed at equal intervals in the circumferential direction of the outer side of the inner tube body 102, and preferably, there is an axial reinforcing rib every 15° to 20°. 103, the above-mentioned shape of the die opening cross section of the die head of the extrusion die 3 can correspond to the cross-sectional shape of the inner tube body 102 to form the inner tube body 102 with axial reinforcing ribs 103, and then the inner tube body 102 with the axial reinforcing ribs 103 distributed at circumferential intervals is subjected to shaping cooling by a vacuum shaping cooling system 4, wherein the vacuum shaping cooling system 4 can be a vacuum shaping cooling water tank, and the cooling temperature is set at 15°C to 25°C, preferably at 20°C to 22°C, to obtain the inner tube body 102 with the axial reinforcing ribs 103 distributed at circumferential intervals.
[0036] Then, the top ends of the axial reinforcing ribs 103 circumferentially spaced on the outer side of the inner tube body 102 are heated for a second time to melt and soften the top ends of all the axial reinforcing ribs 103; specifically, the inner tube body 102 with the axial reinforcing ribs 103 spaced circumferentially is heated for a second time, and preferably, the infrared heating device 5 is used for the secondary heating, so that the inner tube body 102 with the axial reinforcing ribs 103 spaced circumferentially is passed through the heating port 51 of the infrared heating device 5, and the heating temperature is set to 175° C. to 185° C., so that the top ends of the axial reinforcing ribs 103 are heated, melted and softened; combined with Figure 4 and Figure 5As shown, it is best to make the heating element of the heating port 51 of the infrared heating device 5 and the top surface of the axial reinforcing rib 103 of the inner tube body 102 have a spacing distance d along the radial direction of the inner tube body (102), which is equivalent to a gap between the two, without direct contact, which is conducive to better heating the top and avoiding sticking. In addition, by using the radiation heating method, through the control of the spacing and as the radiation distance increases, the top of the axial reinforcing rib 103 can be heated in a targeted manner, and the other parts of the axial reinforcing rib 103 will not be overheated at the same time, avoiding the problems of shrinkage, collapse and deformation during secondary heating, and ensuring the forming quality of the pipe. In order to better achieve the heating of the top of the axial reinforcing rib 103, a more preferred solution is adopted, so that the spacing is 3cm to 6cm, preferably 4cm to 5cm. That is, a certain gap is maintained, which can not only effectively achieve the heating, melting and softening of the top of the axial reinforcing rib 103, but also avoid excessive heating of other parts of the axial reinforcing rib 103, effectively avoiding shrinkage, collapse and deformation, and ensuring the quality of the pipe.
[0037] In a more preferred specific embodiment, it is best to make the melted and softened portion of the top of the axial reinforcing rib 103 located at more than 2 / 3 of the height of the axial reinforcing rib 103 along the diameter direction of the inner tube body 102. A more preferred solution is to make the melted and softened depth of the top of the axial reinforcing rib 103 from the top surface along the diameter direction of the inner tube body 102 be 2 mm to 5 mm, and a more preferred solution is 3 mm.
[0038] Then, the raw material polyethylene plastic particles required for the outer tube body are put into the extruder 26 on the corresponding pipe processing production line, and the temperature of the extruder 26 is set to 185°C ~ 200°C, preferably 190°C. The put polyethylene plastic particles are plasticized and melted, and then extruded through the extrusion die 27 to be coated on the outer side of the inner tube body 102, so that the top of the above-mentioned axial reinforcement rib 103 is melted and composited with the inner wall of the coated outer tube body 101. As the production line passes through the vacuum cooling and shaping system 28, the second cooling and shaping is carried out, and the cooling temperature is set at 15°C ~ 25°C, preferably the temperature is controlled at 20°C ~ 22°C, and then the fixed length is cut by the pipe cutting machine 11 to obtain the corresponding required length of the axial hollow wall polyethylene pipe 1, and then it is sorted by the pipe bracket 12.
[0039] The processing of the axial hollow wall polyethylene pipe 1 is more suitable for processing large-diameter pipes with a diameter greater than 300 mm, and can optimally process large-diameter pipes of 315 mm to 1200 mm. The large-diameter pipes made by the processing method do not shrink, collapse or deform, and the axial reinforcement ribs 103 located inside do not shrink or collapse, and the overall pipe material has the advantage of good quality.
[0040] In a more preferred embodiment, when processing on the above-mentioned pipe processing production line, the production speed of the pipe can be adjusted according to the diameter of the large-diameter axial hollow wall polyethylene pipe 1. During the processing, the above-mentioned pipe moves forward under the traction of the pipe traction machine 10, and it is best to control the speed of the pipe moving forward to be 0.5m / min to 3.0m / min. In a further embodiment, the surface of the pipe can be sprayed with a printer 8 before cutting, so that the required text and other information can be sprayed on it.
[0041] The specific embodiments described in the present invention are merely examples of the spirit of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in similar ways, but they will not deviate from the spirit of the present invention or exceed the scope defined by the attached claims.
[0042] Although the present invention has been described in detail and some specific embodiments have been cited, it is obvious to those skilled in the art that various changes and modifications can be made without departing from the spirit and scope of the present invention.
Claims
1. A method for processing an axial hollow wall polyethylene pipe, wherein the axial hollow wall polyethylene pipe (1) comprises an outer pipe body (101) and an inner pipe body (102) with axial reinforcing ribs (103) distributed at intervals in the circumferential direction, characterized in that: The method comprises the following steps: A. Plasticizing and melting the raw polyethylene plastic and then extruding it to form the inner tube body (102), and then cooling and shaping it for the first time in a vacuum shaping cooling system (4) to obtain the inner tube body (102); B. reheating the top ends of the axial reinforcing ribs (103) distributed circumferentially at intervals on the outer side of the inner tube body (102) so that the top ends of all the axial reinforcing ribs (103) are melted and softened; C. The polyethylene plastic material required for the outer tube body (101) is plasticized and melted, and then extruded and coated on the outer side of the inner tube body (102), so that the top end of the axial reinforcing rib (103) is integrated with the inner wall of the coated outer tube body (101); and then cooled and shaped for the second time by the vacuum cooling and shaping system (8), and then cut to obtain the corresponding axial hollow wall polyethylene tube (1).
2. The method for processing an axially hollow-walled polyethylene pipe according to claim 1, characterized in that: The secondary heating in step B uses an infrared heating device (5) to melt and soften the top end of the axial reinforcing rib (103) by infrared radiation.
3. The method for processing an axially hollow-walled polyethylene pipe according to claim 2, characterized in that: The secondary heating in step B is specifically: The inner tube body (102) is heated by passing through a heating port (51) of an infrared heating device (5), and the spacing between the circumferential heating element of the heating port (51) and the top surface of the circumferential axial reinforcing ribs (103) of the inner tube body (102) along the radial direction of the inner tube body (102) is 3 cm to 6 cm.
4. The method for processing an axially hollow-walled polyethylene pipe according to any one of claims 1 to 3, characterized in that: The melted and softened portion of the top end of the axial reinforcing rib (103) is located at more than 2 / 3 of the height of the axial reinforcing rib (103) along the radial direction of the inner tube body (102).
5. The method for processing an axially hollow-walled polyethylene pipe according to claim 4, characterized in that: The melt softening depth of the top end of the axial reinforcing rib (103) from the top surface along the radial direction of the inner tube blank (103) is 2 mm to 5 mm.
6. The method for processing an axially hollow-walled polyethylene pipe according to any one of claims 1 to 3, characterized in that: The secondary heating temperature in step B is 150°C to 180°C.
7. The method for processing an axially hollow-walled polyethylene pipe according to claim 6, characterized in that: The heating temperature for plasticizing and melting in step C is 185°C to 200°C.
8. The method for processing an axially hollow-walled polyethylene pipe according to any one of claims 1 to 3, characterized in that: The temperature of the first cooling and shaping in step A is controlled at 15°C to 25°C.
9. The method for processing an axially hollow-walled polyethylene pipe according to any one of claims 1 to 3, characterized in that: The temperature of the second cooling and shaping in step C is controlled at 15°C to 25°C.
10. The method for processing an axially hollow-walled polyethylene pipe according to any one of claims 1 to 3, characterized in that: The diameter of the axial hollow wall polyethylene pipe (1) is greater than 300 mm.