Curved-surface photosensitive glass and preparation method and application thereof

By adjusting the oxide composition and treatment process, the shielding performance of curved photosensitive glass is improved, and the problem of insufficient shielding performance of visible and near-infrared light in the exposure area in the prior art is solved, and the application needs of mobile phone covers and smart watches are met.

CN118978333AActive Publication Date: 2024-11-19CHONGQING AUREAVIA HI TECH GLASS CO LTD

Patent Information

Application Number
CN202411042026.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-19
Estimated Expiration
2044-07-31

AI Technical Summary

Technical Problem

After thermal bending, the existing curved photosensitive glass has insufficient shielding performance for visible and near-infrared light in the exposure area, and cannot fully meet the requirements of mobile phone covers and smart watches.

Method used

By adjusting the oxide composition, especially controlling the content range of CeO2, Sb2O3 and Ag2O, the exposure area of ​​the curved photosensitive glass has good shielding performance, and a uniform black effect is formed through radiation treatment and heat treatment, while ensuring the high level of the non-exposed area Light transmittance.

Benefits of technology

It realizes effective shielding performance of curved light-sensitive glass in visible and infrared wavelength ranges, meets the needs of mobile phone covers and smart watches, and maintains good light transmission in non-exposed areas.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118978333A_ABST
    Figure CN118978333A_ABST
Patent Text Reader

Abstract

The invention relates to curved-surface photosensitive glass and a preparation method and application thereof, the curved-surface photosensitive glass meets specific composition, and particularly, the content of CeO2, Sb2O3 and Ag2O is controlled to meet a specific range, so that an exposure area of the curved-surface photosensitive glass has better shielding performance, and the curved-surface photosensitive glass shows uniform black after hot bending treatment; meanwhile, the non-exposure area has good light transmission; and the requirements in the fields of mobile phone cover plates, smart watches and the like can be met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of glass technology, and in particular to a curved photosensitive glass and a preparation method and use thereof. Background Art

[0002] After ultraviolet exposure and heat treatment, the photosensitive glass can form a light-shielding opaque area in the exposed area. The light transmittance of this area is low, and it has light-shielding properties compared to the unexposed part of the glass. Therefore, the application of photosensitive glass in the fields of mobile phone covers, smart watch back covers, etc. can avoid signal crosstalk between test lights of different wavelengths. However, the current curved photosensitive glass, especially after heat bending treatment, still has the problem of insufficient shielding performance for visible light and near-infrared light in its exposed area; thus, the application of curved photosensitive glass in the fields of mobile phone covers, smart watches, etc. cannot fully meet the requirements. Summary of the invention

[0003] The purpose of the present application is to provide a curved photosensitive glass, the exposure area of ​​which has good shielding performance and can meet the requirements of mobile phone cover plates, smart watches and other fields.

[0004] In order to achieve the above objectives, this application provides the following technical solutions:

[0005] In a first aspect, a curved photosensitive glass is provided, which comprises an exposure area and a non-exposure area. The curved photosensitive glass comprises the following components, measured in mass percentage of oxides: SiO2: 65.00% to 75.00%, Al2O3: 5.00% to 10.00%, Li2O: 7.00% to 15.00%, Na2O: 1.00% to 4.00%, K2O: 1.00% to 4.00%, ZrO2: 5.00% to 8.00%, Ag2O: 0.15% to 0.80%, CeO2: 0.05% to 0.15% and Sb2O3: 0.1% to 0.50%.

[0006] As an optional embodiment, the curved photosensitive glass comprises the following components, measured in terms of mass percentage of oxides:

[0007] The content of SiO2 is 66.00% to 74.60%, preferably, the content of SiO2 is 66.50% to 74.00%; and / or,

[0008] The content of Al2O3 is 5.10% to 9.70%, preferably, the content of Al2O3 is 5.20% to 9.40%; and / or,

[0009] The content of Li2O is 7.10% to 14.50%, preferably, the content of Li2O is 8.00% to 14.50%; and / or,

[0010] The content of Na2O is 1.00% to 3.80%, preferably, the content of Na2O is 1.00% to 3.75%; and / or,

[0011] The content of K2O is 1.40% to 3.90%, preferably, the content of K2O is 1.40% to 3.85%; and / or, the content of ZrO2 is 5.00% to 7.50%, preferably, the content of ZrO2 is 5.10% to 7.50%; and / or,

[0012] The content of Ag2O is 0.15% to 0.60%, preferably, the content of Ag2O is 0.15% to 0.50%; and / or,

[0013] The content of CeO2 is 0.05% to 0.14%, preferably, the content of CeO2 is 0.07% to 0.14%; and / or,

[0014] The content of Sb2O3 is 0.20% to 0.50%, and preferably, the content of Sb2O3 is 0.20% to 0.48%.

[0015] As an optional implementation scheme, the curved photosensitive glass includes one or more of 3D photosensitive glass, 4D photosensitive glass, 5D photosensitive glass, special-shaped photosensitive glass, and four-curved photosensitive glass.

[0016] As an optional embodiment, the curved photosensitive glass is obtained by processing the substrate glass, wherein the processing includes radiation treatment and subsequent heat treatment and heat bending treatment.

[0017] As an optional embodiment, the composition of the substrate glass is the same as or substantially the same as the composition of the curved photosensitive glass.

[0018] As an optional implementation scheme, the thickness of the curved photosensitive glass is 0.3-2.0 mm, preferably 0.3-1.0 mm.

[0019] As an optional embodiment, when the thickness of the curved photosensitive glass is 0.30-1.00 mm, the transmittance T1 of the exposure area of ​​the curved photosensitive glass at a wavelength of 550 nm is 0.00%-5.00%, preferably 0.00%-3%; and / or,

[0020] When the thickness of the curved photosensitive glass is 0.30-1.00 mm, the transmittance T2 of the non-exposed area of ​​the curved photosensitive glass at a wavelength of 550 nm is above 90%; and / or,

[0021] When the thickness of the curved photosensitive glass is 0.30-1.00 mm, the transmittance T3 of the exposure area of ​​the curved photosensitive glass at a wavelength of 850 nm is 0.00%-8.00%, preferably 0.00%-5%; and / or,

[0022] When the thickness of the curved photosensitive glass is 0.30-1.00 mm, the transmittance T4 of the non-exposed area of ​​the curved photosensitive glass at a wavelength of 850 nm is above 90%; and / or,

[0023] When the thickness of the curved photosensitive glass is 0.30-1.00 mm, the transmittance T5 of the exposure area of ​​the curved photosensitive glass at a wavelength of 900 nm is 0.00%-10.00%, preferably 0.00%-8%; and / or,

[0024] When the thickness of the curved photosensitive glass is 0.30-1.00 mm, the transmittance T6 of the non-exposed area of ​​the curved photosensitive glass at a wavelength of 900 nm is above 90%.

[0025] As an optional embodiment, the crystalline phase of the exposure area of ​​the curved photosensitive glass includes one or more of lithium metasilicate, lithium disilicate, petalite, quartz, spodumene, eucryptite, zinc oxide, Ag nanocrystals, Cu nanocrystals, Au nanocrystals, and Bi nanocrystals.

[0026] As an optional embodiment, the non-exposed area of ​​the curved photosensitive glass is substantially free of a crystalline phase or includes one or more of lithium metasilicate, lithium disilicate, petalite, quartz, spodumene, eucryptite, zinc oxide, Ag nanocrystals, Cu nanocrystals, Au nanocrystals, and Bi nanocrystals.

[0027] As an optional implementation, the crystal phases of the exposed area and the non-exposed area of ​​the curved photosensitive glass are the same.

[0028] In a second aspect, a method for preparing the above-mentioned curved photosensitive glass is provided, the method comprising:

[0029] obtaining substrate glass;

[0030] The substrate glass comprises a first region and a second region, the first region is subjected to masking treatment, and the second region is not subjected to masking treatment, so as to obtain a masked substrate glass;

[0031] After processing the masked substrate glass, a curved photosensitive glass with a non-exposed area and an exposed area is obtained; wherein the non-exposed area corresponds to the first area, and the exposed area corresponds to the second area; the processing includes radiation treatment and subsequent heat treatment and heat bending treatment.

[0032] As an optional embodiment, the composition of the substrate glass is the same as or substantially the same as the composition of the curved photosensitive glass.

[0033] As an optional implementation, the thickness of the substrate glass is 0.3 to 2.0 mm, preferably 0.3 to 1.0 mm.

[0034] As an optional embodiment, the radiation treatment comprises ultraviolet irradiation treatment.

[0035] As an optional embodiment, the wavelength of the ultraviolet irradiation treatment is 300nm-320nm, and the intensity of the ultraviolet irradiation treatment is 20mw / cm 2 -360mw / cm 2 The UV irradiation treatment time is 5min-60min.

[0036] As an optional embodiment, the masking process includes masking using a masking ink and / or a mask plate.

[0037] As an optional embodiment, the heat treatment includes a nucleation treatment and a crystallization treatment.

[0038] As an optional embodiment, the heating rate of the nucleation treatment is 1°C / min-10°C / min; and / or,

[0039] The temperature of the nucleation treatment is 430°C-500°C; and / or,

[0040] The time of the nucleation treatment is 30 minutes to 360 minutes; and / or,

[0041] The heating rate of the crystallization treatment is 1°C / min-10°C / min; and / or,

[0042] The temperature of the crystallization treatment is higher than the temperature of the nucleation treatment, and the temperature of the crystallization treatment is 500° C.-800° C.; and / or,

[0043] The crystallization treatment time is 30min-480min.

[0044] In a third aspect, a strengthened curved photosensitive glass is provided, the thickness of which is t, comprising a strengthening layer, the strengthening layer extending from the surface of the curved photosensitive glass body toward the inside, the thickness of the strengthening layer being 0 to 0.22t, the strengthening layer comprising the following components, in terms of the mass percentage of oxides: SiO2: 65.00% to 75.00%, Al2O3: 5.00% to 10.00%, Na2O: 5.00% to 20.00%, K2O: 2.00% to 6.00%, ZrO2: 5.00% to 8.00%, Ag2O: 0.15% to 0.80%, CeO2: 0.05% to 0.15% and Sb2O3: 0.1% to 0.50%; the content of Li2O is lower than the content of Li2O at the center;

[0045] The center of the strengthened curved photosensitive glass comprises the following components, in terms of oxide mass percentage: SiO2: 65.00% to 75.00%, Al2O3: 5.00% to 10.00%, Li2O: 7.00% to 15.00%, Na2O: 1.00% to 4.00%, K2O: 1.00% to 4.00%, ZrO2: 5.00% to 8.00%, Ag2O: 0.15% to 0.80%, CeO2: 0.05% to 0.15% and Sb2O3: 0.1% to 0.50%;

[0046] The strengthened curved photosensitive glass comprises a non-exposed area and an exposed area.

[0047] As an optional embodiment, the chemical strengthening includes single-step chemical strengthening or multi-step chemical strengthening.

[0048] As an optional embodiment, the single-step chemical strengthening uses a salt bath containing NaNO3; preferably, the content of NaNO3 is 30-100wt%; preferably, the single-step chemical strengthening uses a mixed salt bath containing NaNO3 and KNO3, preferably, the content of KNO3 in the mixed salt bath is 80-100wt%, and the content of NaNO3 is 0-20wt%.

[0049] As an optional embodiment, the temperature of the single-step chemical strengthening is 380-480° C., and preferably, the ion exchange time of the single-step chemical strengthening is 1-10 h.

[0050] As an optional embodiment, the multi-step chemical strengthening includes two steps of chemical strengthening, wherein the first step of chemical strengthening uses a salt bath containing NaNO3, preferably the content of NaNO3 is 30-100wt%; the second step of chemical strengthening uses a salt bath containing KNO3, preferably the content of KNO3 is 60-100wt%.

[0051] As an optional embodiment, the temperature of the first step chemical strengthening is 380-480°C, and the time of the first step chemical strengthening is preferably 1-10h; preferably, the temperature of the second step chemical strengthening is 380-480°C, and the time of the second step chemical strengthening is preferably 5-120min.

[0052] As an optional implementation, the surface CS of the non-exposed area of ​​the strengthened curved photosensitive glass is above 300 MPa, preferably above 350 MPa, and more preferably 350 MPa to 600 MPa.

[0053] As an optional implementation scheme, the single-bar static pressure strength of the strengthened curved photosensitive glass is above 100N, preferably 100N to 400N, and more preferably 200N to 400N.

[0054] In a fourth aspect, a cover glass is provided, wherein the cover glass is a curved photosensitive glass prepared by the method for preparing the curved photosensitive glass as described in any embodiment of the first aspect or the curved photosensitive glass as described in any embodiment of the second aspect, or a strengthened curved photosensitive glass as described in any embodiment of the third aspect.

[0055] In a fifth aspect, an electronic device is provided, comprising the curved photosensitive glass as described in any embodiment of the first aspect, or the curved photosensitive glass prepared by the method for preparing the curved photosensitive glass as described in any embodiment of the second aspect, or the strengthened curved photosensitive glass as described in any embodiment of the third aspect.

[0056] As an optional embodiment, the electronic device includes a smart wearable device worn on the body, which includes a shell having a top and a bottom, the bottom being designed to contact the user's skin when worn, and the shell of the bottom includes the curved photosensitive glass as described in any embodiment of the first aspect, or the curved photosensitive glass prepared by the method for preparing the curved photosensitive glass as described in any embodiment of the second aspect, or the strengthened curved photosensitive glass as described in any embodiment of the third aspect.

[0057] As an optional embodiment, the electronic device also includes a camera assembly located inside the shell, the shell includes a camera protection cover, the camera protection cover is covered on the camera assembly, the camera protection cover includes the curved photosensitive glass as described in any embodiment of the first aspect, or the curved photosensitive glass prepared by the method for preparing the curved photosensitive glass as described in any embodiment of the second aspect, or the strengthened curved photosensitive glass as described in any embodiment of the third aspect.

[0058] In a sixth aspect, there is provided a use of the curved photosensitive glass or the curved photosensitive glass prepared by the method for preparing the curved photosensitive glass or the tempered photosensitive glass in components for mobile phones, wearable devices, camera modules or vehicles.

[0059] One or more of the above technical solutions provided by the present application have the following advantages compared with the prior art:

[0060] The present application makes the curved photosensitive glass meet a specific composition, especially controls the contents of CeO2, Sb2O3 and Ag2O to meet a specific range, so that the exposure area of ​​the curved photosensitive glass has good shielding performance, and displays a uniform black color after hot bending treatment, and at the same time its non-exposure area has good light transmittance; it can meet the requirements of mobile phone cover plates, smart watches and other fields. BRIEF DESCRIPTION OF THE DRAWINGS

[0061] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present application and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without paying creative work.

[0062] Figure 1 A schematic diagram of the structure of a substrate glass after being masked with masking ink provided in an embodiment of the present application.

[0063] Figure 2 A schematic diagram of the structure of the photosensitive glass provided in an embodiment of the present application.

[0064] Figure 3 A morphological photograph of the photosensitive glass provided for the embodiment of the present application, wherein a is the morphology at a first viewing angle, and b is the morphology at a second viewing angle.

[0065] Figure 4 A schematic diagram of the rear structure of an electronic device provided in an embodiment of the present application.

[0066] Figure 5 A schematic diagram of the structure of a smart watch provided in an embodiment of the present application.

[0067] Figure 6 This is a comparison chart of the transmittance curves of the substrate glass provided in Example 4 and Comparative Example 2 of the present application in the range of 240nm-360nm.

[0068] Figure numerals: 11 - light-transmitting area; 12 - light-shielding area; 21 - exposure area; 22 - non-exposure area; 31 - camera protection cover; 32 - camera assembly; 33 - back cover; 41 - back cover of the smart watch. DETAILED DESCRIPTION

[0069] The embodiments of the present application will be described in detail below in conjunction with the examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present application and should not be considered as limiting the scope of the present application. In the examples, if specific conditions are not specified, they are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0070] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise range or value, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article. Among them, the terms "optional" and "optional" all refer to including or not including (or may have or may not have). "And / or" as referred to herein is inclusive, for example, "A and / or B" means only A, or only B, or both A and B.

[0071] Explanation of terms and test methods:

[0072] In the present application, the main surface refers to the surface with the largest surface area, such as the upper surface or lower surface of a horizontally placed photosensitive glass sheet.

[0073] In the present application, the infrared wavelength range refers to 750nm to 1000nm.

[0074] In this application, the thickness of the glass is measured by a micrometer.

[0075] In this application, the size specifications of the glass sheets are tested using a two-dimensional measuring machine (instrument model: MiyuMY-YXCL-4030).

[0076] The surface CS was tested using FSM-6000 from Orihara, Japan. Test conditions: light source wavelength 596nm, SOC = 28.6 (nm / cm) / MPa, refractive index = 1.52. The surface compressive stress of the glass tested in this application is the CS of the non-exposed area. The exposed area cannot be tested because the light wave cannot penetrate the glass.

[0077] In this application, the crystal phase and crystal content of the glass are confirmed by XRD test as follows:

[0078] (1) XRD test: The photosensitive glass of the present application was crushed and ground into a sample with a particle size of less than 75 μm, and the ground sample was tested using an X-ray diffractometer to obtain an XRD diffraction peak curve and XRD diffraction data. The X-ray diffractometer used in the present application is Shimadzu XRD-6100, the target material is copper, 2θ=10°-50°, the scanning speed is 6° / min, the operating voltage is 40 kV, and the operating current is 30 mA.

[0079] (2) Determination of crystalline phase: XRD diffraction data were analyzed using Jade software (JADE Standard 8.6) to determine the crystalline phase in the sample.

[0080] (3) Determination of crystal content (also known as crystallinity): The XRD test results (RAW format) are imported into the X-ray diffraction data Rietveld refinement software Jade for fitting and calculation to determine the crystallinity of the sample. Specifically, the ratio of the fitted crystal phase peak area to the fitted total peak area is recorded as the crystal content of the sample. This application tests the crystal content at different positions of the same piece of glass and takes the average crystal content.

[0081] In the present application, an ultraviolet-visible spectrophotometer is used to test the transmittance of the exposed area and the non-exposed area of ​​the glass to be tested. The ultraviolet-visible spectrophotometer used in the test of the present application is Shimadzu UV-2000 ultraviolet-visible spectrophotometer.

[0082] The specific method for testing the exposure area of ​​the glass to be tested is: first use a fixture that is consistent with the shape and size of the glass to be tested, and the same area corresponding to the exposure area of ​​the glass to be tested is a hollow area and the non-exposure area corresponding to the glass to be tested is an opaque area, and the connection position between the hollow area and the opaque area is an opaque fixture as a blank sample for test calibration, and then cut the exposure area of ​​the glass to be tested into samples that coincide with the shape of the hollow area of ​​the fixture and put them into the hollow area of ​​the aforementioned fixture for testing to obtain the transmittance. Use an ultraviolet-visible spectrophotometer to test the transmittance of the exposure area of ​​5 pieces of glass to be tested in the same batch to light of different wavelengths, and then take the average value, which is recorded as the transmittance result of the exposure area of ​​the glass to be tested under the wavelength of light.

[0083] In addition, the transmittance of the non-exposed area of ​​5 pieces of tested glass in the same batch to light of different wavelengths was tested using an ultraviolet-visible spectrophotometer. The average value of the transmittance of the non-exposed area of ​​the 5 pieces of tested glass under light of different wavelengths was taken and recorded as the transmittance result of the non-exposed area of ​​the tested glass under the light of the wavelength.

[0084] In this application, the test of single-rod static pressure strength can be: place the glass sample to be tested on the bottom ring of the tensile testing machine (LT-850A), start the test software, and set the moving speed of the extrusion rod (rod diameter 8mm, pressure head arc radius 10mm) to 50mm / min, click to start the test, the extrusion rod will apply force to the center of the glass sample to be tested at the set moving speed until the glass sample cracks and breaks. The test software will automatically read the force (N) when the glass sample breaks as the test result. Take 10 glass samples in the same state for testing, and take the average value of the test results as the single-rod static pressure strength of the glass sample to be tested.

[0085] In some embodiments of the present application, a curved photosensitive glass is provided, which includes an exposure area and a non-exposure area, and the curved photosensitive glass includes the following components, measured by mass percentage of oxides: SiO2: 65.00% to 75.00%, Al2O3: 5.00% to 10.00%, Li2O: 7.00% to 15.00%, Na2O: 1.00% to 4.00%, K2O: 1.00% to 4.00%, ZrO2: 5.00% to 8.00%, Ag2O: 0.15% to 0.80%, CeO2: 0.05% to 0.15% and Sb2O3: 0.1% to 0.50%;

[0086] In the present application, SiO2 is a glass-forming oxide, which forms an irregular continuous network with the structural unit of silicon-oxygen tetrahedron, and is the skeleton of the glass. In some embodiments of the present application, the content of SiO2 in the curved photosensitive glass is 65.00% to 75.00%, preferably 66.00% to 74.60%, and more preferably 66.50% to 74.00%, in terms of the mass percentage of the oxide.

[0087] In some embodiments of the present application, in terms of the mass percentage of oxide, the content of SiO2 in the curved photosensitive glass can be 65.00%, 66.00%, 67.00%, 68.00%, 69.00%, 70.00%, 71.00%, 72.00%, 73.00%, 74.00%, 75.00%, 67.20%, 74.60%, 68.26%, 70.28%, 70.01%, 69.05% or 65.30%, or a value within a numerical range consisting of any two of the above specific values ​​as endpoints. It should be understood that in the embodiments, any of the above ranges can be combined with any other ranges.

[0088] In this application, Al2O3 is a glass network intermediate, and enters the glass network structure as [AlO4] tetrahedron. The increase of Al2O3 can improve the T gTemperature, thermal stability is enhanced, and it is beneficial to inhibit the phase separation during the heat treatment of glass, but too much will increase the melting temperature of the glass. In some embodiments of the present application, the content of Al2O3 in the curved photosensitive glass is 5.00% to 10.00%, preferably 5.10% to 9.70%, and more preferably 5.20% to 9.40%, calculated by mass percentage of oxides.

[0089] In some embodiments of the present application, in terms of the mass percentage of oxide, the content of Al2O3 in the curved photosensitive glass can be 5.00%, 5.50%, 6.00%, 6.50%, 7.00%, 7.50%, 8.00%, 8.50%, 9.00%, 9.50%, 10.00%, 7.25%, 5.83%, 8.76%, 7.62%, 7.89%, 6.47% or 8.96%, or a value within a numerical range consisting of any two of the above specific values ​​as endpoints. It should be understood that in the embodiments, any of the above ranges can be combined with any other ranges.

[0090] In some embodiments of the present application, the content of Li2O in the curved photosensitive glass is 7.00% to 15.00%, preferably 7.10% to 14.50%, and more preferably 8.00% to 14.50%, calculated as a percentage by mass of the oxide.

[0091] In some embodiments of the present application, in terms of the mass percentage of oxide, the content of Li2O in the curved photosensitive glass can be 7.00%, 7.50%, 8.00%, 8.50%, 9.00%, 9.50%, 10.00%, 10.50%, 11.00%, 11.50%, 12.00%, 12.50%, 13.00%, 13.50%, 14.00%, 14.50%, 15.00%, 12.30%, 8.02%, 12.26%, 9.81%, 9.48%, 11.05% or 14.37%, or a value within the numerical range formed by any two of the above specific values ​​as endpoints. It should be understood that in the embodiment, any of the above ranges can be combined with any other ranges.

[0092] In some embodiments of the present application, the content of Na2O in the curved photosensitive glass is 1.00% to 4.00%, preferably 1.00% to 3.80%, and more preferably 1.00% to 3.75%, calculated as a percentage by mass of the oxide. In some embodiments of the present application, the content of Na2O in the curved photosensitive glass can be 1.00%, 1.10%, 1.20%, 1.30%, 1.40%, 1.50%, 1.60%, 1.70%, 1.80%, 1.90%, 2.00%, 2.10%, 2.20%, 2.30%, 2.40%, 2.50%, 2.60%, 2.70%, calculated as a percentage by mass of the oxide. %, 2.80%, 2.90%, 3.00%, 3.10%, 3.20%, 3.30%, 3.40%, 3.50%, 3.60%, 3.70%, 3.80%, 3.90%, 4.00%, 3.22%, 3.71%, 2.08%, 2.42%, 2.40%, 2.50% or 1.02%, or a value within a numerical range consisting of any two of the above specific values ​​as endpoints. It should be understood that, in embodiments, any of the above ranges can be combined with any other ranges.

[0093] In some embodiments of the present application, the content of K2O in the curved photosensitive glass is 1.00% to 4.00%, preferably 1.40% to 3.90%, and more preferably 1.40% to 3.85%, calculated as a percentage by mass of the oxide. In some embodiments of the present application, the content of K2O in the curved photosensitive glass is 1.00%, 1.10%, 1.20%, 1.30%, 1.40%, 1.50%, 1.60%, 1.70%, 1.80%, 1.90%, 2.00%, 2.10%, 2.20%, 2.30%, 2.40%, 2.50%, 2.60%, 2.70%, 2.80%, 2.90%, 3.0 ... %, 3.50%, 3.60%, 3.70%, 3.80%, 3.90%, 4.00%, 3.83%, 1.42%, 3.02%, 3.41%, 3.52%, 2.58% or 2.87%, or a numerical value within a numerical range consisting of any two of the above specific numerical values ​​as endpoints. It should be understood that, in embodiments, any of the above ranges can be combined with any other ranges.

[0094] In some embodiments of the present application, the content of ZrO2 in the curved photosensitive glass is 5.00% to 8.00%, preferably 5.00% to 7.50%, and more preferably 5.10% to 7.50%. In some embodiments of the present application, the content of ZrO2 in the curved photosensitive glass is 5.00%, 5.10%, 5.20%, 5.30%, 5.40%, 5.50%, 5.60%, 5.70%, 5.80%, 5.90%, 6.00%, 6.10%, 6.20%, 6.30%, 6.40%, 6.50%, 6.60%, 6.70%, %, 6.80%, 6.90%, 7.00%, 7.10%, 7.20%, 7.30%, 7.40%, 7.50%, 7.60%, 7.70%, 7.80%, 7.90%, 8.00%, 5.56%, 5.72%, 5.12%, 5.58%, 5.63%, 7.50% or 6.98%, or a value within a numerical range consisting of any two of the above specific values ​​as endpoints. It should be understood that, in embodiments, any of the above ranges can be combined with any other ranges.

[0095] In some embodiments of the present application, the content of Ag2O in the curved photosensitive glass is 0.15% to 0.80%, preferably 0.15% to 0.60%, and more preferably 0.15% to 0.50%, calculated as a percentage by mass of the oxide. In some embodiments of the present application, in terms of the mass percentage of oxide, the content of Ag2O in the curved photosensitive glass can be 0.15%, 0.20%, 0.22%, 0.24%, 0.26%, 0.28%, 0.30%, 0.32%, 0.34%, 0.36%, 0.38%, 0.40%, 0.42%, 0.44%, 0.46%, 0.48%, 0.50%, 0.23%, 0.27%, 0.15%, 0.36%, 0.45%, 0.31%, 0.21%, 0.60%, 0.70% or 0.80%, or a value within the numerical range formed by any two of the above specific values ​​as endpoints. It should be understood that in the embodiments, any of the above ranges can be combined with any other ranges.

[0096] In this application, CeO2 is a photosensitizer and Ag + Provide electrons. When the CeO2 content is less than 0.05%, it cannot provide enough electrons to reduce Ag. + Silver atom Ag 0, reducing the light shielding performance of the exposure area; when the CeO2 content is higher than 0.15%, the penetration depth of ultraviolet light in the exposure area of ​​the glass is reduced, resulting in reduced light shielding performance of the exposure area. In some embodiments of the present application, the mass percentage of CeO2 in the curved photosensitive glass is 0.05% to 0.15%, preferably 0.05% to 0.14%, and more preferably 0.07% to 0.14%, calculated as the mass percentage of oxide.

[0097] In some embodiments of the present application, the content of CeO2 in the curved photosensitive glass can be 0.05%, 0.06%, 0.07%, 0.08%, 0.09%, 0.10%, 0.11%, 0.12%, 0.13%, 0.14% or 0.15%, or a value within a numerical range consisting of any two of the above specific values ​​as endpoints, in terms of the mass percentage of the oxide. It should be understood that in the embodiments, any of the above ranges can be combined with any other ranges.

[0098] In this application, Sb2O3 is a weak reducing agent and also acts as a clarifier. 3+ During the glass melting process, Ce 4+ Oxidation-reduction reaction occurs to maintain Ce 3+ In some embodiments of the present application, in terms of the mass percentage of oxides, the mass percentage of Sb2O3 in the curved photosensitive glass is 0.05% to 0.15%, preferably 0.05% to 0.14%, and more preferably 0.07% to 0.14%.

[0099] In some embodiments of the present application, the content of Sb2O3 in the curved photosensitive glass can be 0.05%, 0.06%, 0.07%, 0.08%, 0.09%, 0.10%, 0.11%, 0.12%, 0.13%, 0.14% or 0.15%, etc., or a value within a numerical range consisting of any two of the above specific values ​​as endpoints. It should be understood that in the embodiments, any of the above ranges can be combined with any other ranges.

[0100] In some embodiments of the present application, the curved photosensitive glass includes one or more of 3D photosensitive glass, 4D photosensitive glass, 5D photosensitive glass, special-shaped photosensitive glass, and four-curved photosensitive glass.

[0101] The curved photosensitive glass is obtained by processing the substrate glass, and the processing includes radiation treatment and subsequent heat treatment and hot bending treatment. In some embodiments of the present application, the temperature of the hot bending treatment is preferably 560°C to 630°C. In some embodiments of the present application, the temperature of the hot bending treatment can be 560°C, 570°C, 580°C, 590°C, 600°C, 610°C, 620°C or 630°C, or a value within the numerical range formed by any two of the above specific values ​​as endpoints. It should be understood that in the implementation scheme, any of the above ranges can be combined with any other ranges.

[0102] In some embodiments of the present application, the composition of the substrate glass is the same or substantially the same as the composition of the curved photosensitive glass, as specifically described above.

[0103] In some embodiments of the present application, the thickness of the curved photosensitive glass and / or photosensitive glass described in the present application is not particularly limited, for example, it can be 0.3 to 2.0 mm; preferably 0.3 to 1.0 mm. In some embodiments of the present application, the thickness of the curved photosensitive glass and / or photosensitive glass described in the present application can be 0.3 mm, 0.4 mm, 0.5 mm, 0.6 mm, 0.7 mm, 0.8 mm, 0.9 mm, 1.0 mm, 1.1 mm, 1.2 mm, 1.3 mm, 1.4 mm, 1.5 mm or 2.0 mm, or a value within the numerical range formed by any two of the above specific values ​​as endpoints. It should be understood that in the embodiments, any of the above ranges can be combined with any other ranges.

[0104] In some embodiments of the present application, the exposure area has a low transmittance in the visible light and infrared wavelength range, and the non-exposure area has a high transmittance in the visible light and infrared wavelength range. The curved photosensitive glass that meets this transmittance can ensure that the non-exposure area has good light transmittance and a good transparent effect, while the exposure area has a lower light transmittance and a better shielding effect, and is suitable for use in cover glass that needs to shield the light source. The "infrared wavelength range" here refers to light with a wavelength of 750nm to 1000nm.

[0105] In some embodiments of the present application, when the thickness of the curved photosensitive glass is 0.30-1.00 mm, the transmittance T1 of the exposure area of ​​the curved photosensitive glass at a wavelength of 550 nm is 0.00%-5.00%, preferably 0.00%-3%.

[0106] In some embodiments of the present application, when the thickness of the curved photosensitive glass is 0.30-1.00 mm, the transmittance T1 of the exposure area of ​​the curved photosensitive glass at a wavelength of 550 nm may be 0%, 1.00%, 2.00%, 3.00%, 4.00% or 5.00%, or a value within a numerical range consisting of any two of the above specific values ​​as endpoints. It should be understood that, in the embodiments, any of the above ranges may be combined with any other ranges.

[0107] In some embodiments of the present application, when the thickness of the curved photosensitive glass is 0.30-1.00 mm, the transmittance T2 of the non-exposed area of ​​the curved photosensitive glass at a wavelength of 550 nm is above 90%. In some embodiments of the present application, when the thickness of the curved photosensitive glass is 0.30-1.00 mm, the transmittance T2 of the non-exposed area of ​​the curved photosensitive glass at a wavelength of 550 nm can be 90.00%, 90.10%, 90.50%, 91.20%, 92.00%, 93.50%, 94.00%, 94.80% or 95.00%, or a value within the numerical range formed by any two of the above specific values ​​as endpoints. It should be understood that in the embodiments, any of the above ranges can be combined with any other ranges.

[0108] In some embodiments of the present application, when the thickness of the curved photosensitive glass is 0.30-1.00 mm, the transmittance T3 of the exposure area of ​​the curved photosensitive glass at a wavelength of 850 nm is 0.00%-10.00%, preferably 0.00%-8%.

[0109] In some embodiments of the present application, when the thickness of the curved photosensitive glass is 0.30-1.00 mm, the transmittance T3 of the exposure area of ​​the curved photosensitive glass at a wavelength of 850 nm may be 0%, 1.00%, 2.00%, 3.00%, 4.00%, 5.00%, 6.00%, 7.00%, 8.00%, 9.00% or 10.00%, or a value within a numerical range consisting of any two of the above specific values ​​as endpoints. It should be understood that, in the embodiments, any of the above ranges may be combined with any other ranges.

[0110] In some embodiments of the present application, when the thickness of the curved photosensitive glass is 0.30-1.00 mm, the transmittance T4 of the non-exposed area of ​​the curved photosensitive glass at a wavelength of 850 nm is above 90%. In some embodiments of the present application, when the thickness of the curved photosensitive glass is 0.30-1.00 mm, the transmittance T4 of the non-exposed area of ​​the curved photosensitive glass at a wavelength of 850 nm can be 90.00%, 90.10%, 90.50%, 91.20%, 92.00%, 93.50%, 94.00%, 94.80% or 95.00%, or a value within the numerical range formed by any two of the above specific values ​​as endpoints. It should be understood that in the embodiment, any of the above ranges can be combined with any other ranges.

[0111] In some embodiments of the present application, when the thickness of the curved photosensitive glass is 0.30-1.00 mm, the transmittance T5 of the exposure area of ​​the curved photosensitive glass at a wavelength of 900 nm is 0.00%-10.00%, and preferably the transmittance T3 is 0.00%-8%.

[0112] In some embodiments of the present application, when the thickness of the curved photosensitive glass is 0.30-1.00 mm, the transmittance T5 of the exposure area of ​​the curved photosensitive glass at a wavelength of 900 nm may be 0%, 1.00%, 2.00%, 3.00%, 4.00%, 5.00%, 6.00%, 7.00%, 8.00%, 9.00% or 10.00%, or a value within a numerical range consisting of any two of the above specific values ​​as endpoints. It should be understood that, in the embodiments, any of the above ranges may be combined with any other ranges.

[0113] In some embodiments of the present application, when the thickness of the curved photosensitive glass is 0.30-1.00 mm, the transmittance T6 of the non-exposed area of ​​the curved photosensitive glass at a wavelength of 900 nm is above 90%. In some embodiments of the present application, when the thickness of the curved photosensitive glass is 0.30-1.00 mm, the transmittance T6 of the non-exposed area of ​​the curved photosensitive glass at a wavelength of 900 nm can be 90.00%, 90.10%, 90.50%, 91.20%, 92.00%, 93.50%, 94.00%, 94.80% or 95.00%, or a value within the numerical range formed by any two of the above specific values ​​as endpoints. It should be understood that in the embodiments, any of the above ranges can be combined with any other ranges.

[0114] In some embodiments of the present application, the crystalline phase of the exposure area of ​​the curved photosensitive glass includes one or more of lithium metasilicate, lithium disilicate, petalite, quartz, spodumene, eucryptite, zinc oxide, Ag nanocrystals, Cu nanocrystals, Au nanocrystals, and Bi nanocrystals.

[0115] In some embodiments of the present application, the non-exposed area of ​​the curved photosensitive glass is substantially free of a crystalline phase or includes one or more of lithium metasilicate, lithium disilicate, petalite, quartz, spodumene, eucryptite, zinc oxide, Ag nanocrystals, Cu nanocrystals, Au nanocrystals, and Bi nanocrystals.

[0116] In some embodiments of the present application, the crystal phases of the exposed area and the non-exposed area of ​​the curved photosensitive glass are the same.

[0117] In some embodiments of the present application, a method for preparing the above-mentioned curved photosensitive glass is provided, which comprises:

[0118] obtaining substrate glass;

[0119] The substrate glass comprises a first region and a second region, the first region is subjected to masking treatment, and the second region is not subjected to masking treatment, so as to obtain a masked substrate glass;

[0120] After processing the masked substrate glass, a curved photosensitive glass having a non-exposed area and an exposed area is obtained; wherein the non-exposed area corresponds to the first area, and the exposed area corresponds to the second area; the processing includes radiation treatment and subsequent heat treatment and heat bending treatment.

[0121] In some embodiments of the present application, the composition of the substrate glass of the present application is the same or substantially the same as the composition of the curved photosensitive glass; the specific composition is as described above.

[0122] In the present application, the substrate glass can be prepared by a molding method in the prior art, and the present application has no limitation on this. For example, the molding method of the substrate glass can include but is not limited to float, overflow, rolling or casting processes. For example, the substrate glass can be obtained by uniformly mixing the components according to the formula, melting and molding, cooling and annealing.

[0123] Exemplarily, each raw material is configured according to the formula ratio, a clarifier is added, and then mixed for a period of time to obtain a uniform raw material mixture. The raw material mixture is placed in a platinum crucible, heated to 1250°C to 1680°C, preferably the melting temperature is 1480°C to 1680°C, and preferably kept warm for 3 to 12 hours under this temperature condition, and then poured into a molding mold for cooling and molding, preferably cooled to 750°C to 1000°C, and then placed in an annealing furnace for annealing treatment, preferably the annealing temperature is 400°C to 650°C, and the annealing time is preferably 10 to 48 hours; then cooled to room temperature with the furnace, the substrate glass can be obtained. Those skilled in the art can select the type and amount of clarifier according to needs, and they do not need to pay creative labor. Further, the clarifier may include but is not limited to one or more of sodium chloride, tin oxide, antimony oxide or arsenic oxide, and the amount of clarifier added may be 0wt%-1wt% of the total amount of each raw material.

[0124] In some embodiments of the present application, the thickness of the substrate glass described in the present application is not particularly limited, for example, it can be 0.3 to 2.0 mm; preferably 0.3 to 1.0 mm. In some embodiments of the present application, the thickness of the substrate glass described in the present application can be 0.3 mm, 0.4 mm, 0.5 mm, 0.6 mm, 0.7 mm, 0.8 mm, 0.9 mm, 1.0 mm, 1.1 mm, 1.2 mm, 1.3 mm, 1.4 mm, 1.5 mm or 2.0 mm, or a value within the numerical range formed by any two of the above specific values ​​as endpoints. It should be understood that in the embodiments, any of the above ranges can be combined with any other ranges.

[0125] In some embodiments of the present application, the masking process includes masking using masking ink and / or a mask plate.

[0126] For example, the schematic diagram of the structure of the substrate glass after masking with masking ink is as follows: Figure 1 The composite circular hole has a light-transmitting area 11 of the inner diameter and a light-shielding area 12 outside the inner diameter; the structural schematic diagram of the corresponding photosensitive glass is as shown in Figure 2 The position corresponding to the light-transmitting area 11 forms an exposure area 21, and the position corresponding to the light-shielding area 12 forms a non-exposure area 22.

[0127] In some embodiments of the present application, the radiation treatment method includes ultraviolet irradiation treatment, wherein the wavelength of the ultraviolet irradiation treatment is 300nm to 320nm, and the intensity of the ultraviolet irradiation treatment is 20mw / cm 2 ~360mw / cm 2 The UV irradiation treatment time is 5min-60min.

[0128] In some embodiments of the present application, the wavelength of the ultraviolet irradiation treatment is 300nm, 302nm, 305nm, 308nm, 310nm, 312nm, 315nm, 317nm or 320nm, or a value within a numerical range consisting of any two of the above specific values ​​as endpoints. In some embodiments of the present application, the intensity of the ultraviolet irradiation treatment is 20mw / cm 2 、40mw / cm 2 、60mw / cm 2 、80mw / cm 2 、100mw / cm 2 、120mw / cm 2 、140mw / cm 2 、160mw / cm 2 、180mw / cm 2 、200mw / cm 2 、210mw / cm 2 、220mw / cm 2 、230mw / cm 2 、240mw / cm 2 、250mw / cm 2 、260mw / cm 2 、270mw / cm 2 、280mw / cm 2 、290mw / cm 2 、300mw / cm 2 、310mw / cm 2 、320mw / cm 2 、330mw / cm 2 、340mw / cm 2 、350mw / cm 2 or 360mw / cm 2 , or a value within the numerical range formed by any two of the above specific values ​​as endpoints. In some embodiments of the present application, the time of ultraviolet irradiation treatment is 5min, 10min, 15min, 20min, 25min, 30min, 35min, 40min, 45min, 50min, 55min or 60min, or a value within the numerical range formed by any two of the above specific values ​​as endpoints; as long as the photosensitive glass with the required performance of the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the photosensitive glass with the required performance of the present application can be obtained.

[0129] In some embodiments of the present application, the heat treatment includes a nucleation treatment and a crystallization treatment, which are common processes in the art.

[0130] In some embodiments of the present application, the heating rate of the nucleation treatment is 1°C / min-10°C / min. In some embodiments of the present application, the time of the nucleation treatment can be 1°C / min, 2°C / min, 3°C / min, 4°C / min, 5°C / min, 6°C / min, 7°C / min, 8°C / min, 9°C / min or 10°C / min, or a value within the numerical range consisting of any two of the above specific values ​​as endpoints. In some embodiments of the present application, the temperature of the nucleation treatment can be 430°C-500°C. In some embodiments of the present application, the temperature of the nucleation treatment can be 430°C, 440°C, 450°C, 460°C, 470°C, 480°C, 490°C or 500°C, or a value within the numerical range consisting of any two of the above specific values ​​as endpoints. In some embodiments of the present application, the time of the nucleation treatment is 30min-360min. In some embodiments of the present application, the time of the nucleation treatment can be 30 min, 45 min, 50 min, 55 min, 60 min, 90 min, 100 min, 120 min, 140 min, 150 min, 160 min, 170 min, 180 min, 190 min, 200 min, 220 min, 240 min, 280 min, 300 min, 320 min, 340 min or 360 min, or a value within the numerical range formed by any two of the above specific values ​​as endpoints.

[0131] In the present application, the crystallization treatment includes a one-step crystallization treatment and a multi-step crystallization treatment. In some embodiments of the present application, the heating rate of the crystallization treatment is 1°C / min-10°C / min. In some embodiments of the present application, the time of the crystallization treatment can be 1°C / min, 2°C / min, 3°C / min, 4°C / min, 5°C / min, 6°C / min, 7°C / min, 8°C / min, 9°C / min or 10°C / min, or a value within the numerical range consisting of any two of the above specific values ​​as endpoints.

[0132] In some embodiments of the present application, the temperature of the one-step crystallization treatment may be 500°C-800°C. In some embodiments of the present application, the temperature of the one-step crystallization treatment may be 500°C, 510°C, 520°C, 530°C, 540°C, 550°C, 560°C, 570°C, 580°C, 600°C, 650°C, 700°C, 750°C or 800°C, or a value within the numerical range consisting of any two of the above specific values ​​as endpoints. In some embodiments of the present application, the time of the one-step crystallization treatment is 30min-480min. In some embodiments of the present application, the time for the crystallization treatment can be 30 min, 45 min, 50 min, 55 min, 60 min, 90 min, 100 min, 120 min, 140 min, 150 min, 160 min, 170 min, 180 min, 190 min, 200 min, 220 min, 240 min, 280 min, 300 min, 340 min, 380 min, 400 min, 430 min, 450 min or 480 min, or a value within the numerical range formed by any two of the above specific values ​​as endpoints.

[0133] In some embodiments of the present application, the multi-step crystallization process includes a two-step crystallization process. In some embodiments of the present application, the temperature of the first crystallization process in the two-step crystallization process is 500°C-560°C, and the temperature of the second crystallization process is 560°C-800°C. In some embodiments of the present application, the temperature of the first crystallization process in the two-step crystallization process may be 500°C, 510°C, 520°C, 530°C, 540°C, 550°C or 560°C, or a value within the numerical range consisting of any two of the above specific values ​​as endpoints. In some embodiments of the present application, the temperature of the second crystallization process in the two-step crystallization process may be 560°C, 570°C, 580°C, 600°C, 650°C, 700°C, 750°C or 800°C, or a value within the numerical range consisting of any two of the above specific values ​​as endpoints.

[0134] In some embodiments of the present application, the time of the first crystallization treatment in the two-step crystallization treatment is 30 min-240 min, and the time of the second crystallization treatment is 30 min-240 min. In some embodiments of the present application, the time of the first crystallization treatment in the two-step crystallization treatment can be 30 min, 45 min, 50 min, 55 min, 60 min, 90 min, 100 min, 120 min, 140 min, 150 min, 160 min, 170 min, 180 min, 190 min, 200 min, 220 min or 240 min, or a value within the numerical range consisting of any two of the above specific values ​​as endpoints. In some embodiments of the present application, the time of the second crystallization treatment in the two-step crystallization treatment can be 30 min, 45 min, 50 min, 55 min, 60 min, 90 min, 100 min, 120 min, 140 min, 150 min, 160 min, 170 min, 180 min, 190 min, 200 min, 220 min or 240 min, or a value within the numerical range formed by any two of the above specific values ​​as endpoints.

[0135] Before and / or after the heat treatment, those skilled in the art may also perform other conventional steps to obtain a substrate glass or curved photosensitive glass sample that meets the required specifications or requirements, such as shaping, cutting (such as cutting with a multi-wire cutting machine), CNC machining (computer numerical control, i.e., CNC machine tools), thinning, or polishing. In the present application, there is no limitation on the size of the substrate glass or curved photosensitive glass sample, such as 50 mm×50 mm×0.7 mm, 300 mm×120 mm×0.7 mm, etc.

[0136] In some embodiments of the present application, a strengthened curved photosensitive glass is provided, the thickness of which is t, and the strengthened layer includes a strengthening layer, the strengthening layer extends from the surface of the curved photosensitive glass body toward the inside, the thickness of the strengthening layer is 0 to 0.22t, and the strengthening layer, in terms of the mass percentage of oxides, includes the following components: SiO2: 65.00% to 75.00%, Al2O3: 5.00% to 10.00%, Na2O: 5.00% to 20.00%, K2O: 2.00% to 6.00%, ZrO2: 5.00% to 8.00%, Ag2O: 0.15% to 0.80%, CeO2: 0.05% to 0.15% and Sb2O3: 0.1% to 0.50%; the content of Li2O is lower than the content of Li2O at the center;

[0137] The center of the strengthened curved photosensitive glass comprises the following components, in terms of oxide mass percentage: SiO2: 65.00% to 75.00%, Al2O3: 5.00% to 10.00%, Li2O: 7.00% to 15.00%, Na2O: 1.00% to 4.00%, K2O: 1.00% to 4.00%, ZrO2: 5.00% to 8.00%, Ag2O: 0.15% to 0.80%, CeO2: 0.05% to 0.15% and Sb2O3: 0.1% to 0.50%;

[0138] The strengthened curved photosensitive glass comprises a non-exposed area and an exposed area.

[0139] In some embodiments of the present application, there is also provided a strengthened curved photosensitive glass having a thickness of t, which is obtained by chemically strengthening the curved photosensitive glass or the curved photosensitive glass prepared by the method for preparing the curved photosensitive glass.

[0140] In some embodiments of the present application, the strengthened curved photosensitive glass contains a strengthening layer, and the strengthening layer comprises the following components, measured by mass percentage of oxides: SiO2: 65.00% to 75.00%, Al2O3: 5.00% to 10.00%, Na2O: 5.00% to 20.00%, K2O: 2.00% to 6.00%, ZrO2: 5.00% to 8.00%, Ag2O: 0.15% to 0.80%, CeO2: 0.05% to 0.15% and Sb2O3: 0.1% to 0.50%; the content of Li2O is lower than the content of Li2O at the center;

[0141] In the present application, chemical strengthening can be performed by existing known methods; for example, chemical strengthening includes single-step chemical strengthening or multi-step chemical strengthening. In some embodiments of the present application, the single-step chemical strengthening uses a salt bath containing NaNO3; preferably, the content of NaNO3 is 30-100wt%; preferably, the single-step chemical strengthening uses a mixed salt bath containing NaNO3 and KNO3, preferably, the content of KNO3 in the mixed salt bath is 80-100wt%, and the content of NaNO3 is 0-20wt%.

[0142] In some embodiments of the present application, the temperature of the single-step chemical strengthening is 380-480° C., and preferably, the ion exchange time of the single-step chemical strengthening is 1-10 h.

[0143] In some embodiments of the present application, the multi-step chemical strengthening includes two steps of chemical strengthening, wherein the first step of chemical strengthening uses a salt bath containing NaNO3, preferably the content of NaNO3 is 30-100wt%; the second step of chemical strengthening uses a salt bath containing KNO3, preferably the content of KNO3 is 60-100wt%.

[0144] In some embodiments of the present application, the temperature of the first step chemical strengthening is 380-480°C, and the time of the first step chemical strengthening is preferably 1-10h; preferably, the temperature of the second step chemical strengthening is 380-480°C, and the time of the second step chemical strengthening is preferably 5-120min.

[0145] In some embodiments of the present application, the above-mentioned strengthened curved photosensitive glass includes one or more of strengthened 3D photosensitive glass, strengthened 4D photosensitive glass, strengthened 5D photosensitive glass, strengthened special-shaped photosensitive glass, and strengthened four-curved photosensitive glass.

[0146] In some embodiments of the present application, the thickness t of the tempered glass is not particularly limited, for example, it can be 0.3 to 2.0 mm; preferably 0.3 to 1.0 mm. In some embodiments of the present application, the thickness of the tempered glass can be 0.3 mm, 0.4 mm, 0.5 mm, 0.6 mm, 0.7 mm, 0.8 mm, 0.9 mm, 1.0 mm, 1.1 mm, 1.2 mm, 1.3 mm, 1.4 mm, 1.5 mm or 2.0 mm, or a value within a numerical range consisting of any two of the above specific values ​​as endpoints. It should be understood that in the embodiments, any of the above ranges can be combined with any other ranges.

[0147] In some embodiments of the present application, the surface CS of the non-exposed area of ​​the above-mentioned strengthened curved photosensitive glass is above 300 MPa, preferably above 350 MPa, and more preferably 350 MPa to 600 MPa. In some embodiments of the present application, the surface CS of the non-exposed area of ​​the strengthened curved photosensitive glass can be 350 MPa, 351 MPa, 395 MPa, 438 MPa, 385 MPa, 391 MPa, 398 MPa, 402 MPa, 422 MPa, 450 MPa, 480 MPa, 500 MPa, 530 MPa, 550 MPa, 580 MPa or 600 MPa, or a value within the numerical range formed by any two of the above-mentioned specific values ​​as endpoints; as long as the photosensitive glass with the performance required by the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the photosensitive glass with the performance required by the present application can be obtained.

[0148] In some embodiments of the present application, the horizontal bar static pressure strength of the above-mentioned strengthened curved photosensitive glass is above 100N, preferably 100N to 400N, and more preferably 200N to 400N. In some embodiments of the present application, the horizontal bar static pressure strength of the strengthened curved photosensitive glass in the present application can be 294N, 361N, 392N, 301N, 314N, 375N, 376N, 390N or 400N, or a value within the numerical range formed by any two of the above-mentioned specific values ​​as endpoints; as long as the photosensitive glass with the performance required by the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the photosensitive glass with the performance required by the present application can be obtained.

[0149] The curved photosensitive glass and / or strengthened curved photosensitive glass with excellent performance provided in the present application can be used in electronic devices, including but not limited to mobile phones, tablet computers, handheld game consoles, portable digital devices (such as digital cameras), smart homes, smart wearables (such as smart bracelets, smart watches, smart glasses), and can also be used in vehicles, aircraft or aircraft, and can also be used in any glass device with required curved photosensitive glass. For example, it can be used in the back cover glass of mobile phones, the shell glass of smart watches, etc.; for example, it can be used in the windshield of vehicles, aircraft or aircraft, such as the front windshield or side windshield.

[0150] For example, the curved photosensitive glass and / or strengthened curved photosensitive glass with excellent performance provided by the present application can be used to manufacture cover glass, and the cover glass can be a back cover or camera protection cover of an electronic device such as a mobile phone. For example, the curved photosensitive glass and / or strengthened curved photosensitive glass with excellent performance provided by the present application can be used in electronic devices. In some embodiments of the present application, an electronic device is provided, which can be a mobile phone (such as Figure 4 As shown, the curved photosensitive glass and / or the strengthened curved photosensitive glass can be used as the back cover of a mobile phone), a tablet computer, a smart wearable device (such as Figure 5 As shown, the curved photosensitive glass and / or the strengthened curved photosensitive glass can be used as the bottom shell of electronic products such as smart watches.

[0151] In some embodiments of the present application, the electronic device includes a smart wearable device worn on the body, which includes a shell having a top and a bottom, the bottom being designed to contact the user's skin when worn, and the shell of the bottom includes the curved photosensitive glass and / or tempered curved photosensitive glass mentioned above in the present application.

[0152] In some embodiments of the present application, Figure 4As shown, the electronic device also includes a camera assembly 32 located inside the housing, and the housing may include a camera protection cover 31, which is covered on the camera assembly 32 to protect the camera assembly 32, and the camera protection cover 31 uses the aforementioned curved photosensitive glass and / or strengthened curved photosensitive glass. In some embodiments of the present application, the camera protection cover 31 may partially use the aforementioned curved photosensitive glass and / or strengthened curved photosensitive glass, or may use the aforementioned curved photosensitive glass and / or strengthened curved photosensitive glass in its entirety. In some embodiments of the present application, the setting position of the camera protection cover 31 is determined according to the setting position of the camera assembly 32, and may be located on the front side of the electronic device or on the rear side of the electronic device. In some embodiments of the present application, the camera protection cover 31 may be a separate structure from the back cover 33. In other embodiments of the present application, the camera protection cover 31 may also be an integrated structure with the back cover 33.

[0153] The technical solution of the present application is further described in detail below in conjunction with the embodiments. The embodiments of the present application described in detail below are exemplary and are only used to explain the present application, and cannot be understood as limiting the present application.

[0154] Example 1

[0155] (1) The raw materials were prepared according to the proportions of the components in Table 1. The total mass of the prepared raw materials was 2000 g. 10 g of clarifier sodium chloride (NaCl) was added to the prepared raw materials, and then mixed in a V-type mixer for 30 minutes to obtain a uniform raw material mixture.

[0156] The mixed raw materials are transferred to a platinum crucible at 1450℃ in small amounts and multiple times, with a time interval of 40 minutes between each addition. After all the raw materials are added, the temperature is raised to 1500℃ and stirred and clarified with a platinum stirring rod for a total of 10 hours, and then pulled into shape and continuously drawn into glass bricks of the required specifications. The glass bricks are placed in an annealing furnace at 450℃ for 12 hours, and then naturally cooled to room temperature to obtain the base glass sample bricks.

[0157] The obtained substrate glass bricks are cut, CNC processed (the CNC equipment model used in this application is: RCG500S), and polished in turn to obtain substrate glass that meets the required specifications and requirements. The size of the substrate glass is 50mm×50mm×0.7mm.

[0158] (2) The glass substrate is ultrasonically cleaned in deionized water, anhydrous ethanol, propanol and deionized water for 10 minutes, and then dried in a drying oven; a masking ink is applied to local areas of the upper and lower main surfaces of the photosensitive substrate glass after cleaning, such as Figure 1As shown, the black area is the masked area; then the double-sided irradiation treatment was carried out under parallel ultraviolet light with a wavelength of 310nm (UVHX800*850 drawer type) for a total of 20 minutes, and the irradiation light energy density was 200mw / cm 2 ; The UV irradiated glass is heat treated according to the heat treatment process in Table 1 to obtain photosensitive glass; the heat treatment includes nucleation treatment and crystallization treatment; the heating rate of nucleation treatment and crystallization treatment is 10℃ / min; the above photosensitive glass is subjected to cold processing such as laser cutting, splitting, polishing, chamfering, etc. in sequence to obtain a size of Photosensitive glass, such as Figure 2 shown.

[0159] (3) The above-mentioned photosensitive glass is subjected to heat bending treatment to obtain 3D photosensitive glass, which contains an exposure area and a non-exposure area. The glass shape is as follows Figure 3 shown.

[0160] The hot bending process includes 4 preheating stations, 3 hot pressing stations and 3 cooling stations; the specific hot bending process is shown in Table 2 below.

[0161] The crystal phase and transmittance of the exposed area of ​​the 3D photosensitive glass were tested (transmittance T1 at a wavelength of 550nm, transmittance T3 at a wavelength of 850nm, and transmittance T5 at a wavelength of 900nm), and the crystal phase and transmittance of the non-exposed area of ​​the 3D photosensitive glass were tested (transmittance T2 at a wavelength of 550nm, transmittance T4 at a wavelength of 850nm, and transmittance T6 at a wavelength of 900nm). The results are shown in Table 3.

[0162] (4) The 3D photosensitive glass obtained in (3) is subjected to a chemical strengthening treatment, wherein the chemical strengthening treatment is performed by chemically strengthening in a 100wt% NaNO3 salt bath at 450°C for 3h and chemically strengthening in a 100wt% KNO3 salt bath at 430°C for 15min to obtain a strengthened 3D photosensitive glass.

[0163] The surface CS and horizontal bar static pressure strength of the non-exposed area of ​​the strengthened 3D photosensitive glass were tested, and the results are shown in Table 4.

[0164] Embodiment 2 to Embodiment 7

[0165] The above methods are respectively carried out with reference to Example 1, except that the raw material composition, process parameters and corresponding test results of each example are shown in Tables 1 to 4, respectively.

[0166] Comparative Example 1 to Comparative Example 3

[0167] The above methods are respectively carried out with reference to Example 1, except that the raw material composition, process parameters and corresponding test results of each example are shown in Tables 1 to 4, respectively.

[0168] Table 1

[0169]

[0170]

[0171] Table 2

[0172]

[0173] Table 3

[0174]

[0175]

[0176] Table 4

[0177] Example 1 Example 2 Example 3 Example 4 Example 5 Example 6 Example 7 Non-exposure area CS / Mpa 351 395 438 385 391 398 402 Horizontal bar static pressure strength / N 294 361 392 301 314 375 376

[0178] It can be seen from the above table that the 3D photosensitive glass prepared by the embodiment of the present application has good shielding performance in the exposed area, especially good shading performance in the infrared wavelength range, and shows a beautiful black appearance; at the same time, its non-exposed area has good light transmittance in the visible light and infrared wavelength ranges, and can meet the requirements of fields such as mobile phone cover plates and back covers 41 of smart watches.

[0179] By comparing the data of Example 4 of the present application with that of Comparative Example 1, it can be seen that when the hot bending process is process 1, the 3D photosensitive glass of Comparative Example 1 is not within the scope of the present application due to the low content of Sb2O3, and the glass cannot produce enough Ce. 3+ , and thus cannot convert enough Ag into + Reduced to silver atoms Ag 0 , resulting in the shading effect of the exposed area not meeting the requirements and having a brown appearance.

[0180] By comparing Example 4 of the present application with Comparative Example 1, it can be seen that when the hot bending treatment process is Process 2, the 3D photosensitive glass of Comparative Example 1 cannot meet the requirements for the shading effect in the exposed area after hot bending, phase separation occurs in the non-exposed area, the transmittance is significantly reduced, and the light transmission performance requirements are not met.

[0181] By comparing Example 4 of the present application with Comparative Example 2, it can be seen that when the 3D photosensitive glass of Comparative Example 2 has an excessive CeO2 content, the penetration depth of ultraviolet light in the exposure area of ​​the glass is reduced. Figure 6 As shown, there is not enough Ce 3+ The UV excitation will be enough Ag + Reduced to silver atoms Ag 0 , which results in the shading effect of the exposure area not meeting the requirements.

[0182] By comparing Example 4 of the present application with Comparative Example 3, it can be seen that the 3D photosensitive glass of Comparative Example 3 cannot reduce enough silver atoms Ag due to the low content of Ag2O. 0 , which results in the shading effect of the exposure area not meeting the requirements.

[0183] The above description is only a specific embodiment of the present application and is not intended to limit the present application. For those skilled in the art, the present application may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application shall be included in the protection scope of the present application.

Claims

1. A curved photosensitive glass, It is characterized in that It includes an exposure area and a non-exposure area. The curved photosensitive glass comprises the following components in terms of oxide mass percentage: SiO 2 :65.00%~75.00%、Al 2 O 3 :5.00%~10.00%, Li 2 O: 7.00% to 15.00%, Na 2 O: 1.00% to 4.00%, K 2 O: 1.00% to 4.00%, ZrO 2 :5.00%~8.00%, Ag 2 O: 0.15% to 0.80%, CeO 2 :0.05%~0.15% and Sb 2 O 3 :0.1%~0.50%.

2. The curved photosensitive glass according to claim 1, It is characterized in that The curved photosensitive glass comprises the following components in terms of mass percentage of oxides: SiO 2 The content of SiO is 66.00% to 74.60%, preferably, SiO 2 The content of is 66.50% to 74.00%; and / or, Al 2 O 3 The content of Al is 5.10% to 9.70%, preferably, Al 2 O 3 The content of is 5.20% to 9.40%; and / or, Li 2 The content of O is 7.10% to 14.50%, preferably, Li 2 The content of O is 8.00% to 14.50%; and / or, Na 2 The content of O is 1.00% to 3.80%, preferably, Na 2 The content of O is 1.00% to 3.75%; and / or, K 2 The content of O is 1.40% to 3.90%, preferably, K 2 The content of O is 1.40% to 3.85%; and / or, ZrO 2 The content of ZrO is 5.00% to 7.50%, preferably, ZrO 2 The content of is 5.10% to 7.50%; and / or, Ag 2 The content of O is 0.15% to 0.60%, preferably Ag 2 The content of O is 0.15% to 0.50%; and / or, CeO 2 The content of CeO is 0.05% to 0.14%, preferably CeO 2 The content of is 0.07% to 0.14%; and / or, Sb 2 O 3 The content of Sb is 0.20% to 0.50%, preferably, Sb 2 O 3 The content is 0.20%~0.48%.

3. The curved photosensitive glass according to claim 1 or 2, It is characterized in that The curved photosensitive glass includes one or more of 3D photosensitive glass, 4D photosensitive glass, 5D photosensitive glass, special-shaped photosensitive glass, and four-curved photosensitive glass.

4. The curved photosensitive glass according to any one of claims 1 to 3, It is characterized in that The curved photosensitive glass is obtained by processing the substrate glass, wherein the processing includes radiation treatment and subsequent heat treatment and heat bending treatment.

5. The curved photosensitive glass according to claim 4, It is characterized in that The composition of the substrate glass is the same or substantially the same as that of the curved photosensitive glass.

6. The curved photosensitive glass according to any one of claims 1 to 5, It is characterized in that The thickness of the curved photosensitive glass is 0.3-2.0 mm, preferably 0.3-1.0 mm.

7. The curved photosensitive glass according to any one of claims 1 to 6, It is characterized in that When the thickness of the curved photosensitive glass is 0.30-1.00 mm, the transmittance T of the exposure area of ​​the curved photosensitive glass at a wavelength of 550 nm is 1 0.00%-5.00%, preferably the transmittance T 1 0.00%-3%; and / or, When the thickness of the curved photosensitive glass is 0.30-1.00 mm, the transmittance T of the non-exposed area of ​​the curved photosensitive glass at a wavelength of 550 nm is 2 is 90% or more; and / or, When the thickness of the curved photosensitive glass is 0.30-1.00 mm, the transmittance T of the exposure area of ​​the curved photosensitive glass at a wavelength of 850 nm is 3 0.00%-8.00%, preferably the transmittance T 3 0.00%-5%; and / or, When the thickness of the curved photosensitive glass is 0.30-1.00 mm, the transmittance T of the non-exposed area of ​​the curved photosensitive glass at a wavelength of 850 nm is 4 is 90% or more; and / or, When the thickness of the curved photosensitive glass is 0.30-1.00 mm, the transmittance T of the exposure area of ​​the curved photosensitive glass at a wavelength of 900 nm is 5 0.00%-10.00%, preferably the transmittance T 5 0.00%-8%; and / or, When the thickness of the curved photosensitive glass is 0.30-1.00 mm, the transmittance T of the non-exposed area of ​​the curved photosensitive glass at a wavelength of 900 nm is 6 More than 90%.

8. The curved photosensitive glass according to any one of claims 1 to 7, It is characterized in that The crystalline phase of the exposure area of ​​the curved photosensitive glass includes one or more of lithium metasilicate, lithium disilicate, petalite, quartz, spodumene, eucryptite, zinc oxide, Ag nanocrystals, Cu nanocrystals, Au nanocrystals, and Bi nanocrystals.

9. The curved photosensitive glass according to claim 8, It is characterized in that The non-exposed area of ​​the curved photosensitive glass is substantially free of a crystalline phase or comprises one or more of lithium metasilicate, lithium disilicate, petalite, quartz, spodumene, eucryptite, zinc oxide, Ag nanocrystals, Cu nanocrystals, Au nanocrystals, and Bi nanocrystals.

10. The curved photosensitive glass according to claim 9, It is characterized in that The crystal phase of the exposed area and the non-exposed area of ​​the curved photosensitive glass is the same.

11. A method for preparing the curved photosensitive glass according to any one of claims 1 to 10, It is characterized in that It includes: obtaining substrate glass; The substrate glass comprises a first region and a second region, the first region is subjected to masking treatment, and the second region is not subjected to masking treatment, so as to obtain a masked substrate glass; After processing the masked substrate glass, a curved photosensitive glass with a non-exposed area and an exposed area is obtained; wherein the non-exposed area corresponds to the first area, and the exposed area corresponds to the second area; the processing includes radiation treatment and subsequent heat treatment and heat bending treatment.

12. The method for preparing the curved photosensitive glass according to claim 11, It is characterized in that The composition of the substrate glass is the same as or substantially the same as that of the curved photosensitive glass.

13. The method for preparing the curved photosensitive glass according to claim 11 or 12, It is characterized in that The thickness of the substrate glass is 0.3 to 2.0 mm, preferably 0.3 to 1.0 mm.

14. A method for preparing a curved photosensitive glass according to any one of claims 11 to 13, It is characterized in that Masking includes masking using masking inks and / or masking sheets.

15. A method for preparing a curved photosensitive glass according to any one of claims 11 to 14, It is characterized in that The heat treatment includes a nucleation treatment and a crystallization treatment.

16. The method for preparing the curved photosensitive glass according to claim 15, It is characterized in that The heating rate of the nucleation treatment is 1°C / min-10°C / min; and / or, The temperature of the nucleation treatment is 430°C-500°C; and / or, The time of the nucleation treatment is 30 min to 360 min; and / or, The heating rate of the crystallization treatment is 1°C / min-10°C / min; and / or, The temperature of the crystallization treatment is higher than the temperature of the nucleation treatment, and the temperature of the crystallization treatment is 500° C.-800° C.; and / or, The crystallization treatment time is 30min-480min.

17. A reinforced curved photosensitive glass, It is characterized in that The thickness is t, and it includes a strengthening layer, the strengthening layer extends from the surface of the curved photosensitive glass body toward the inside, and the thickness of the strengthening layer is 0 to 0.22t, The center of the strengthened curved photosensitive glass comprises the following components in terms of oxide mass percentage: SiO 2 :65.00%~75.00%、Al 2 O 3 :5.00%~10.00%, Li 2 O: 7.00% to 15.00%, Na 2 O: 1.00% to 4.00%, K 2 O: 1.00% to 4.00%, ZrO 2 :5.00%~8.00%, Ag 2 O: 0.15% to 0.80%, CeO 2 :0.05%~0.15% and Sb 2 O 3 : 0.1%~0.50%; The strengthening layer comprises the following components in terms of oxide mass percentage: SiO 2 :65.00%~75.00%、Al 2 O 3 :5.00%~10.00%,Na 2 O: 5.00% to 20.00%, K 2 O: 2.00% to 6.00%, ZrO 2 :5.00%~8.00%, Ag 2 O: 0.15% to 0.80%, CeO 2 :0.05%~0.15% and Sb 2 O 3 :0.1%~0.50%;The Li in the strengthening layer 2 The content of O is lower than that of Li in the center. 2 O content; The strengthened curved photosensitive glass comprises a non-exposed area and an exposed area.

18. The tempered curved photosensitive glass according to claim 17, It is characterized in that The surface CS of the non-exposed region of the tempered curved photosensitive glass is greater than 300 MPa, preferably greater than 350 MPa, and more preferably 350 MPa to 600 MPa.

19. The tempered curved photosensitive glass according to claim 17 or 18, It is characterized in that The single bar static pressure strength of the tempered curved photosensitive glass is above 100N, preferably 100N to 400N, and more preferably 200N to 400N.

20. A cover glass, It is characterized in that The cover glass is made of the curved photosensitive glass according to any one of claims 1 to 10, the curved photosensitive glass prepared by the preparation method according to any one of claims 11 to 16, or the strengthened curved photosensitive glass according to any one of claims 17 to 19.

21. An electronic device, It is characterized in that The electronic device comprises the curved photosensitive glass according to any one of claims 1 to 10, the curved photosensitive glass prepared by the preparation method according to any one of claims 11 to 16, or the strengthened curved photosensitive glass according to any one of claims 17 to 19.

22. The electronic device according to claim 21, It is characterized in that The electronic device comprises a shell having a top and a bottom, wherein the shell at the bottom comprises the curved photosensitive glass according to any one of claims 1 to 10, the curved photosensitive glass prepared by the preparation method according to any one of claims 11 to 16, or the strengthened curved photosensitive glass according to any one of claims 17 to 19.

23. The electronic device according to claim 21, It is characterized in that The electronic device also includes a camera assembly, and the housing of the electronic device includes a camera protection cover, which is disposed on the camera assembly, and the camera protection cover is made of the curved photosensitive glass described in any one of claims 1-10, the curved photosensitive glass prepared by the preparation method described in any one of claims 11-16, or the strengthened curved photosensitive glass described in any one of claims 17-19.

24. Use of the curved photosensitive glass according to any one of claims 1 to 10, or the curved photosensitive glass prepared by the preparation method according to any one of claims 11 to 16, or the strengthened curved photosensitive glass according to any one of claims 17 to 19 in components for mobile phones, wearable devices, camera modules or vehicles.

Citation Information

Patent Citations

  • Method for preparing photosensitive glass-ceramics mobile phone shell

    CN106830678A

  • Lighting unit with laminate structure

    CN109689585A

  • Glass ceramic, glass ceramic product and manufacturing method thereof

    CN113754286A

  • Glass ceramic and glass ceramic product

    CN118388139A

Cited By

  • Photosensitive microcrystalline glass, preparation method thereof and chemically strengthened photosensitive microcrystalline glass

    CN122212483A

  • Photosensitive glass-ceramics and method for preparing the same, chemically strengthened photosensitive glass-ceramics

    CN122212483B

  • Photosensitive glass, preparation method thereof, reinforced photosensitive glass and application

    CN122380651A

  • A photosensitive glass, its preparation method, a strengthened photosensitive glass, and its applications.

    CN122380651B

  • Photosensitive glass, preparation method thereof, reinforced photosensitive glass and application

    CN122464609A