Preparation method of high-purity vanadium pentoxide
Through the pH adjustment after vanadium slag roasting and acid leaching, combined with ammonium carbonate leaching and phosphorus removal and cold crystallization, the preparation process of vanadium pentoxide is simplified, the multi-step phosphorus control and wastewater circulation is solved, and high-purity pentoxide is achieved Efficient preparation and low cost production of vanadium.
Patent Information
- Application Number
- CN202411186739.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-11-19
AI Technical Summary
In the process of preparing high-purity vanadium pentoxide, the prior art requires multiple steps to control phosphorus, energy-consuming materials, and wastewater contains ammonium, which cannot be recycled, resulting in increased costs.
Use vanadium slag to add calcium salt to obtain calcified clinker, and then acid leaching is performed to adjust the pH value. The vanadium liquid is leached through ammonium carbonate, and the phosphorus removal and cold crystallization is performed. Finally, vanadium pentoxide is obtained, which simplifies the phosphorus control step and realizes wastewater circulation. .
The preparation of high-purity vanadium pentoxide is realized, which reduces production costs, reduces wastewater discharge, improves vanadium recycling efficiency, and simplifies the phosphorus control process.
Smart Images

Figure CN118978180A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of vanadium pentoxide preparation, and in particular to a method for preparing high-purity vanadium pentoxide. Background Art
[0002] In the process of using calcified vanadium liquid acid leaching solution to precipitate ammonium polyvanadate to prepare high-purity vanadium pentoxide, it is necessary to start by adding ammonium salts and then precipitate at high temperature. However, this will cause ammonium to be contained in the wastewater, which is not recycled, and consumes energy and materials, which significantly increases the cost. In addition, the above-mentioned vanadium slag extraction also needs to control a relatively high pH value to prevent the phosphorus content in the leaching solution from being too high to precipitate vanadium, and phosphorus is controlled multiple times during the secondary and tertiary leaching processes. At the same time, since phosphorus control in acidic vanadium liquid has always been a difficult point, multi-step phosphorus control is required. Summary of the invention
[0003] In view of this, in order to overcome at least one aspect of the above problems, an embodiment of the present invention provides a method for preparing high-purity vanadium pentoxide, comprising the following steps: Adding calcium salt to vanadium slag and roasting to obtain calcified clinker; Acid leaching is performed on the calcified clinker to obtain an acidic leaching solution; Adjusting the pH value of the acidic leaching solution, stirring and filtering to obtain a primary precipitate; alkaline leaching of the primary precipitated slag with ammonium carbonate to obtain alkaline vanadium liquid; Dephosphorizing the alkaline vanadium solution and then cooling and crystallizing it to obtain ammonium metavanadate; The ammonium metavanadate is calcined to obtain vanadium pentoxide.
[0004] In some embodiments, acid leaching the calcified clinker to obtain an acidic leachate further comprises: Acid leaching is carried out for 60-90 minutes under the conditions that the liquid-to-solid ratio of the leaching agent to the calcified clinker is 2-3:1 mL / g and the pH value is 2.4-2.8, and an acidic leaching solution and a primary residue are obtained.
[0005] In some embodiments, the pH value of the acidic leachate is adjusted, and then stirred and filtered to obtain a primary precipitate, further comprising: The pH value of the acidic leaching solution is adjusted to 9-10 with lime, and stirred for 30-40 minutes to obtain primary precipitate and primary wastewater.
[0006] In some embodiments, alkaline leaching of the primary precipitated slag with ammonium carbonate to obtain alkaline vanadium liquid further comprises: Mixing the primary precipitated residue with water to obtain a mixed solution, wherein the liquid-to-solid ratio of water to the primary precipitated residue is 1.5-2.0 mL / g; The ammonium carbonate is added to the mixed solution and leached at 80-95° C. for 30-50 min to obtain the alkaline vanadium solution and the secondary residue, wherein the ratio of the weight of the ammonium carbonate to the wet weight of the primary precipitated residue is 1-1.5:1.
[0007] In some embodiments, it also includes: The secondary residue is leached with the primary wastewater to obtain a primary leaching solution, wherein the leaching time is 30-60 minutes, so as to extract the residual vanadium in the secondary residue.
[0008] In some embodiments, it also includes: When the primary wastewater is used to leach the secondary residue, the pH value is adjusted to 2.8-3.0.
[0009] In some embodiments, it also includes: Leaching the primary residue with the leaching solution to obtain a secondary leaching solution, wherein the leaching time is 10-20 minutes, so as to extract residual vanadium in the primary residue; The secondary leachate is returned as a leaching agent to carry out leaching of the calcified clinker.
[0010] In some embodiments, it also includes: When the primary residue is leached with the leaching solution, the pH value is adjusted to 1.2-1.5.
[0011] In some embodiments, the alkaline vanadium solution is dephosphorized and then cooled and crystallized to obtain ammonium metavanadate, further comprising: Adding aluminum sulfate to the alkaline vanadium solution, wherein the aluminum sulfate is added in an amount such that the mass ratio of Al / P is 0.6-0.87; Stirring for 15-20 minutes, standing and aging for 20-30 minutes, and then filtering to obtain the alkaline vanadium solution after impurities are removed; The alkaline vanadium liquid after impurity removal is cooled and crystallized at a temperature of 5-15° C. to obtain ammonium metavanadate and secondary wastewater.
[0012] In some embodiments, it also includes: The secondary wastewater is returned to be mixed with the primary sedimentation residue.
[0013] The present invention has one of the following beneficial technical effects: the scheme proposed by the present invention is to use a vanadium precipitator to adjust the pH value of the vanadium-containing acid leaching solution obtained after acid leaching of calcified clinker, directly precipitate all vanadium and impurities, and then use ammonium carbonate to leach the vanadium therein with the precipitated slag as a raw material, and only phosphorus removal needs to be carried out in the alkaline vanadium solution, without the need for multi-step phosphorus removal. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings in the following description are only some embodiments of the present invention. For ordinary technicians in this field, other embodiments can be obtained based on these drawings without paying creative work.
[0015] Figure 1 A schematic flow chart of a method for preparing high-purity vanadium pentoxide provided in an embodiment of the present invention; Figure 2 A flowchart of a method for preparing high-purity vanadium pentoxide provided in an embodiment of the present invention. DETAILED DESCRIPTION
[0016] In order to make the objectives, technical solutions and advantages of the present invention more clearly understood, the embodiments of the present invention are further described in detail below in combination with specific embodiments and with reference to the accompanying drawings.
[0017] It should be noted that all expressions using "first" and "second" in the embodiments of the present invention are for distinguishing two non-identical entities with the same name or non-identical parameters. It can be seen that "first" and "second" are only for the convenience of expression and should not be understood as limitations on the embodiments of the present invention. The subsequent embodiments will not explain this one by one.
[0018] According to one aspect of the present invention, an embodiment of the present invention provides a method for preparing high-purity vanadium pentoxide, such as Figure 1 As shown, it may include the steps of: Adding calcium salt to vanadium slag and roasting to obtain calcified clinker; Acid leaching is performed on the calcified clinker to obtain an acidic leaching solution; Adjusting the pH value of the acidic leaching solution, stirring and filtering to obtain a primary precipitate; alkaline leaching of the primary precipitated slag with ammonium carbonate to obtain alkaline vanadium liquid; Dephosphorizing the alkaline vanadium solution and then cooling and crystallizing it to obtain ammonium metavanadate; The ammonium metavanadate is calcined to obtain vanadium pentoxide.
[0019] The solution proposed by the present invention is to use a vanadium precipitator to adjust the pH value of the vanadium-containing acid leaching solution obtained after acid leaching of calcified clinker, directly precipitate all vanadium and impurities, and then use ammonium carbonate to leach the vanadium therein using the precipitated slag as a raw material. In addition, phosphorus removal only needs to be carried out in the alkaline vanadium solution, and multi-step phosphorus removal is not required.
[0020] In some embodiments, acid leaching the calcified clinker to obtain an acidic leachate further comprises: Acid leaching is carried out for 60-90 minutes under the conditions that the liquid-to-solid ratio of the leaching agent to the calcified clinker is 2-3:1 mL / g and the pH value is 2.4-2.8, and an acidic leaching solution and a primary residue are obtained.
[0021] In some embodiments, the pH value of the acidic leachate is adjusted, and then stirred and filtered to obtain a primary precipitate, further comprising: The pH value of the acidic leaching solution is adjusted to 9-10 with lime, and stirred for 30-40 minutes to obtain primary precipitate and primary wastewater.
[0022] In some embodiments, alkaline leaching of the primary precipitated slag with ammonium carbonate to obtain alkaline vanadium liquid further comprises: Mixing the primary precipitated residue with water to obtain a mixed solution, wherein the liquid-to-solid ratio of water to the primary precipitated residue is 1.5-2.0 mL / g; The ammonium carbonate is added to the mixed solution and leached at 80-95° C. for 30-50 min to obtain the alkaline vanadium solution and the secondary residue, wherein the ratio of the weight of the ammonium carbonate to the wet weight of the primary precipitated residue is 1-1.5:1.
[0023] In some embodiments, it also includes: The secondary residue is leached with the primary wastewater to obtain a primary leaching solution, wherein the leaching time is 30-60 minutes, so as to extract the residual vanadium in the secondary residue.
[0024] In some embodiments, it also includes: When the primary wastewater is used to leach the secondary residue, the pH value is adjusted to 2.8-3.0.
[0025] In some embodiments, it also includes: Leaching the primary residue with the leaching solution to obtain a secondary leaching solution, wherein the leaching time is 10-20 minutes, so as to extract residual vanadium in the primary residue; The secondary leachate is returned as a leaching agent to carry out leaching of the calcified clinker.
[0026] In some embodiments, it also includes: When the primary residue is leached with the leaching solution, the pH value is adjusted to 1.2-1.5.
[0027] In some embodiments, the alkaline vanadium solution is dephosphorized and then cooled and crystallized to obtain ammonium metavanadate, further comprising: Adding aluminum sulfate to the alkaline vanadium solution, wherein the aluminum sulfate is added in an amount such that the mass ratio of Al / P is 0.6-0.87; Stirring for 15-20 minutes, standing and aging for 20-30 minutes, and then filtering to obtain the alkaline vanadium solution after impurities are removed; The alkaline vanadium liquid after impurity removal is cooled and crystallized at a temperature of 5-15° C. to obtain ammonium metavanadate and secondary wastewater.
[0028] In some embodiments, it also includes: The secondary wastewater is returned to be mixed with the primary sedimentation residue.
[0029] Specifically, Figure 2 As shown in the figure, calcium salt is added to vanadium slag for roasting to obtain calcified clinker, wherein V 2 O 5 Content is 9%-25%, CaO / V 2 O 5 The content of calcium is 0.3%-0.6%, the content of phosphorus is 0.03%-1.5%, and the rest are impurities. Then weigh a certain amount of calcified clinker, use a liquid-solid ratio of 2-3:1 and leach for 60-90 minutes at a pH of 2.4-2.8 to obtain an acidic leachate and a primary residue; the acidic leachate is adjusted to pH 9-10 with lime, stirred for 30-40 minutes and filtered to obtain a primary precipitate and primary wastewater; the precipitate is treated with tap water or returned secondary wastewater at a liquid-solid ratio of 1.5-2.0:1, ammonium carbonate is added (the amount added is the weight of ammonium carbonate: the wet weight of precipitate is 1-1.5:1), and leached for 30-50 minutes at 80-95°C, and then filtered to obtain an alkaline vanadium liquid and a secondary residue; the alkaline vanadium liquid is added with aluminum sulfate impurity remover at Al / P=0.6-0.87, After impurities are removed, the ammonium metavanadate is cooled to 5-15°C to crystallize and precipitate, and ammonium metavanadate and secondary wastewater are obtained after filtration; ammonium metavanadate is calcined to obtain vanadium pentoxide, and the secondary wastewater is returned as a precipitate slag leaching agent; the primary wastewater is returned to leach the secondary residue, and the pH value is adjusted to 2.8-3.0 during the leaching process, and the leaching is performed for 30-60 minutes, and the tertiary residue and the acidic leaching solution of the certain value are obtained by filtering; the acidic leaching solution with a pH value of 2.8-3.0 is obtained to leach the primary residue again, and the pH value is adjusted to 1.2-1.5 during the leaching process, and the leaching is performed for 10-20 minutes and then filtered to obtain the quaternary residue and the acidic leaching solution with a pH value of 1.2-1.5, and the acidic leaching solution with a pH value of 1.2-1.5 is returned as a leaching agent to leach the clinker.
[0030] It should be noted that since the secondary residue has been leached once, most of the vanadium is already present in the alkaline vanadium solution. Therefore, when using the primary wastewater to leach the secondary residue, the pH value needs to be controlled not to be too low to prevent impurities such as manganese from being leached. When leaching the primary residue, since it has already been leached once at an acidic pH of 2.4-2.8, the pH value needs to be further lowered to leach the vanadium remaining in the primary residue.
[0031] Example 1 Weigh 200g of calcified clinker (V 2 O 5 Content 9%, CaO / V 2 O 5 (mass ratio) is 0.3, P content is 0.03%), and a liquid-to-solid ratio of 2:1 is used for leaching at a pH value of 2.4 for 60 minutes to obtain an acidic leachate and a primary residue; the acidic leachate is adjusted to pH 9 with lime, stirred for 30 minutes and then filtered to obtain a primary precipitate and a primary wastewater; the precipitate is leached at 80°C for 30 minutes with tap water or returned secondary wastewater at a liquid-to-solid ratio of 1.5:1, and ammonium carbonate is added (the amount added is the weight of ammonium carbonate: the wet weight of the precipitate is 1:1) and then filtered to obtain an alkaline vanadium liquid and a secondary residue; the alkaline vanadium liquid is added with aluminum sulfate as an impurity remover at Al / P=0.6 After impurities are removed, the ammonium metavanadate is cooled to 5°C for crystallization and precipitation, and ammonium metavanadate and secondary wastewater are obtained after filtration; ammonium metavanadate is calcined to obtain vanadium pentoxide, and the secondary wastewater is returned as a precipitate leaching agent; the primary wastewater is returned to leach the secondary residue, and the pH value is adjusted to 2.8 during the leaching process, and the leaching is carried out for 30 minutes, and the tertiary residue and the acidic leachate of the certain value are obtained by filtration; the pH2.8 acidic leachate obtained is used to leach the primary residue again, and the pH value is adjusted to 1.2 during the leaching process, and the pH value is filtered after leaching for 10 minutes to obtain the quaternary residue and the acidic leachate of pH 1.2, and the acidic leachate of pH 1.2 is returned as a leaching agent to leach the clinker.
[0032] The composition of vanadium pentoxide obtained is: V 2 O 5 Content 99.75%, Si: 0.015%, Fe<0.01%, P: 0.012%, S: 0.015%, As<0.01%, Na 2 O+K 2 O: 0.015%, Ca: 0.015%, Mg: 0.014%, Mn < 0.025%; the V content in the secondary residue component is 0.68%; the V content in the quaternary residue component is 0.53%; the V content in the tertiary residue is 0.28%, and the Mn content is 78.2%.
[0033] Comparative Example: The obtained acidic vanadium solution is directly precipitated with vanadium, and the vanadium pentoxide obtained by calcination is: V 2 O 5 Content 98.2%, Si: 0.272%, Fe: 0.08%, P: 0.04%, S: 0.08%, As < 0.01%, Na 2 O+K 2 O: 0.025%, Ca: 0.13%, Mg: 0.18%, Mn: 0.34%. Obviously, the calcium, magnesium and manganese content is very high.
[0034] Example 2 Weigh a certain amount of calcified clinker (V 2 O 5 Content 15%, CaO / V 2 O 5 (mass ratio) 0.5, P content 0.9%), using a liquid-to-solid ratio of 2.5:1 at a pH value of 2.6 for 80 minutes to obtain an acidic leachate and a primary residue; the acidic leachate is adjusted to pH 9.5 with lime, stirred for 35 minutes and then filtered to obtain a primary precipitate and primary wastewater; the precipitate is leached at 90°C for 40 minutes with tap water or returned secondary wastewater at a liquid-to-solid ratio of 1.8:1 and ammonium carbonate (the amount of ammonium carbonate added is 1.2:1: the wet weight of the precipitate) and then filtered to obtain an alkaline vanadium solution and a secondary residue; the alkaline vanadium solution is added with aluminum sulfate as an impurity remover at Al / P=0.7 to remove After impurities, cool to 5-15℃ to crystallize and precipitate ammonium metavanadate, and filter to obtain ammonium metavanadate and secondary wastewater; calcine ammonium metavanadate to obtain vanadium pentoxide, and the secondary wastewater is returned as a precipitate leaching agent; the primary wastewater is returned to leach the secondary residue, and the pH value is adjusted to 2.9 during the leaching process, leaching for 50 minutes, and filtering to obtain a tertiary residue and an acidic leachate of a certain value; the obtained pH2.9 acidic leachate is used to leach the primary residue again, and the pH value is adjusted to 1.35 during the leaching process, and leaching for 15 minutes is filtered to obtain a quaternary residue and an acidic leachate of pH 1.35, and the acidic leachate of pH 1.35 is returned as a leaching agent to leach clinker.
[0035] The composition of vanadium pentoxide obtained is: V 2 O 5 Content 99.78%, Si: 0.012%, Fe<0.01%, P: 0.010%, S: 0.011%, As<0.01%, Na 2 O+K 2 O: 0.012%, Ca: 0.012%, Mg: 0.010%, Mn < 0.014%; the V content in the secondary residue component is 0.72%; the V content in the quaternary residue component is 0.54%; the V content in the tertiary residue is 0.26%, and the Mn content is 82.2%.
[0036] Comparative Example: The obtained acidic vanadium solution is directly precipitated with vanadium, and the vanadium pentoxide obtained by calcination is: V 2 O 5 Content: 98.4%, Si: 0.24%, Fe: 0.07%, P: 0.035%, S: 0.08%, As < 0.01%, Na 2 O+K 2 O: 0.022%, Ca: 0.15%, Mg: 0.18%, Mn: 0.35%. The phosphorus is obviously high and needs to be controlled. The calcium, magnesium and manganese content is very high.
[0037] Example 3 Weigh a certain amount of calcified clinker, use a liquid-solid ratio of 3:1 to leach at pH 2.8 for 90 minutes to obtain an acidic leachate and a primary residue; adjust the pH of the acidic leachate to 10 with lime, stir for 40 minutes and filter to obtain a primary precipitate and primary wastewater; use tap water or returned secondary wastewater at a liquid-solid ratio of 2.0:1, add ammonium carbonate (the added amount of ammonium carbonate weight: the wet weight of the precipitate is 1.5:1) to leach the precipitate at 95°C for 50 minutes, and then filter to obtain an alkaline vanadium liquid and a secondary residue; add aluminum sulfate impurity remover at Al / P=0.87 to the alkaline vanadium liquid, remove impurities and cool it down. Crystallize and precipitate ammonium metavanadate at 15℃, and obtain ammonium metavanadate and secondary wastewater after filtration; calcine ammonium metavanadate to obtain vanadium pentoxide, and the secondary wastewater is returned as a precipitate slag leaching agent; the primary wastewater is returned to leach the secondary residue, and the pH value is adjusted to 3.0 during the leaching process, leaching for 60 minutes, and filtering to obtain a tertiary residue and an acidic leaching solution of a certain value; the obtained pH2.8-3.0 acidic leaching solution is used to leach the primary residue again, and the pH value is adjusted to 1.5 during the leaching process, and leaching for 20 minutes is filtered to obtain a quaternary residue and an acidic leaching solution with a pH value of 1.5, and the acidic leaching solution with a pH value of 1.5 is returned as a leaching agent to leach clinker.
[0038] The composition of vanadium pentoxide obtained is: V 2 O 5 Content 99.85%, Si<0.01%, Fe<0.01%, P<0.01%, S: 0.012%, As<0.01%, Na 2 O+K 2 O: 0.013%, Ca: 0.09%, Mg: 0.011%, Mn < 0.01%; the V content in the secondary residue component is 0.80%, the V content in the quaternary residue component is 0.56%; the V content in the tertiary residue is 0.16%, and the Mn content is 85.6%.
[0039] Comparative Example: The obtained acidic vanadium solution is directly precipitated with vanadium, and the vanadium pentoxide obtained by calcination is: V 2 O 5 Content 98.6%, Si: 0.23%, Fe: 0.06%, P: 0.028%, S: 0.08%, As < 0.01%, Na 2 O+K 2 O: 0.023%, Ca: 0.10%, Mg: 0.17%, Mn: 0.32%. The phosphorus is obviously high and needs to be controlled. The calcium, magnesium and manganese content is very high.
[0040] The scheme proposed in the present invention adopts the vanadium-containing acid leaching solution and the primary residue obtained after the acid leaching of the calcified clinker. The vanadium-containing acid leaching solution uses a precipitant to directly precipitate all vanadium and impurities to obtain a primary precipitate residue and a primary vanadium precipitation wastewater. The primary precipitate residue is then leached with ammonium carbonate to obtain alkaline vanadium liquid and secondary residue; then the pH of the secondary residue is adjusted with the primary vanadium precipitation wastewater to obtain an acidic leaching solution with a certain pH value, and the pH value is then adjusted to leach the primary residue. The acidic leaching solution with a certain pH value is returned to the clinker for leaching; the secondary vanadium precipitation wastewater after vanadium precipitation in the alkaline leaching solution is continuously returned to leach the primary precipitate residue. The vanadium product precipitated in this way is of good quality, with low residual vanadium, high vanadium recovery, and the wastewater is recycled without external discharge. The process does not require deliberate phosphorus control, and it is very easy to remove phosphorus in the alkaline vanadium liquid obtained by the second leaching.
[0041] The above are exemplary embodiments disclosed in the present invention, but it should be noted that various changes and modifications may be made without departing from the scope disclosed in the embodiments of the present invention as defined in the claims. The functions, steps and / or actions of the method claims according to the disclosed embodiments described herein do not need to be performed in any particular order. In addition, although the elements disclosed in the embodiments of the present invention may be described or required in individual form, they may also be understood as multiple unless explicitly limited to the singular.
[0042] It should be understood that, as used herein, the singular forms "a", "an" are intended to include the plural forms as well, unless the context clearly supports an exception. It should also be understood that, as used herein, "and / or" refers to any and all possible combinations including one or more of the associated listed items.
[0043] The serial numbers of the embodiments disclosed in the above embodiments of the present invention are only for description and do not represent the advantages or disadvantages of the embodiments.
[0044] A person skilled in the art should understand that the discussion of any of the above embodiments is only exemplary and is not intended to imply that the scope of the disclosure of the embodiments of the present invention (including the claims) is limited to these examples; under the concept of the embodiments of the present invention, the technical features in the above embodiments or different embodiments can also be combined, and there are many other changes in different aspects of the above embodiments of the present invention, which are not provided in detail for the sake of simplicity. Therefore, any omissions, modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the embodiments of the present invention should be included in the protection scope of the embodiments of the present invention.
Claims
1. A method for preparing high-purity vanadium pentoxide, characterized in that: The following steps are involved: Add calcium salt to vanadium slag and roast it to obtain calcified clinker; Acid leaching is performed on the calcified clinker to obtain an acidic leaching solution; Adjusting the pH value of the acidic leaching solution, stirring and filtering to obtain a primary precipitate; alkaline leaching of the primary precipitated slag with ammonium carbonate to obtain alkaline vanadium liquid; Dephosphorizing the alkaline vanadium solution and then cooling and crystallizing it to obtain ammonium metavanadate; The ammonium metavanadate is calcined to obtain vanadium pentoxide.
2. The method according to claim 1, characterized in that Acid leaching the calcified clinker to obtain an acidic leachate further comprises: Acid leaching is carried out for 60-90 minutes under the conditions that the liquid-to-solid ratio of the leaching agent to the calcified clinker is 2-3:1 mL / g and the pH value is 2.4-2.8, and an acidic leaching solution and a primary residue are obtained.
3. The method according to claim 2, characterized in that After adjusting the pH value of the acidic leaching solution, stirring and filtering to obtain a primary precipitate residue, further comprising: The pH value of the acidic leaching solution is adjusted to 9-10 with lime, and stirred for 30-40 minutes to obtain primary precipitate and primary wastewater.
4. The method according to claim 3, characterized in that The primary precipitated slag is subjected to alkaline leaching with ammonium carbonate to obtain alkaline vanadium liquid, further comprising: Mixing the primary precipitated residue with water to obtain a mixed solution, wherein the liquid-to-solid ratio of water to the primary precipitated residue is 1.5-2.0 mL / g; The ammonium carbonate is added to the mixed solution and leached at 80-95° C. for 30-50 min to obtain the alkaline vanadium solution and the secondary residue, wherein the ratio of the weight of the ammonium carbonate to the wet weight of the primary precipitated residue is 1-1.5:
1.
5. The method according to claim 4, characterized in that Also includes: The secondary residue is leached with the primary wastewater to obtain a primary leaching solution, wherein the leaching time is 30-60 minutes, so as to extract the residual vanadium in the secondary residue.
6. The method according to claim 5, characterized in that Also includes: When the primary wastewater is used to leach the secondary residue, the pH value is adjusted to 2.8-3.
0.
7. The method according to claim 5, characterized in that Also includes: Leaching the primary residue with the leaching solution to obtain a secondary leaching solution, wherein the leaching time is 10-20 minutes, so as to extract residual vanadium in the primary residue; The secondary leachate is returned as a leaching agent to carry out leaching of the calcified clinker.
8. The method according to claim 7, characterized in that Also includes: When the primary residue is leached with the leaching solution, the pH value is adjusted to 1.2-1.
5.
9. The method according to claim 4, characterized in that The alkaline vanadium solution is dephosphorized and then cooled and crystallized to obtain ammonium metavanadate, further comprising: Adding aluminum sulfate to the alkaline vanadium solution, wherein the aluminum sulfate is added in an amount such that the mass ratio of Al / P is 0.6-0.87; Stirring for 15-20 minutes, standing and aging for 20-30 minutes, and then filtering to obtain the alkaline vanadium solution after impurities are removed; The alkaline vanadium liquid after impurity removal is cooled and crystallized at a temperature of 5-15° C. to obtain ammonium metavanadate and secondary wastewater.
10. The method according to claim 5, characterized in that Also includes: The secondary wastewater is returned to be mixed with the primary sedimentation residue.
Citation Information
Cited By
Preparation method of high-purity vanadium pentoxide
CN121361833A
Method for preparing vanadium-aluminum alloy through adaptation of multi-impurity vanadium-containing solution
CN122061001A