Spherical silicon dioxide, polytetrafluoroethylene film, high-frequency copper-clad plate and preparation method of high-frequency copper-clad plate
By preparing highly dispersed spherical silica and polytetrafluoroethylene films, the dielectric instability and high loss problems of spherical silica as a filler for high-frequency substrates were solved, achieving stable transmission of high-frequency signals and low loss.
Patent Information
- Application Number
- CN202411070952.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-06
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-08-06
AI Technical Summary
When spherical silicon dioxide is used as a filler in high-frequency substrates, the dielectric constant is unstable and the dielectric loss increases, which affects the transmission of high-frequency signals.
By adding polytetrafluoroethylene (PTFE) to the preparation method, treating silica with cationic surfactants and modifiers, controlling particle size distribution and reducing surface adsorbed water and polar functional groups, highly dispersed spherical silica is prepared, and then combined with a PTFE film to stabilize dielectric properties.
It achieves ultra-low dielectric loss of high-frequency copper-clad laminate in high-frequency environment, ensures stable dielectric constant, reduces signal loss, and improves copper foil peel strength.
Smart Images

Figure CN118978164A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of copper-clad laminates, and in particular to spherical silicon dioxide, a polytetrafluoroethylene film and a high-frequency copper-clad laminate and a preparation method thereof. Background Art
[0002] As communication speeds and frequencies increase rapidly in the 5G / 6G communication field, the use of high-frequency bands in electronic devices and communication equipment is expanding. The use of the 10GHz band is becoming more popular due to its wideband, linear propagation, and permeability. For example, in the automotive field, millimeter-wave radars used to prevent collisions must use high-frequency materials of 76 to 79 GHz.
[0003] In high-frequency applications, the transmission loss of circuit signals increases rapidly as the frequency increases. The reasons are mainly the skin effect of the wire, the glass fiber effect and the dielectric loss of the substrate material. The dielectric loss of the substrate material contributes particularly significantly to the transmission loss of the circuit signal. Therefore, the substrate material used in high-frequency equipment requires a stable dielectric constant and extremely low dielectric loss.
[0004] Most polymer materials used in high-frequency substrate materials have low dielectric constants but high dielectric loss. However, most ceramic materials have the opposite characteristics, that is, high dielectric constants but low dielectric loss. In order to combine the characteristics of both and prepare high-frequency substrate materials with low dielectric constants and low dielectric loss, ceramic materials are filled with polymer resin materials to obtain new composite materials, which is a common method in the world.
[0005] Since silicon dioxide (SiO2) has a small dielectric constant (3.7), a relatively small dielectric loss value (0.0002@1MHZ), and a thermal expansion coefficient (0.5×10 -6 ) is low, and is currently the first choice for fillers of high-frequency substrate materials. In order to facilitate the uniform mixing of various resins for use as high-frequency substrate fillers, silica is synthesized into spherical shapes as much as possible. However, existing spherical silica fillers are basically limited to: the uniform distribution of the particle size of the obtained spherical silica is difficult to control, and the surface contains a large amount of adsorbed water and polar functional groups (such as silanol hydroxyl groups, etc.), which will lead to unstable dielectric constant and increased dielectric loss when used as high-frequency substrate fillers, thereby affecting the transmission of high-frequency signals. Summary of the invention
[0006] The purpose of the present invention is to overcome the problem that the existing spherical silica in the prior art, when used as a high-frequency substrate filler, will lead to unstable dielectric constant and increased dielectric loss, thereby affecting the transmission of high-frequency signals, and provide a spherical silica, a polytetrafluoroethylene film and a high-frequency copper clad laminate and a preparation method thereof.
[0007] In order to achieve the above object, the present invention provides a method for preparing spherical silicon dioxide.
[0008] The method comprises the following steps:
[0009] (1) mixing a cationic surfactant with a sodium hydroxide solution to obtain a first solution;
[0010] (2) mixing polytetrafluoroethylene with the first solution to obtain a second solution;
[0011] (3) mixing tetraethoxysilane and a modifier to obtain a mixed solution;
[0012] (4) mixing the mixed solution with the second solution at 70 to 90° C., and then stirring at 20 to 30° C. to obtain a mixture;
[0013] (5) separating the mixture into solid and liquid, and performing vacuum freeze-drying on the obtained solid;
[0014] (6) vacuum drying the solid obtained in step (5), then reflux extraction, and then vacuum drying to obtain spherical silica;
[0015] The modifier is selected from at least one of (3,3,3-trifluoropropyl)trimethoxysilane, (3,3,3-trifluoropropyl)triethoxysilane, 3-aminopropyltrimethoxysilane and 3-aminopropyltriethoxysilane.
[0016] Preferably, in step (1), the cationic surfactant is hexadecyltrimethylammonium bromide and / or hexadecyltriethylammonium bromide;
[0017] Preferably, in step (1), the weight ratio of the cationic surfactant to the sodium hydroxide in the sodium hydroxide solution is 1:0.01-0.2;
[0018] Preferably, in step (1), the mass fraction of sodium hydroxide in the sodium hydroxide solution is 0.01 to 0.1%;
[0019] Preferably, in step (1), the mixing conditions include: a temperature of 80 to 100° C. and a stirring speed of 500 to 1000 rpm;
[0020] Preferably, in step (2), the mixing conditions include: a temperature of 80 to 100° C. and a stirring speed of 500 to 1000 rpm.
[0021] Preferably, in step (3), the weight ratio of the tetraethoxysilane to the modifier is 100:1-15.
[0022] Preferably, in step (6), the solvent used for reflux extraction is 95% ethanol;
[0023] Preferably, in step (6), the reflux extraction time is 5 to 7 hours.
[0024] The second aspect of the present invention provides spherical silica prepared by the method as described above.
[0025] A third aspect of the present invention provides a method for preparing polytetrafluoroethylene, the method comprising the following steps:
[0026] A1. Mix spherical silica with water, disperse by ultrasonic, let stand, remove the precipitate, and obtain a stable dispersion;
[0027] A2. Adding the dispersion into the polytetrafluoroethylene solution under stirring to obtain a slurry;
[0028] A3, coating the slurry on a mold, and drying to obtain a polytetrafluoroethylene film;
[0029] Wherein, the spherical silica is the spherical silica according to claim 5.
[0030] Preferably, the weight ratio of the spherical silicon dioxide to polytetrafluoroethylene is 1:1.5-4.
[0031] Preferably, in step A2, the polytetrafluoroethylene solution is prepared according to the following process: mixing polytetrafluoroethylene with water, wherein the weight ratio of polytetrafluoroethylene to water is 1:1 to 20;
[0032] Preferably, in step A2, the stirring speed is 500-1000 rpm;
[0033] Preferably, in step A2, the dispersion is added at a rate of 50 to 70 mL / min;
[0034] Preferably, in step A3, the drying conditions include: a temperature of 110 to 130° C. and a time of 60 to 90 min.
[0035] A fourth aspect of the present invention provides a polytetrafluoroethylene film produced by the method described above.
[0036] A fifth aspect of the present invention provides a high-frequency copper-clad laminate, which comprises the spherical silicon dioxide or polytetrafluoroethylene film as described above.
[0037] The preparation method of spherical silica provided by the present invention stabilizes a metastable intermediate hydrogel in a reaction process by adding polytetrafluoroethylene; adjusts the size, crystallization speed and crystallization state of the obtained silica nucleus by changing the addition and hydrolysis speed of the precursor, so that the composition and structure of the synthesized silica are uniform and stable, and the size distribution is narrow; and the surface of the silica is modified by using a modifier, and the content of adsorbed water and polar functional groups on the surface of the prepared spherical silica is reduced by designing the preparation steps, and the spherical silica has a high dispersion degree.
[0038] The method for preparing a polytetrafluoroethylene film provided by the present invention uses the spherical silica with high dispersion as filler, so that the spherical silica can be evenly dispersed in a polytetrafluoroethylene skeleton, thereby making the performance of the obtained polytetrafluoroethylene film uniform and stable; in a high-frequency use environment, it is difficult for the polytetrafluoroethylene and the spherical silica in the polytetrafluoroethylene film to transform into each other, so the dielectric constant is low and very stable.
[0039] The high-frequency copper clad laminate provided by the present invention uses the above-mentioned spherical silica or polytetrafluoroethylene film as a raw material, so that when the high-frequency copper clad laminate is used at a high frequency (i.e., within the millimeter wave frequency band), when the high-frequency electromagnetic wave passes through the medium, the high-dispersion spherical silica and polytetrafluoroethylene molecules will also reduce the probability of lattice collisions back and forth, so that the high-frequency copper clad laminate has ultra-low dielectric loss, which can effectively reduce the signal loss generated by the high-frequency PCB board made of the copper clad laminate in a high-frequency use environment. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] Figure 1 The spherical silicon dioxide prepared in Example 1 of the present invention;
[0041] Figure 2 The polytetrafluoroethylene film prepared in Example 1 of the present invention;
[0042] Figure 3 The high-frequency copper-clad laminate is prepared according to the test example of the present invention. DETAILED DESCRIPTION
[0043] The specific implementation of the present invention is described in detail below in conjunction with the accompanying drawings. It should be understood that the specific implementation described here is only used to illustrate and explain the present invention, and is not used to limit the present invention.
[0044] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0045] The present invention provides a method for preparing spherical silicon dioxide, which comprises the following steps:
[0046] (1) mixing a cationic surfactant with a sodium hydroxide solution to obtain a first solution;
[0047] (2) mixing polytetrafluoroethylene with the first solution to obtain a second solution;
[0048] (3) mixing tetraethoxysilane and a modifier to obtain a mixed solution;
[0049] (4) mixing the mixed solution with the second solution at 70 to 90° C., and then stirring at 20 to 30° C. to obtain a mixture;
[0050] (5) separating the mixture into solid and liquid, and performing vacuum freeze-drying on the obtained solid;
[0051] (6) vacuum drying the solid obtained in step (5), then reflux extraction, and then vacuum drying to obtain spherical silica;
[0052] The modifier is selected from at least one of (3,3,3-trifluoropropyl)trimethoxysilane, (3,3,3-trifluoropropyl)triethoxysilane, 3-aminopropyltrimethoxysilane and 3-aminopropyltriethoxysilane.
[0053] In the present invention, by adding a cationic surfactant, the silicon dioxide particles generated subsequently can be stably dispersed in a solvent. The present invention does not make any particular limitation on the specific selection of the cationic surfactant, which can be a cationic surfactant commonly used in the art. In a preferred embodiment, the cationic surfactant is hexadecyltrimethylammonium bromide and / or hexadecyltriethylammonium bromide. By selecting the above cationic surfactant, the performance of the obtained spherical silicon dioxide is better and the cost is low.
[0054] In a preferred embodiment, the modifier is (3,3,3-trifluoropropyl)trimethoxysilane and / or (3,3,3-trifluoropropyl)triethoxysilane. By selecting the above modifier, the dielectric properties of the high-frequency copper-clad laminate made from the spherical silica are better. This may be because the surface functional group (3,3,3-trifluoropropyl) after the reaction of [(3,3,3-trifluoropropyl)trimethoxysilane and / or (3,3,3-trifluoropropyl)triethoxysilane] with the surface hydroxyl group of the oxide is easier to fuse with the PTFE resin body than the surface functional group (3-aminopropyl) after the reaction of [3-aminopropyltrimethoxysilane and / or 3-aminopropyltriethoxysilane] with the surface hydroxyl group of the oxide, thereby making the structure of the obtained PTFE film film and the high-frequency copper-clad laminate more uniform and stable, and less likely to absorb moisture from the environment.
[0055] In a preferred embodiment, in step (1), the weight ratio of the cationic surfactant to the sodium hydroxide in the sodium hydroxide solution is 1:0.01-0.2, specifically, for example, it can be 1:0.01, 1:0.02, 1:0.05, 1:0.07, 1:0.09, 1:0.1, 1:0.15, 1:0.18 or 1:0.2.
[0056] In a preferred embodiment, in step (1), the mass fraction of sodium hydroxide in the sodium hydroxide solution is 0.01 to 0.1%, more preferably 0.01 to 0.02%.
[0057] In a specific embodiment, in step (1), the mixing conditions include: a temperature of 80 to 100° C. and a stirring speed of 500 to 1000 rpm.
[0058] In a specific embodiment, in step (2), the mixing conditions include: a temperature of 80 to 100° C. and a stirring speed of 500 to 1000 rpm.
[0059] In order to reduce the content of adsorbed water and polar functional groups on the surface of the prepared spherical silica and improve the dispersion, in a preferred embodiment, in step (3), the weight ratio of the tetraethoxysilane and the modifier is 100:1 to 15, specifically, for example, 100:1, 100:2, 100:5, 100:8, 100:10, 100:12 or 100:15.
[0060] In a specific embodiment, step (4) comprises: slowly dripping the mixed solution into the second solution at 70-90°C and a stirring speed of 500-1000 rpm, and then stirring at 20-30°C and a stirring speed of 500-1000 rpm, until flocculent precipitation is slowly formed, and after stirring for 1-3 hours, a mixture is obtained. More specifically, the addition rate of the mixed solution is 10 mL / min.
[0061] The present invention does not limit the specific implementation of the solid-liquid separation in step (5), which can be a solid-liquid separation operation commonly used in the art. In a specific implementation, in step (5), the solid-liquid separation is filtration.
[0062] In a preferred embodiment, in step (6), the solvent used for reflux extraction is 95% ethanol.
[0063] In a preferred embodiment, in step (6), the reflux extraction time is 5 to 7 hours.
[0064] In a specific embodiment, step (6) comprises: heating the solid to 110-130°C at a rate of 1-5°C / min, vacuum drying, maintaining the set temperature for 5-6h, cooling to room temperature and taking it out, then refluxing and extracting with ethanol (95%) for 5-7h, heating the obtained solid to 120°C at a rate of 1-5°C / min, vacuum drying, maintaining the set temperature for 5-6h, and cooling to room temperature to obtain spherical silica.
[0065] In this article, room temperature refers to 23±3°C.
[0066] The preparation method of spherical silicon dioxide provided by the present invention changes the addition and hydrolysis speed of the precursor and uses a modifier to perform surface modification on the silicon dioxide, so that the adsorbed water and polar functional group content on the surface of the obtained spherical silicon dioxide are very low and the dispersion is high. In this way, when the spherical silicon dioxide is used as a filler for a high-frequency substrate (including a high-frequency copper-clad laminate and a high-frequency PCB board), the obtained high-frequency substrate has a uniform structure, a large peel strength, a uniform and stable dielectric constant and extremely low dielectric loss.
[0067] The present invention also provides spherical silica prepared by the above-mentioned preparation method of spherical silica, wherein the spherical silica has a high sphericity, a low surface silanol content and is not easy to absorb water.
[0068] The present invention also provides a method for preparing a polytetrafluoroethylene film, wherein the method uses the spherical silica as a filler. The present invention does not limit the specific method for preparing the polytetrafluoroethylene film, and the method may be a preparation step of a polytetrafluoroethylene film filled with a conventional filler in the art. In a preferred embodiment, the method for preparing the polytetrafluoroethylene film comprises the following steps:
[0069] A1. Mix spherical silica with water, disperse by ultrasonic, let stand, remove the precipitate, and obtain a stable dispersion;
[0070] A2. Adding the dispersion into the polytetrafluoroethylene solution under stirring to obtain a slurry;
[0071] A3, coating the slurry on a mold, and drying to obtain a polytetrafluoroethylene film;
[0072] Wherein, the spherical silica is the spherical silica described above.
[0073] The present invention does not limit the time of ultrasonic dispersion in step A1, as long as the spherical silica can be evenly dispersed in water. In a specific embodiment, in step A1, the time of ultrasonic dispersion is 10 to 60 minutes.
[0074] In a preferred embodiment, the weight ratio of the spherical silica to polytetrafluoroethylene is 1:1.5-4. Within the above dosage range, the obtained polytetrafluoroethylene has better performance, so that the dielectric constant of the high-frequency copper clad laminate made therefrom is more stable and the dielectric loss is lower.
[0075] In a specific embodiment, in step A2, the polytetrafluoroethylene solution is prepared according to the following process: polytetrafluoroethylene is mixed with water, wherein the weight ratio of polytetrafluoroethylene to water is 1:1-20.
[0076] In a specific embodiment, in step A2, the stirring speed is 500-1000 rpm, and the spherical silica can be more evenly dispersed in the polytetrafluoroethylene skeleton by fully mixing the dispersion containing spherical silica with the polytetrafluoroethylene solution at the above stirring speed.
[0077] Furthermore, in step A2, the dispersion is added at a rate of 50 to 70 mL / min. At the above addition rate, the spherical silica and polytetrafluoroethylene are mixed evenly and the operation time is short.
[0078] In a preferred embodiment, in step A3, the drying conditions include: a temperature of 110 to 130° C. and a time of 60 to 90 min.
[0079] The present invention also provides a polytetrafluoroethylene film prepared by the polytetrafluoroethylene film preparation method as described above.
[0080] The present invention also provides a high-frequency copper-clad laminate, which includes the spherical silica or polytetrafluoroethylene film as described above. Since the surface adsorbed water and polar group content of spherical silica are low and the dispersion is high, the high-frequency copper-clad laminate made of spherical silica or polytetrafluoroethylene film filled with spherical silica has a uniform and stable structure, a large copper foil peeling strength, a stable and low dielectric constant, and extremely low dielectric loss.
[0081] The present invention does not limit the preparation method of the high-frequency copper clad laminate, and the high-frequency copper clad laminate can be prepared according to conventional procedures in the art. In a preferred embodiment, the high-frequency copper clad laminate is prepared according to the following procedures:
[0082] S1. Sinter the polytetrafluoroethylene film at 400-450°C for 2-10 minutes, then take it out and cool it down;
[0083] S2, cutting the cooled polytetrafluoroethylene film into a required size, covering the upper surface of the cut polytetrafluoroethylene film with a first electronic copper foil and the lower surface with a second electronic copper foil, to obtain a sandwich-like system;
[0084] S3. Place the sandwich-like system obtained in step S2 between two mirror steel plates (surface roughness less than ±2um), and place them flat in a vacuum hot press. Perform vacuum hot pressing at 380-400°C and 400-600psi. After 1-2 hours, cool naturally while maintaining the pressure (cooling rate less than 10°C / min), remove the two mirror steel plates at room temperature, and obtain a high-frequency copper clad laminate.
[0085] The present invention will be described in detail below by way of examples, but the protection scope of the present invention is not limited thereto. The experimental methods in the following examples, unless otherwise specified, are conventional methods in the art. The experimental materials used in the following examples, unless otherwise specified, are all commercially available.
[0086] In the following examples and comparative examples, parts are by weight.
[0087] Example 1
[0088] 1. Preparation of spherical silica
[0089] (1) dissolving 0.1 parts of sodium hydroxide in 500 parts of deionized water to obtain a sodium hydroxide solution, and mixing 1 part of a cationic surfactant, hexadecyltrimethylammonium bromide, with the sodium hydroxide solution at 80° C. and stirring (stirring speed is 1000 rpm) to obtain a first solution;
[0090] (2) slowly dropping 1 part of polytetrafluoroethylene into the first solution at 80° C. and stirring (stirring speed is 1000 rpm), and mixing well to obtain a second solution;
[0091] (3) mixing 1 part of tetraethoxysilane and 1 / 10 part of a modifier at room temperature to obtain a mixed solution, wherein the modifier is (3,3,3-trifluoropropyl)trimethoxysilane;
[0092] (4) slowly dripping the mixed solution obtained in step (3) into the second solution obtained in step (2) at 80° C. and high-speed stirring (stirring speed of 1000 rpm), and then stirring at room temperature and high-speed stirring (stirring speed of 1000 rpm) for 2 h, and a flocculent precipitate is slowly formed to obtain a mixture;
[0093] (5) filtering the mixture containing the precipitate, freeze-drying the obtained solid under vacuum, and collecting the obtained solid;
[0094] (6) The solid obtained in step (5) was heated to 120° C. at a rate of 5° C. / min, vacuum dried, maintained at the set temperature for 6 h, cooled to room temperature and taken out, and then refluxed and extracted with ethanol (95%) for 6 h. The solid obtained was heated to 120° C. at a rate of 10° C. / min, vacuum dried, maintained at the set temperature for 6 h, cooled to room temperature and taken out to obtain spherical silica with a diameter of about 100 nm ( Figure 1 ), the spherical silicon dioxide is a white powdery solid particle aggregate.
[0095] 2. Preparation of polytetrafluoroethylene film
[0096] A1. Mix 1 part of the above spherical silica with 100 parts of deionized water, and disperse by ultrasonic for 60 minutes. After standing at room temperature for 30 minutes, remove the precipitate to obtain a stable dispersion;
[0097] A2, 1.88 parts of polytetrafluoroethylene and 10 parts of deionized water were mixed, and the mixture was slowly stirred (stirring speed 300 rpm) for 1 hour at room temperature to obtain a polytetrafluoroethylene solution; under conditions of high-speed stirring (stirring speed 1000 rpm) and room temperature, the dispersion obtained in A1 was slowly added (addition rate 60 mL / min) to the polytetrafluoroethylene solution to obtain a uniform coating slurry;
[0098] A3, the coating slurry is evenly applied on the polytetrafluoroethylene mold by dripping, and dried at 120°C for 60 minutes, and then the mold is taken out and the film formed on the mold is peeled off while hot to obtain a polytetrafluoroethylene film film ( Figure 2 ), the polytetrafluoroethylene film is milky white, opaque and has a certain elasticity.
[0099] Example 2
[0100] 1. Preparation of spherical silica
[0101] (1) dissolving 0.1 parts of sodium hydroxide in 500 parts of deionized water to obtain a sodium hydroxide solution, and mixing 1 part of a cationic surfactant, hexadecyltriethylammonium bromide, with the sodium hydroxide solution at 80° C. and stirring (stirring speed is 1000 rpm) to obtain a first solution;
[0102] (2) slowly dropping 1 part of polytetrafluoroethylene into the first solution at 80° C. and stirring (stirring speed is 1000 rpm), and mixing well to obtain a second solution;
[0103] (3) mixing 1 part of tetraethoxysilane and 1 / 10 part of a modifier at room temperature to obtain a mixed solution, wherein the modifier is (3,3,3-trifluoropropyl)trimethoxysilane;
[0104] (4) slowly dripping the mixed solution obtained in step (3) into the second solution obtained in step (2) at 80° C. and high-speed stirring (stirring speed of 1000 rpm), and then stirring at room temperature and high-speed stirring (stirring speed of 1000 rpm) for 2 h, and a flocculent precipitate is slowly formed to obtain a mixture;
[0105] (5) filtering the mixture containing the precipitate, freeze-drying the obtained solid under vacuum, and collecting the obtained solid;
[0106] (6) The solid obtained in step (5) is heated to 120°C at a rate of 5°C / min, vacuum dried, maintained at the set temperature for 6 hours, cooled to room temperature and taken out, and then reflux extracted with ethanol (95%) for 6 hours, and the solid is heated to 120°C at a rate of 10°C / min, vacuum dried, maintained at the set temperature for 6 hours, cooled to room temperature and taken out to obtain spherical silica.
[0107] 2. Preparation of polytetrafluoroethylene film
[0108] A1. Mix 1 part of the above spherical silica with 100 parts of deionized water, and disperse by ultrasonic for 60 minutes. After standing at room temperature for 30 minutes, remove the precipitate to obtain a stable dispersion;
[0109] A2, 1.88 parts of polytetrafluoroethylene and 10 parts of deionized water were mixed, and the mixture was slowly stirred (stirring speed 300 rpm) for 1 hour at room temperature to obtain a polytetrafluoroethylene solution; under conditions of high-speed stirring (stirring speed 1000 rpm) and room temperature, the dispersion obtained in step A1 was slowly added (addition rate 60 mL / min) to the polytetrafluoroethylene solution to obtain a uniform coating slurry;
[0110] A3. The coating slurry is evenly dripped onto a polytetrafluoroethylene mold, dried at 120° C. for 60 min, and then the mold is taken out and the film formed on the mold is peeled off while hot to obtain a polytetrafluoroethylene film film.
[0111] Example 3
[0112] 1. Preparation of spherical silica
[0113] (1) dissolving 0.1 parts of sodium hydroxide in 500 parts of deionized water to obtain a sodium hydroxide solution, and mixing 1 part of a cationic surfactant, hexadecyltrimethylammonium bromide, with the sodium hydroxide solution at 80° C. and stirring (stirring speed is 1000 rpm) to obtain a first solution;
[0114] (2) slowly dropping 1 part of polytetrafluoroethylene into the first solution at 80° C. and stirring (stirring speed is 1000 rpm), and mixing well to obtain a second solution;
[0115] (3) mixing 1 part of tetraethoxysilane and 1 / 10 part of a modifier at room temperature to obtain a mixed solution, wherein the modifier is (3,3,3-trifluoropropyl)triethoxysilane;
[0116] (4) slowly dripping the mixed solution obtained in step (3) into the second solution obtained in step (2) at 80° C. and high-speed stirring (stirring speed of 1000 rpm), and then stirring at room temperature and high-speed stirring (stirring speed of 1000 rpm) for 2 h, and a flocculent precipitate is slowly formed to obtain a mixture;
[0117] (5) filtering the mixture containing the precipitate, freeze-drying the obtained solid under vacuum, and collecting the obtained solid;
[0118] (6) The solid obtained in step (5) is heated to 120°C at a rate of 5°C / min, vacuum dried, maintained at the set temperature for 6 hours, cooled to room temperature and taken out, and then reflux extracted with ethanol (95%) for 6 hours, and the solid is heated to 120°C at a rate of 10°C / min, vacuum dried, maintained at the set temperature for 6 hours, cooled to room temperature and taken out to obtain spherical silica.
[0119] 2. Preparation of polytetrafluoroethylene film
[0120] A1. Mix 1 part of the above spherical silica with 100 parts of deionized water, and disperse by ultrasonic for 60 minutes. After standing at room temperature for 30 minutes, remove the precipitate to obtain a stable dispersion;
[0121] A2, 1.88 parts of polytetrafluoroethylene and 10 parts of deionized water were mixed, and the mixture was slowly stirred (stirring speed 300 rpm) for 1 hour at room temperature to obtain a polytetrafluoroethylene solution; under conditions of high-speed stirring (stirring speed 1000 rpm) and room temperature, the dispersion obtained in step A1 was slowly added (addition rate 60 mL / min) to the polytetrafluoroethylene solution to obtain a uniform coating slurry;
[0122] A3. The coating slurry is evenly dripped onto a polytetrafluoroethylene mold, dried at 120° C. for 60 min, and then the mold is taken out and the film formed on the mold is peeled off while hot to obtain a polytetrafluoroethylene film film.
[0123] Example 4
[0124] 1. Preparation of spherical silica
[0125] (1) dissolving 0.1 parts of sodium hydroxide in 500 parts of deionized water to obtain a sodium hydroxide solution, and mixing 1 part of a cationic surfactant, hexadecyltriethylammonium bromide, with the sodium hydroxide solution at 80° C. and stirring (stirring speed is 1000 rpm) to obtain a first solution;
[0126] (2) slowly dropping 1 part of polytetrafluoroethylene into the first solution at 80° C. and stirring (stirring speed is 1000 rpm), and mixing well to obtain a second solution;
[0127] (3) mixing 1 part of tetraethoxysilane and 1 / 10 part of a modifier at room temperature to obtain a mixed solution, wherein the modifier is (3,3,3-trifluoropropyl)triethoxysilane;
[0128] (4) slowly dripping the mixed solution obtained in step (3) into the second solution obtained in step (2) at 80° C. and high-speed stirring (stirring speed of 1000 rpm), and then stirring at room temperature and high-speed stirring (stirring speed of 1000 rpm) for 2 h, and a flocculent precipitate is slowly formed to obtain a mixture;
[0129] (5) filtering the mixture containing the precipitate, freeze-drying the obtained solid under vacuum, and collecting the obtained solid;
[0130] (6) The solid obtained in step (5) is heated to 120°C at a rate of 5°C / min, vacuum dried, maintained at the set temperature for 6 hours, cooled to room temperature and taken out, and then reflux extracted with ethanol (95%) for 6 hours, and the solid is heated to 120°C at a rate of 10°C / min, vacuum dried, maintained at the set temperature for 6 hours, cooled to room temperature and taken out to obtain spherical silica.
[0131] 2. Preparation of polytetrafluoroethylene film
[0132] A1. Mix 1 part of the above spherical silica with 100 parts of deionized water, and disperse by ultrasonic for 60 minutes. After standing at room temperature for 30 minutes, remove the precipitate to obtain a stable dispersion;
[0133] A2, 1.88 parts of polytetrafluoroethylene and 10 parts of deionized water were mixed, and the mixture was slowly stirred (stirring speed 300 rpm) for 1 hour at room temperature to obtain a polytetrafluoroethylene solution; under conditions of high-speed stirring (stirring speed 1000 rpm) and room temperature, the dispersion obtained in step A1 was slowly added (addition rate 60 mL / min) to the polytetrafluoroethylene solution to obtain a uniform coating slurry;
[0134] A3. The coating slurry is evenly dripped onto a polytetrafluoroethylene mold, dried at 120° C. for 60 min, and then the mold is taken out and the film formed on the mold is peeled off while hot to obtain a polytetrafluoroethylene film film.
[0135] Example 5
[0136] The method described in Example 1 was followed, except that when preparing the polytetrafluoroethylene film, the amount of polytetrafluoroethylene was adjusted to 2.33 parts;
[0137] That is, the weight ratio of spherical silica to polytetrafluoroethylene is 1:2.33, and the weight ratio of polytetrafluoroethylene to water is 2.33:10.
[0138] Example 6
[0139] The method described in Example 1 was followed, except that when preparing the polytetrafluoroethylene film, the amount of polytetrafluoroethylene was adjusted to 1.5 parts;
[0140] That is, the weight ratio of spherical silica to polytetrafluoroethylene is 1:1.5, and the weight ratio of polytetrafluoroethylene to water is 1.5:10.
[0141] Example 7
[0142] The method described in Example 1 was followed, except that the modifier was 3-aminopropyltrimethoxysilane.
[0143] Comparative Example 1
[0144] The method described in Example 1 is different from that in step (3) of preparing spherical silica, no modifier is added.
[0145] Comparative Example 2
[0146] The method described in Example 1 is different from that in the step (1) of preparing spherical silica, no cationic surfactant is added.
[0147] Comparative Example 3
[0148] The method described in Example 1 was followed, except that polytetrafluoroethylene was not added in step (2) of preparing spherical silica.
[0149] Material Testing
[0150] The polytetrafluoroethylene film obtained in the embodiment and the comparative example is made into a high-frequency copper-clad laminate, and the preparation method thereof comprises the following steps: sintering the polytetrafluoroethylene film at 400°C for 3-7 minutes, taking it out and cooling it; cutting the cooled polytetrafluoroethylene film into a required certain size, covering the upper surface of the cut polytetrafluoroethylene film with a first electronic copper foil (1oz / 35micron) and the lower surface with a second electronic copper foil (1oz / 35micron) to obtain a sandwich-like system; the obtained sandwich-like system is placed between two mirror steel plates (surface roughness is less than ±2um), and placed flat in a vacuum hot press, and vacuum hot pressing is performed under the conditions of 385°C and 460psi. After 2 hours, the pressure is maintained and the film is naturally cooled (the cooling rate is 5°C / min), and the two mirror steel plates are removed and taken out at room temperature to obtain a spherical silica-filled polytetrafluoroethylene-based high-frequency copper-clad laminate ( Figure 3 ).
[0151] The high-frequency copper clad laminate was subjected to performance testing. The testing method was as follows: According to the IPC-TM-6502.5.5.5C (1998) standard, the dielectric constant and dielectric loss of the high-frequency copper clad laminates prepared in the above Examples 1-7 and Comparative Examples 1-3 were tested under 10 GHz frequency electron wave radiation conditions; at the same time, the peel strength of the copper foil of the product was tested according to the IPC-TM-650 2.4.8C (1994) standard. The test results are shown in Table 1 below.
[0152] Table 1
[0153]
[0154] It can be seen from the results in Table 1 that the high-frequency copper clad laminates made from the polytetrafluoroethylene films of Examples 1-7 of the present invention have stable dielectric constants, low dielectric losses, and high copper foil peeling strength, and the high-frequency copper clad laminate made from the polytetrafluoroethylene film obtained in Example 1 has the best dielectric properties.
[0155] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A method for preparing spherical silicon dioxide, characterized in that: The method comprises the following steps: (1) mixing a cationic surfactant with a sodium hydroxide solution to obtain a first solution; (2) mixing polytetrafluoroethylene with the first solution to obtain a second solution; (3) mixing tetraethoxysilane and a modifier to obtain a mixed solution; (4) mixing the mixed solution with the second solution at 70 to 90° C., and then stirring at 20 to 30° C. to obtain a mixture; (5) separating the mixture into solid and liquid, and performing vacuum freeze-drying on the obtained solid; (6) vacuum drying the solid obtained in step (5), then reflux extraction, and then vacuum drying to obtain spherical silica; Wherein, the modifier is selected from at least one of (3,3,3-trifluoropropyl)trimethoxysilane, (3,3,3-trifluoropropyl)triethoxysilane, 3-aminopropyltrimethoxysilane and 3-aminopropyltriethoxysilane.
2. The method according to claim 1, characterized in that In step (1), the cationic surfactant is hexadecyltrimethylammonium bromide and / or hexadecyltriethylammonium bromide; Preferably, in step (1), the weight ratio of the cationic surfactant to the sodium hydroxide in the sodium hydroxide solution is 1:0.01-0.2; Preferably, in step (1), the mass fraction of sodium hydroxide in the sodium hydroxide solution is 0.01 to 0.1%; Preferably, in step (1), the mixing conditions include: a temperature of 80 to 100° C. and a stirring speed of 500 to 1000 rpm; Preferably, in step (2), the mixing conditions include: a temperature of 80 to 100° C. and a stirring speed of 500 to 1000 rpm.
3. The method according to claim 1, characterized in that In step (3), the weight ratio of the tetraethoxysilane to the modifier is 100:1-15.
4. The method according to claim 1, characterized in that: In step (6), the solvent used for reflux extraction is 95% ethanol; Preferably, in step (6), the reflux extraction time is 5 to 7 hours.
5. A spherical silicon dioxide prepared by the method described in any one of claims 1 to 4.
6. A method for preparing a polytetrafluoroethylene film, characterized in that: The method comprises the following steps: A1. Mix spherical silica with water, disperse by ultrasonic, let stand, remove the precipitate, and obtain a stable dispersion; A2. Adding the dispersion into the polytetrafluoroethylene solution under stirring to obtain a slurry; A3, coating the slurry on a mold, and drying to obtain a polytetrafluoroethylene film; Wherein, the spherical silica is the spherical silica according to claim 5.
7. The method according to claim 6, characterized in that The weight ratio of the spherical silicon dioxide to polytetrafluoroethylene is 1:1.5-4.
8. The method according to claim 6, characterized in that In step A2, the polytetrafluoroethylene solution is prepared according to the following process: polytetrafluoroethylene is mixed with water, wherein the weight ratio of polytetrafluoroethylene to water is 1:1 to 20; Preferably, in step A2, the stirring speed is 500-1000 rpm; Preferably, in step A2, the dispersion is added at a rate of 50 to 70 mL / min; Preferably, in step A3, the drying conditions include: a temperature of 110 to 130° C. and a time of 60 to 90 min.
9. A polytetrafluoroethylene film obtained by the method according to any one of claims 6 to 8.
10. A high frequency copper clad laminate, characterized in that: The high-frequency copper-clad laminate comprises the spherical silicon dioxide described in claim 5 or the polytetrafluoroethylene film described in claim 9.
Citation Information
Patent Citations
Organosilane compound, packing, resin composition and copper-clad plate
CN107641135A
Preparation method of polytetrafluoroethylene copper-clad plate with low dielectric constant and low loss
CN116731456A
Polytetrafluoroethylene film, polytetrafluoroethylene-based high-frequency copper-clad plate and preparation method thereof
CN117924858A
Low dielectric silica powder, resin composition containing the silica powder, and method for manufacturing low dielectric silica powder