Alkali-resistant and metal ion-resistant bimetallic catalyst and preparation method thereof
By using carboxyl-containing polymers in the bimetallic cyanide complex catalyst to coordinate reaction with zinc salt and cobalt salt, an alkali-resistant and metal ions-resistant bimetallic catalyst was prepared, which solved the basic environment of existing catalysts. and the problem of inactivation under high metal ions achieves efficient catalytic and industrial production under wide range of conditions.
Patent Information
- Application Number
- CN202411130565.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-08-16
AI Technical Summary
Existing bimetallic cyanide complex catalysts are prone to deactivate under alkaline environments and high metal ion concentrations, and are difficult to use stably in industrial production.
A polymer containing a large amount of carboxyl group is used to coordinate reaction with zinc salt and cobalt salt to prepare a bimetallic catalyst that is resistant to alkali and metal ions. By washing and post-treatment in a weak acid environment, a highly efficient catalytic capability is obtained. catalyst.
The catalyst maintains activity in an environment with alkaline pH ≤9 and metal ions ≤20ppm, simplifies the production process of polyether polyols, reduces production costs, and realizes the feasibility of industrial production.
Smart Images

Figure BDA0004997695660000021 
Figure BDA0004997695660000051 
Figure BDA0004997695660000052
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of catalyst synthesis and specifically relates to a bimetallic catalyst and a preparation method thereof. Background Art
[0002] Polyether polyols are the main raw materials for synthesizing polyurethane materials. They are now widely used in the synthesis of various polymer materials such as foam plastics, elastomers, coatings, fibers, adhesives, synthetic leather, etc. They have important uses in various fields such as transportation, construction, electronic equipment, furniture, textiles and clothing, printing, petrochemicals, and medical treatment.
[0003] Since the General Tire & Rubber Company of the United States first discovered the use of double metal cyanide complex (DMC) as a catalyst for the preparation of long-chain polyether polyols in the 1960s, propylene oxide polyether polyols prepared by DMC catalysts have the advantages of low unsaturation (0.005-0.008 mol / kg) and narrow distribution (Mw / Mn<1.2). Their quality is significantly better than general industrial polyethers (KOH catalyzed), and the catalytic efficiency of DMC catalysts is much higher than other catalytic systems. Since then, this technology has attracted widespread attention.
[0004] At present, most of the bimetallic cyanide complex catalysts on the market use zinc and cobalt as the main structure, and coordinate with a variety of small molecules or polymers with oxygen atoms to obtain the final catalyst. This type of catalyst has the advantages of high activity and generally does not require post-treatment. However, the activity of the catalyst is easily affected by environmental factors, such as system pH, metal ion content, etc. When the system pH is greater than 7 or the metal ion (potassium, sodium) content is greater than 5ppm, the catalyst will be partially or completely deactivated. Patent CN 111072948A discloses a method for preparing a bimetallic catalyst. The catalyst prepared in this patent can be used under weak alkaline conditions, and the alkalinity in the initiator is only 0.01mgKOH / g (potassium ion content 7ppm, pH 7.5).
[0005] Therefore, it is very necessary to develop an efficient bimetallic catalyst that is resistant to alkaline environment and metal ions. Summary of the invention
[0006] In view of the problems existing in the prior art, the purpose of the present invention is to provide a bimetallic catalyst resistant to alkalinity and metal ions and a preparation method thereof. The bimetallic catalyst prepared by the present invention has the characteristics of being resistant to alkalinity and metal ions, and can be used for the synthesis of polyether polyols in an alkaline environment with a metal ion content of up to 20 ppm. Moreover, the preparation process of the bimetallic catalyst of the present invention is simple, the raw materials are easily available, and industrial production can be realized.
[0007] To achieve its purpose, the present invention adopts the following technical solutions:
[0008] A method for preparing a bimetallic catalyst comprises the following steps:
[0009] 1) mixing the ligand polymer and the alcohol compound to obtain a bimetallic catalyst ligand;
[0010] 2) slowly dropping the zinc salt aqueous solution and the potassium hexacyanocobaltate aqueous solution into the bimetallic catalyst ligand in step 1) to react, and obtaining a solid precipitate as a crude bimetallic catalyst;
[0011] 3) The crude bimetallic catalyst is washed with a weak acid aqueous solution, filtered to remove water, and then post-processed to obtain the bimetallic catalyst.
[0012] According to the preparation method of the present invention, in step 1), the ligand polymer structure is:
[0013]
[0014] Among them, a:b=10:1-20:1, 30≤m+n≤50, m:n=1:1-1:10.
[0015] According to the preparation method of the present invention, in step 1), the alcohol compound is isopropanol, tert-butanol, propylene glycol, ethylene glycol, preferably isopropanol, and its amount is 5-10 times the mass of the ligand polymer.
[0016] According to the preparation method of the present invention, in step 2), the zinc salt includes one or more of zinc sulfate, zinc chloride, zinc acetate, and zinc nitrate, preferably zinc chloride, and its concentration ranges from 10 to 30 wt%.
[0017] According to the preparation method of the present invention, in step 2), the concentration of the potassium hexacyanocobaltate aqueous solution is in the range of 10-30 wt %.
[0018] According to the preparation method of the present invention, in step 2), the mass ratio of the zinc salt aqueous solution to the bimetallic catalyst ligand is 1:10-1:40, preferably 1:20-1:30.
[0019] According to the preparation method of the present invention, in step 2), the mass ratio of the potassium hexacyanocobaltate aqueous solution to the zinc salt aqueous solution is 1:3-1:10, preferably 1:5-1:8.
[0020] According to the preparation method of the present invention, in step 2), the reaction temperature is 20-40° C., and the reaction time is 1 h to 5 h, preferably the reaction temperature is 25-35° C., and the reaction time is 2 h to 4 h.
[0021] According to the preparation method of the present invention, in step 3), the weak acid is one or more of lactic acid, acetic acid, and formic acid, preferably acetic acid; the pH of the weak acid aqueous solution is 5-6.8, preferably 5.5-6.5.
[0022] According to the preparation method of the present invention, in step 3), the post-treatment includes drying and grinding, wherein the drying temperature is 40-60° C. and the drying time is 8 h to 24 h.
[0023] According to the preparation method of the present invention, the ligand polymer is prepared by the following steps:
[0024] S1: dissolving methacrylic acid and methallyl alcohol polyether in desalted water to prepare a monomer aqueous solution;
[0025] S2: adding an initiator to the monomer aqueous solution to carry out a polymerization reaction;
[0026] S3: removing water from the reaction solution to obtain a ligand polymer.
[0027] According to the preparation method of the present invention, in step S1, the concentration of the monomer aqueous solution is 20-40wt%, preferably 30-35wt%.
[0028] According to the preparation method of the present invention, in step S1, the mass ratio of methacrylic acid to methallyl alcohol polyether is 1:0.8 to 1:5, preferably 1:1 to 1:3.
[0029] According to the preparation method of the present invention, in step S2, the initiator is one or more of potassium persulfate, sodium persulfate, and azobisisobutyramidine hydrochloride, preferably potassium persulfate.
[0030] According to the preparation method of the present invention, in step S2, the amount of the initiator added is 0.20 wt% to 0.24 wt% of the monomer aqueous solution.
[0031] According to the preparation method of the present invention, in step S2, the reaction temperature is 40-60° C. and the reaction time is 10-14 h.
[0032] According to the preparation method of the present invention, in step S3, the water in the reaction liquid is removed under a vacuum condition of -0.095-0.100 MPaG, preferably at 100-120°C.
[0033] Another object of the present invention is to provide a bimetallic catalyst, which is prepared by the above method, and the use environment of the bimetallic catalyst is: alkaline pH ≤ 9, metal ions ≤ 20 ppm.
[0034] Compared with the prior art, the beneficial effects of the present invention are mainly reflected in the following aspects:
[0035] A polymer containing a large number of carboxyl groups is used as a ligand polymer to carry out coordination reaction with zinc salt and cobalt salt to obtain an efficient bimetallic catalyst. When the bimetallic catalyst synthesized by the present invention is used to prepare polyether polyols, the catalyst can be used in an alkaline environment with a pH value less than 9 and an environment in which the metal ions are within 20 ppm. When the base catalytic system is switched to the bimetallic catalytic system, the alkali metal catalyst in the reactor needs to be cleaned, and the alkali metal ion content needs to be cleaned to less than 5 ppm to ensure the smooth activation of the bimetallic catalyst. The catalyst facilitates the switching of the base catalytic system to the bimetallic catalytic system, greatly simplifies the conditions for washing the reactor, and greatly reduces the switching cost of the polyether production system. The present invention has a simple process, readily available raw materials, and is easy to realize industrial production. DETAILED DESCRIPTION
[0036] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field belong to the scope of protection of the present invention.
[0037] Unless otherwise defined, all the professional terms used below have the same meanings as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.
[0038] Gel permeation chromatography test conditions: Waters 515 liquid chromatograph was used for testing, the chromatographic columns were HR-3, HR-4, and HR-6, the detector was a parallax detector Waters 2414, the mobile phase was tetrahydrofuran, the flow rate was 1 mL / min, the column temperature was 40°C, the sample concentration was 5 mg / mL, and narrow distribution polyethylene glycol was used as a sample.
[0039] Source of raw materials:
[0040] Unless otherwise specified, the reagents used in the examples can be purchased from reagent manufacturers, and the product purity is chemically pure.
[0041] The methyl allyl alcohol polyether used for preparing the ligand polymer can be prepared by conventional methods. The preparation method of the methyl allyl alcohol polyether of the present invention is described as follows.
[0042] Preparation Example 1: Preparation of methyl allyl alcohol polyether a
[0043]
[0044] Add 150.0g of methyl allyl alcohol and 10g of sodium metal to a 10L reactor, control the temperature at 40°C for 1h under stirring at 200rpm, raise the temperature to 110°C, control the flow rate to keep the pressure in the reactor less than 0.3MPaG, and continue to introduce 3020g of propylene oxide into the reactor at 110°C. After the feeding is completed, maintain the temperature at 110°C for 1.5h, control the flow rate to keep the pressure in the reactor less than 0.3MPaG, and continue to introduce propylene oxide into the reactor at 110°C. 2292g of ethylene oxide was added, and the reaction was maintained at 110°C for 1.5h after the feeding was completed. The vacuum degree was controlled to be -0.098MPaG and the temperature was 110°C to remove unreacted propylene oxide and ethylene oxide under reduced pressure. 50.2 phosphoric acid and 300g of water were added to the reaction solution for neutralization for 1h, and 3g of magnesium silicate adsorbent was added for adsorption for 1h. Dehydration was performed until the water content was less than 0.05wt%. Methyl allyl alcohol polyether a (hydroxyl value 21.4mgKOH / g, m=25, n=25) was obtained by filtration.
[0045] According to the same preparation method as in Preparation Example 1, methyl allyl alcohol polyether b of Preparation Example 2 and methyl allyl alcohol polyether c of Preparation Example 3 were obtained, wherein the reaction conditions were the same as in Preparation Example 1, except for the feed ratio. The feed amounts of methyl allyl alcohol polyether b and methyl allyl alcohol polyether c are shown in Table 1 below.
[0046] Table 1
[0047]
[0048] The structure of the prepared methyl allyl alcohol polyether b is m=5, n=25, and the hydroxyl value is 32.2 mgKOH / g; the structure of the methyl allyl alcohol polyether c is m=4, n=40, and the hydroxyl value is 21.8 mgKOH / g.
[0049] Example
[0050] Example 1 Preparation of bimetallic catalyst a
[0051] Synthesis of ligand polymer a: 86 g of methacrylic acid and 262 g of methyl allyl alcohol polyether a were dissolved in 1392 g of desalted water to prepare a 20 wt% monomer aqueous solution, 2.70 g of potassium persulfate was added to the monomer aqueous solution, the temperature was raised to 50° C. under stirring at 200 rpm, and the reaction was continued at 50° C. for 12 h, the vacuum degree was controlled to be -0.098 MPaG and the temperature was 100° C. to remove moisture from the reaction solution, the product was placed in a dialysis bag for dialysis purification, the vacuum degree was controlled to be -0.098 MPaG and the temperature was 100° C. to remove moisture from the purified product, and 335 g of ligand polymer a was obtained (the number average molecular weight tested by gel permeation chromatography was 34,000, and the PDI was 1.50; a:b=10:1, m=25, n=25).
[0052] 100g of ligand polymer a and 500g of isopropanol were stirred and mixed to obtain a bimetallic catalyst ligand; 15g of zinc chloride aqueous solution (30wt%) and 5g of potassium hexacyanocobaltate aqueous solution (30wt%) were simultaneously added dropwise to the bimetallic catalyst ligand under stirring conditions, and the addition took 1 hour to complete. After the addition was completed, stirring and reacting were continued for 1 hour. The temperature of this process was maintained at 20°C throughout the whole process. After the reaction was completed, a solid precipitate was filtered to obtain a crude bimetallic catalyst; the crude bimetallic catalyst was washed three times with 500mL of acetic acid aqueous solution with a pH of 5, filtered to remove water after washing, and then dried in a vacuum environment at 40°C for 24 hours, taken out and ground to obtain a bimetallic catalyst product a.
[0053] Example 2 Preparation of bimetallic catalyst b
[0054] Synthesis of ligand polymer b: 172g of methacrylic acid and 174g of methyl allyl alcohol polyether b were dissolved in 807g of desalted water to prepare a 30wt% monomer aqueous solution, 2.70g of potassium persulfate was added to the monomer aqueous solution, the temperature was raised to 50°C under stirring at 200rpm, and the reaction was continued at 50°C for 12h. The vacuum degree was controlled to be -0.098MPaG and the temperature was 100°C to remove moisture from the reaction solution. The product was placed in a dialysis bag for dialysis purification, and the vacuum degree was controlled to be -0.098MPaG and the temperature was 100°C to remove moisture from the purified product to obtain 328g of ligand polymer b (the number average molecular weight of the gel permeation chromatography test was 32000, and the PDI was 1.52; its a:b=20:1, m=5, n=25).
[0055] 100g of ligand polymer b and 1000g of propylene glycol were stirred and mixed to obtain a bimetallic catalyst ligand; 510g of zinc sulfate aqueous solution (10wt%) and 51g of potassium hexacyanocobaltate aqueous solution (10wt%) were simultaneously added dropwise to the bimetallic catalyst ligand under stirring conditions, and the addition took 1 hour to complete. After the addition was completed, stirring and reacting were continued for 5 hours. The temperature of this process was maintained at 40°C throughout the whole process. After the reaction was completed, a solid precipitate was filtered to obtain a crude bimetallic catalyst; the crude bimetallic catalyst was washed three times with 2000mL of lactic acid aqueous solution with a pH of 6.8, filtered to remove water after washing, and then dried in a vacuum environment at 60°C for 8 hours, taken out and ground to obtain a bimetallic catalyst product b.
[0056] Example 3 Preparation of bimetallic catalyst c
[0057] Synthesis of ligand polymer c: 129 g of methacrylic acid and 256 g of methyl allyl alcohol polyether c were dissolved in 578 g of desalted water to prepare a 40 wt% monomer aqueous solution, 2.70 g of potassium persulfate was added to the monomer aqueous solution, the temperature was raised to 50° C. under stirring at 200 rpm, and the reaction was continued at 50° C. for 12 h, the vacuum degree was controlled to be -0.098 MPaG and the temperature was 100° C. to remove moisture from the reaction solution, the product was placed in a dialysis bag for dialysis purification, the vacuum degree was controlled to be -0.098 MPaG and the temperature was controlled to be 100° C. to remove moisture from the purified product, and 371 g of ligand polymer c was obtained (the number average molecular weight tested by gel permeation chromatography was 37,000, and the PDI was 1.46; a:b=15:1, m=4, and n=40).
[0058] 100g of ligand polymer c and 700g of tert-butanol were stirred and mixed to obtain a bimetallic catalyst ligand; 32g of zinc nitrate aqueous solution (20wt%) and 5.3g of potassium hexacyanocobaltate aqueous solution (20wt%) were simultaneously added dropwise to the bimetallic catalyst ligand under stirring conditions, and the addition took 1 hour to complete. After the addition was completed, stirring and reacting were continued for 3 hours. The temperature of this process was maintained at 30°C throughout the whole process. After the reaction was completed, a solid precipitate was filtered to obtain a crude bimetallic catalyst; the crude bimetallic catalyst was washed three times with 1000mL of formic acid aqueous solution with a pH of 6, filtered to remove water after washing, and then dried in a vacuum environment at 50°C for 12 hours, taken out and ground to obtain a bimetallic catalyst product c.
[0059] Example 4 Synthesis of polyether polyols
[0060] 600 g of glycerol starting polyether polyol (potassium ion content 1 ppm, pH 5.5) with a molecular weight of 600 g / mol was used as an initiator and was mixed with 0.10 g of the bimetallic catalyst a in the above embodiment, the temperature was raised to 100° C., and the mixture was stirred until the materials were evenly dispersed. The temperature was maintained at 100° C. and the mixture was stirred and dehydrated for 2 h under a vacuum environment; the temperature was raised to 140° C., and 60 g of propylene oxide (10% by weight of the initiator) was added, and the pressure change was observed; when the pressure dropped to half of the initial pressure, the catalyst was considered to be activated; 2350 g of propylene oxide was continuously introduced into the reactor under the conditions of controlling the flow rate to keep the pressure in the reactor less than 0.3 MPaG and the temperature at 140° C., and the reaction was continued for 1.5 h after the feeding was completed, and the unreacted propylene oxide was removed under reduced pressure at a vacuum degree of -0.098 MPaG and a temperature of 140° C. to obtain 3000 g of a polyether polyol product.
[0061] Example 5 Synthesis of polyether polyols
[0062] The difference from Example 4 is that the bimetallic catalyst b in Example 2 is used, and the other conditions are the same.
[0063] Example 6 Synthesis of polyether polyols
[0064] The difference from Example 4 is that the bimetallic catalyst c in Example 3 is used, and the other conditions are the same.
[0065] Example 7 Synthesis of polyether polyols
[0066] 600g of glycerol starting polyether polyol (potassium ion content 20ppm, pH 8.5) with a molecular weight of 600g / mol was used as an initiator and was mixed with 0.10g of the bimetallic catalyst a in the above embodiment, the temperature was raised to 100°C, and the mixture was stirred until the materials were evenly dispersed. The temperature was maintained at 100°C, and the mixture was stirred and dehydrated for 2h under a vacuum environment; the temperature was raised to 140°C, and 60g of propylene oxide, which was 10% of the mass of the initiator, was added, and the pressure change was observed; when the pressure dropped to half of the initial pressure, the catalyst was considered to be activated; 2350g of propylene oxide was continuously introduced into the reactor under the conditions of controlling the flow rate to keep the pressure in the reactor less than 0.3MPaG and the temperature at 140°C. After the feeding was completed, the reaction was continued for 1.5h, and the vacuum degree was controlled to be -0.098MPaG and the temperature was 140°C to remove unreacted propylene oxide under reduced pressure to obtain 3000g of polyether polyol product.
[0067] Example 8 Synthesis of polyether polyols
[0068] The difference from Example 7 is that the bimetallic catalyst b in Example 2 is used, and the other conditions are the same.
[0069] Example 9 Synthesis of polyether polyols
[0070] The difference from Example 7 is that the bimetallic catalyst c in Example 3 is used, and the other conditions are the same.
[0071] Comparative Example 1
[0072] The difference between this comparative example and the above-mentioned Example 4 is that the bimetallic catalyst used in the preparation of the polyether polyol in this comparative example is a commercially available product of Huaian Bader Polyurethane Technology Co., Ltd., and the other conditions are the same.
[0073] Comparative Example 2
[0074] The difference between this comparative example and the above-mentioned Example 7 is that the bimetallic catalyst used in the preparation of the polyether polyol in this comparative example is a commercially available product of Huaian Bader Polyurethane Technology Co., Ltd., and the other conditions are the same.
[0075] Comparative Example 3
[0076] The difference between this comparative example and the above-mentioned Example 7 is that the bimetallic catalyst used in the preparation of the polyether polyol in this comparative example is the catalyst prepared by reference to patent CN 111072948 A, and the other conditions are the same.
[0077] The hydroxyl values of the polyether polyols prepared in Examples 4-9 and the polyether polyols prepared in Comparative Examples 1-3 were tested with reference to GB / T12008.3-2009 Plastic Polyether Polyols Part 3: Determination of Hydroxyl Value. The results are shown in Table 2.
[0078] Table 2 Test results
[0079]
[0080]
[0081] Note: The system pressure before feeding propylene oxide is the initial pressure, and the time it takes for the pressure to drop to half of the initial pressure after starting to feed propylene oxide is the activation time.
[0082] From the test results of Examples 4-6 and Comparative Example 1 in Table 2, it can be seen that the key indicators of the polyether polyol prepared by the bimetallic catalyst synthesized by the present invention and the bimetallic catalyst of Comparative Example 1 under the same conditions are basically the same in terms of hydroxyl value and PDI, but the activation time of the catalyst described in this patent is shorter than that of the catalyst in Comparative Example 1, and the catalytic ability of the catalyst is stronger. From the test results of Examples 7-9 and Comparative Examples 2 and 3, it can be seen that under the conditions of pH 8.5 and 20ppm of potassium ions, the bimetallic catalyst synthesized by the present invention still has good catalytic activity, while the catalysts of Comparative Examples 2 and 3 are not activated, indicating that the bimetallic catalyst synthesized by the present invention has excellent characteristics of resistance to alkalinity and metal ions.
Claims
1. A method for preparing a bimetallic catalyst, comprising the following steps: 1) mixing the ligand polymer and the alcohol compound to obtain a bimetallic catalyst ligand; 2) slowly dropping the zinc salt aqueous solution and the potassium hexacyanocobaltate aqueous solution into the bimetallic catalyst ligand in step 1) to react, and obtaining a solid precipitate as a crude bimetallic catalyst; 3) The crude bimetallic catalyst is washed with a weak acid aqueous solution, filtered to remove water, and then post-processed to obtain the bimetallic catalyst.
2. The preparation method according to claim 1, wherein In step 1), the ligand polymer structure is: Among them, a:b=10:1-20:1, 30≤m+n≤50, m:n=1:1-1:
10.
3. The preparation method according to claim 1 or 2, wherein In step 1), the alcohol compound is isopropanol, tert-butanol, propylene glycol, ethylene glycol, preferably isopropanol, and its amount is 5-10 times the mass of the ligand polymer.
4. The preparation method according to any one of claims 1 to 3, wherein In step 2), The zinc salt includes one or more of zinc sulfate, zinc chloride, zinc acetate, and zinc nitrate, preferably zinc chloride, and the concentration range is 10-30wt%; the concentration range of potassium hexacyanocobaltate aqueous solution is 10-30wt%; The mass ratio of the zinc salt aqueous solution to the bimetallic catalyst ligand is 1:10-1:40, preferably 1:20-1:30; the mass ratio of the potassium hexacyanocobaltate aqueous solution to the zinc salt aqueous solution is 1:3-1:10, preferably 1:5-1:
8.
5. The preparation method according to any one of claims 1 to 4, wherein In step 2), the reaction temperature is 20-40° C., and the reaction time is 1 h to 5 h. Preferably, the reaction temperature is 25-35° C., and the reaction time is 2 h to 4 h.
6. The preparation method according to any one of claims 1 to 5, wherein In step 3), the weak acid is one or more of lactic acid, acetic acid, and formic acid, preferably acetic acid; the pH of the weak acid aqueous solution is 5-6.8, preferably 5.5-6.5; and the post-treatment includes drying and grinding, wherein the drying temperature is 40-60° C. and the drying time is 8 h to 24 h.
7. The preparation method according to any one of claims 1 to 6, wherein The ligand polymer is prepared by the following steps: S1: dissolving methacrylic acid and methallyl alcohol polyether in desalted water to prepare a monomer aqueous solution; S2: adding an initiator to the monomer aqueous solution to carry out a polymerization reaction; S3: removing water from the reaction solution to obtain a ligand polymer.
8. The preparation method according to claim 7, wherein: In step S1, the concentration of the monomer aqueous solution is 20-40wt%, preferably 30-35wt%; the mass ratio of methacrylic acid to methallyl alcohol polyether is 1:0.8-1:5, preferably 1:1-1:
3.
9. The preparation method according to claim 7 or 8, wherein: In step S2, the initiator is one or more of potassium persulfate, sodium persulfate, and azobisisobutylamidine hydrochloride, preferably potassium persulfate; the amount of the initiator added is 0.20wt% to 0.24wt% of the monomer aqueous solution; the reaction temperature is 40-60°C, and the reaction time is 10-14h.
10. The preparation method according to any one of claims 7 to 9, wherein In step S3, the water in the reaction liquid is removed under a vacuum condition of -0.095-0.100 MPaG, preferably at 100-120°C.
Citation Information
Patent Citations
Bimetallic catalyst, preparation method thereof and application of bimetallic catalyst in preparation of polyether polyol
CN111072948A
High-activity double-metal cyanide catalyst as well as preparation method and application thereof
CN118255978A
Bimetallic cyanide catalyst for preparing polyether polybasic alcohol