Niobium-containing 5.5 Ni steel plate based on cooling hot rolling process and preparation method of niobium-containing 5.5 Ni steel plate

By employing a cooling hot rolling process and chemical composition design, and incorporating Ni, Mo, and Nb elements, a low-energy-consumption niobium-containing 5.5Ni steel plate was prepared. This solved the problem of high energy consumption in existing technologies and enabled the preparation of steel plates with high strength, plasticity, and low-temperature toughness, making them suitable for LNG storage tanks.

CN118979197AActive Publication Date: 2024-11-19NORTHEASTERN UNIV CHINA

Patent Information

Application Number
CN202411082839.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-08
Publication Date
2024-11-19
Estimated Expiration
2044-08-08

AI Technical Summary

Technical Problem

Existing technologies consume a lot of energy when producing 9Ni steel plates and cannot meet the service requirements of LNG storage tanks. There is a need to develop a low-energy preparation method to produce steel plates with excellent low-temperature toughness and high strength and plasticity.

Method used

A method for preparing niobium-containing 5.5Ni steel plates based on a cooling hot rolling process is adopted. Through cooling rolling and two-phase quenching and tempering process, combined with the chemical composition design of elements such as Ni, Mo, and Nb, the grains are refined and precipitation strengthening is achieved, eliminating the need for high-temperature quenching.

Benefits of technology

Niobium-containing 5.5Ni steel plates with room temperature yield strength of 585–620 MPa, room temperature tensile strength of 700–750 MPa, room temperature elongation after fracture of 22–26%, and impact energy of 150 J–200 J at -196℃ were obtained to replace 9Ni steel for LNG storage tanks, thus achieving low material cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004984276930000081
    Figure BDA0004984276930000081
  • Figure HDA0004984276940000011
    Figure HDA0004984276940000011
  • Figure HDA0004984276940000012
    Figure HDA0004984276940000012
Patent Text Reader

Abstract

The invention relates to a niobium-containing 5.5 Ni steel plate based on a cooling hot rolling process and a preparation method of the niobium-containing 5.5 Ni steel plate, and belongs to the technical field of alloy steel manufacturing. The niobium-containing 5.5 Ni steel plate provided by the invention comprises the following chemical components in percentage by weight: 0.03 to 0.06 percent of C, 0.05 to 0.12 percent of Si, 0.52 to 1.10 percent of Mn, 5.20 to 5.70 percent of Ni, 0.10 to 0.30 percent of Mo, 0.01 to 0.02 percent of Nb, less than or equal to 0.006 percent of P, less than or equal to 0.005 percent of S and the balance of Fe and inevitable impurities. According to the preparation method disclosed by the invention, on the basis of saving Ni alloy, the niobium-containing 5.5 Ni steel plate with excellent low-temperature toughness and high-strength plasticity is obtained by adopting a technological process heat treatment process of cooling rolling, two-phase region quenching and tempering, the comprehensive mechanical property reaches the level of 9Ni steel, and the low cost of the material is realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of alloy steel manufacturing, and in particular relates to a niobium-containing 5.5Ni steel plate based on a temperature-drop hot rolling process and a preparation method thereof. Background Art

[0002] LNG is a liquid formed by liquefaction of natural gas at -162℃ and 0.1MPa, and its volume is about 1 / 625 of gaseous natural gas. In view of the special physical and chemical properties of LNG, from the perspective of safety, the structural materials of ultra-low temperature storage and transportation facilities are required to have a combination of high strength, excellent ultra-low temperature toughness, good welding performance and easy processing. At present, the materials commonly used in ultra-low temperature environments are austenitic stainless steel, Ni-based alloys, aluminum alloys and Ni-based ultra-low temperature 9Ni steel. Compared with austenitic stainless steel and Ni-based alloys, 9Ni steel has lower alloy cost and higher strength; compared with aluminum alloys, 9Ni steel has higher strength and better welding performance. Therefore, 9Ni steel is widely used as the liner structural material of ultra-low temperature storage and transportation facilities internationally.

[0003] In recent years, in order to reduce the production cost of 9Ni steel and its dependence on the high-priced Ni element, the development of Ni-saving steel plates has become an important development direction for Ni-based ultra-low temperature steel. However, the reduction of Ni content in 7Ni steel is limited, so it is necessary to continue to reduce Ni.

[0004] Patent CN201410600875.5 discloses a 5Ni steel plate for ultra-low temperature pressure vessels and its production method technology. It adopts the design of low carbon equivalent composition and the production process of controlled rolling and controlled cooling + heat treatment to produce 8-50mm thick continuous casting type 5Ni steel plates that meet the requirements of low temperature pressure vessels; the product has high purity, uniform composition, excellent mechanical properties, good low temperature impact toughness, excellent welding performance, low production cost, excellent -125℃ transverse impact energy, etc., and can be mass-produced. However, the applicable temperature range of this patent is -45℃~-120℃, which cannot meet the service requirements of LNG storage tanks. And the heat treatment process is high temperature quenching + sub-temperature quenching + tempering, which is relatively complicated and energy-intensive.

[0005] Patent CN202310562946.6 discloses a 5.5Ni steel plate for ultra-low temperature environment and its manufacturing method, and by adding Cr and Mo elements, the hardenability of the steel plate is improved to ensure the core performance of the steel plate. And the corresponding mechanical properties are achieved. The tensile strength Rm of the transverse and longitudinal specimens of the steel plate is 700-830MPa, the yield strength Rel≥590MPa, and the elongation A≥21%; the specimen is bent at room temperature under the conditions of D=3a, b=2a, the bending angle is 180°, and there is no crack; and under the ultra-low temperature condition of -196℃, the impact absorption energy KV2 of the impact specimen is ≥100J. However, the patented heat treatment process is high temperature quenching + sub-temperature quenching + tempering, which is relatively complex, energy-intensive, and has low impact energy at -196℃. Summary of the invention

[0006] The purpose of the present invention is to produce a niobium-containing 5.5Ni steel plate with a strength equivalent to that of a 9Ni steel plate and a low-temperature impact energy of ≥150J at -196°C based on a cooling hot rolling process. The technical problem to be solved by the present invention is to overcome the disadvantage of high energy consumption in the prior art and provide a method for preparing a niobium-containing 5.5Ni steel plate based on a cooling hot rolling process. The manufacturing method, on the basis of saving Ni alloy, adopts a process flow heat treatment process of cooling rolling, two-phase zone quenching and tempering to obtain a niobium-containing 5.5Ni steel plate with excellent low-temperature toughness and high-strength plasticity, and the comprehensive mechanical properties reach the level of 9Ni steel, and can replace 9Ni steel for the construction of LNG storage tanks, etc., to achieve low cost of materials.

[0007] A niobium-containing 5.5Ni steel plate based on a cooling hot rolling process, wherein the chemical composition of the niobium-containing 5.5Ni steel plate is as follows by weight percentage: C: 0.03-0.06%, Si: 0.05-0.12%, Mn: 0.52-1.10%, Ni: 5.20-5.70%, Mo: 0.10-0.30%, Nb: 0.01-0.02%, P: ≤0.006%, S: ≤0.005%, and the balance is Fe and unavoidable impurities.

[0008] Furthermore, the mechanical properties of the niobium-containing 5.5Ni steel plate are room temperature yield strength of 585-620MPa, room temperature tensile strength of 700-750MPa, room temperature elongation after fracture of 22-26%, and impact energy of 150J-200J at -196°C.

[0009] A method for preparing a Nb5.5Ni-containing steel plate based on a cooling hot rolling process comprises the following steps:

[0010] (1) according to the chemical composition design of the niobium-containing 5.5Ni steel plate, a steel ingot is produced by using a vacuum induction melting furnace, the steel ingot is heated to 1200° C. after the riser is cut off, and the steel ingot is kept at this temperature for 2 hours and then forged into a steel billet;

[0011] (2) The steel billet is kept at 1200°C for 1.5 to 2.5 hours, and then cooled to 990 to 1020°C for multiple rough rolling. The rough rolling stage is in the static recrystallization zone of austenite to obtain a rough rolled steel plate;

[0012] (3) subjecting the rough-rolled steel sheet to multiple passes of finish rolling, wherein the finish rolling stage is in the austenite non-recrystallization region to obtain a rolled steel sheet;

[0013] (4) performing a two-phase zone quenching heat treatment on the rolled steel plate;

[0014] (5) The steel plate after two-phase region quenching is subjected to high temperature tempering at a temperature lower than Ac1 and air-cooled to room temperature to obtain a niobium-containing 5.5Ni low-temperature steel plate with excellent room temperature strength and plasticity and -196°C impact toughness.

[0015] Furthermore, in the step (1), the thickness of the steel billet is 100 to 110 mm, and the steel billet is heated in a box-type resistance furnace.

[0016] Furthermore, in the step (2), the rough rolling stage has four passes, the reduction rate of each pass is 20-25%, the thickness of the intermediate billet is 45-50 mm, the cumulative reduction rate is 45-50%, and the rough rolling final rolling temperature is 890-930°C.

[0017] Furthermore, in the step (2), the thickness of the rough-rolled steel plate is 45 to 50 mm.

[0018] Furthermore, in the step (3), the finishing rolling stage has three passes, the reduction rate of each pass is 20-25%, the thickness of the rolled steel plate is 6-20 mm, the total reduction rate is ≥65%, the final rolling temperature is 810-830° C., and the steel is water-cooled to room temperature after rolling.

[0019] Furthermore, in the step (3), the thickness of the rolled steel plate is 6 to 20 mm.

[0020] Furthermore, the two-phase region sub-temperature quenching temperature in step (4) is between Ac1 and Ac3, the two-phase region sub-temperature quenching temperature is 670-710° C., and the holding time is 30-40 min.

[0021] Furthermore, the tempering temperature in step (5) is 570-610° C., and the holding time is 18-30 min.

[0022] The following is a detailed description of the effects and dosage of the components in the present invention:

[0023] C: is the most important strengthening element in steel and also the element that has the greatest impact on toughness, especially low temperature toughness. For 5.5Ni steel plate, considering that the Ni content is significantly lower than that in 9Ni, the C content is lower than that in conventional 9Ni steel. Based on this, the present invention controls the carbon content to be 0.03-0.06%.

[0024] Si: It is a weak deoxidizing element in steel and is cheap. Si in steel improves the strength of steel in the form of solid solution strengthening; when the Si content is less than 0.05%, the deoxidation effect is poor; when the Si content is higher, the toughness and welding performance will decrease. The Si content of the present invention is controlled to be 0.05-0.12%.

[0025] Mn: It has a solid solution strengthening and deoxidation effect, but its deoxidation ability is relatively weak. Compared with 9Ni steel, due to the lower C content and Ni content, a higher Mn content is designed to improve the strength of the steel plate. The Mn content of the present invention is controlled to be 0.52-0.98%.

[0026] Ni: It is a beneficial element that can significantly improve low-temperature toughness, especially has a significant impact on the impact toughness and tough-to-brittle transition process of steel plates in ultra-low temperature environments, but too high a Ni content will greatly increase the manufacturing cost of the steel plate. Therefore, the present invention controls its content to 5.20-5.80%.

[0027] Mo: It can improve hardenability, thereby increasing strength; it can improve the tempering stability of steel; when it coexists with chromium or manganese, it can reduce or inhibit the temper brittleness caused by other elements.

[0028] Nb: Nb has all the important functions of a microalloying element in steel. Different forms of Nb have different functions. Part of Nb can be dissolved in the Fe matrix, and part of it can form stable carbides, nitrides or carbonitrides with C and N. Nb dissolved in austenite can inhibit the recrystallization of deformed austenite and increase the recrystallization temperature of austenite, thereby refining the ferrite grains after rolling. At the same time, the coincidence of the temperature reduction hot rolling and the precipitation temperature of Nb in austenite can promote the precipitation of fine Nb (C, N), which is one of the innovations of the present invention.

[0029] P: is a harmful impurity element in steel. Phosphorus combines with iron to form iron phosphide, which is easy to form segregation at the grain boundary, weaken the grain boundary and cause cold brittleness. The content of P in the present invention is controlled to ≤ 0.006%.

[0030] S: It is a harmful impurity element in steel, which is easy to form defects such as segregation and inclusions. During the solidification process of the slab, Mn is easy to segregate with S in the center of the slab to form lamellar MnS inclusions, reducing the formation of low-melting FeS at the austenite grain boundary. However, MnS inclusions are easy to cause unstable impact toughness in the core of the steel plate. In the later stage of refining, the Ca treatment technology is used to make the inclusion morphology spheroidized and evenly distributed, reduce the viscosity of the molten steel, and promote the floating of the inclusions. The present invention controls its content to ≤0.005%.

[0031] Elements such as Mn, Mo, and Ni in steel are all elements that improve the hardenability of steel plates. A lamellar martensitic structure is obtained by water cooling after hot rolling. During the sub-temperature quenching process in the two-phase zone, part of the original martensite is re-austenitized, and new martensite is obtained in the subsequent water cooling process, which refines the grains. During this process, the stability of the original martensite is reduced. During the high-temperature tempering process, C and Ni have certain diffusion and migration capabilities, and part of the unstable original martensite phase decomposes, breaking through the potential energy barrier under the action of carbon and nickel elements, and inverting to form austenite.

[0032] The Nb element in steel can reduce the transformation temperature of austenite to BCC phase. Under the same conditions, especially at high cooling rates, Nb can promote the formation of low-temperature phase transformation products such as acicular ferrite and bainite. During hot rolling, Nb can form stable carbonitrides, which prevent the growth of austenite grains during controlled heating before rolling, refine the original austenite grains, and improve their stability; and the dispersed and fine Nb (C, N) particles precipitated during controlled rolling and post-rolling cooling can produce a strong precipitation strengthening effect and improve the strength of steel.

[0033] In the step (2), the steel billet is cooled to 990-1020°C and then subjected to multiple rough rolling. This temperature coincides with the precipitation temperature of Nb(C,N) in austenite, and when the temperature is ≥810°C, the hot rolling deformation resistance does not change significantly, and the hot rolling compliance is not increased. Therefore, the cooling hot rolling process can not only refine the original austenite grains, but also promote the precipitation of Nb(C,N), achieving the coupling effect of grain refinement and precipitation strengthening.

[0034] Compared with the prior art, the niobium-containing 5.5Ni steel plate based on the cooling hot rolling process and the preparation method thereof of the present invention have the following advantages and beneficial effects:

[0035] 1. A niobium-containing 5.5Ni steel plate based on a cooling hot rolling process and its preparation method are proposed, and the corresponding mechanical properties are achieved. The room temperature yield strength is 585-620MPa, the room temperature tensile strength is 700-750MPa, the room temperature elongation is 22-26%, and the impact energy at -196℃ is 150J-200J.

[0036] 2. The chemical composition design adds additional Nb elements to improve its stability by expanding the austenite phase area and refining the original austenite grain size, thereby obtaining residual austenite in the final structure, and precipitation strengthening can be achieved through Nb (C, N).

[0037] 3. The cooling hot rolling process is adopted to stably overlap with the precipitation nose of Nb(C,N) in austenite, promote the precipitation of Nb(C,N) in austenite, and enhance the precipitation strengthening effect.

[0038] 4. Compared with the traditional QLT process, the process of water cooling after hot rolling + LT can not only improve the heritability of hot-rolled structure (fine grains and precipitation, etc.), but also eliminate the high-energy consumption step of high-temperature quenching, which is more green and efficient. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] Figure 1 This is a typical SEM microstructure image of rolled state of 1# steel prepared in Example 1 based on the cooling hot rolling process;

[0040] Figure 2 The final heat treatment structure diagram of a 1# steel prepared in Example 1 based on a cooling hot rolling process;

[0041] Figure 3 A typical tensile engineering stress-strain curve of 1# steel prepared in Example 1 based on a cooling hot rolling process;

[0042] Figure 4 The final heat treatment structure diagram of 2# steel prepared in Example 2 based on the temperature reduction hot rolling process;

[0043] Figure 5 The final heat treatment structure diagram of 3# steel prepared in Example 3 based on the temperature reduction hot rolling process;

[0044] Figure 6 The final heat treatment structure diagram of 4# steel prepared in Example 4 based on the temperature reduction hot rolling process;

[0045] Figure 7 The final heat treatment structure diagram of 5# steel prepared in Example 5 based on the temperature reduction hot rolling process;

[0046] Figure 8 The final heat treatment structure diagram of 6# steel prepared in Example 6 based on the temperature reduction hot rolling process;

[0047] Fig. 9 This is a longitudinal tensile performance curve of 2#-6# steel prepared based on a cooling hot rolling process in Example 2-6. DETAILED DESCRIPTION

[0048] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and do not limit the present invention.

[0049] The hot rolling forming process of the following examples was carried out on a 450mm two-roll reversible hot rolling experimental rolling mill.

[0050] Example 1

[0051] A niobium-containing 5.5Ni steel plate based on a cooling hot rolling process is a 1# steel plate, wherein the chemical composition of the 1# steel plate is as follows by weight: C: 0.045%, Si: 0.112%, Mn: 0.95%, Ni: 5.58%, Mo: 0.216%, Nb: 0.019%, P: 0.005%, S: 0.003%, and the balance is Fe and unavoidable impurities.

[0052] A method for preparing a Nb5.5Ni-containing steel plate based on a cooling hot rolling process comprises the following steps:

[0053] (1) According to the chemical composition design of the niobium-containing 5.5Ni steel plate, a steel ingot is produced by using a vacuum induction melting furnace, the steel ingot is heated to 1200° C. after the riser is cut off, and the steel ingot is kept at this temperature for 2 hours and then forged into a steel billet 1# with a thickness of 100 mm;

[0054] (2) The steel billet is kept at 1200°C for 2 hours, and then the steel billet 1# is blown cold to 1000°C for rough rolling in the austenite static recrystallization zone, the starting rolling temperature is 1004°C, the final rolling temperature is 897°C, the rolling passes are 4 times, the single pass reduction rate is 20-22%, and the total reduction rate is 53.4%. After rolling, the steel billet is water-cooled to obtain a rough-rolled steel plate;

[0055] (3) After the rough rolling is completed, multiple passes of finishing rolling are performed, the finishing rolling stage is in the austenite non-recrystallization zone, the finishing rolling stage has three passes, the starting rolling temperature is 864°C, the final rolling temperature is 824°C, the single pass reduction rate is 20-22%, the total reduction rate is 68.2%, and air cooling is performed after rolling to obtain a rolled steel plate;

[0056] (4) performing a two-phase zone quenching heat treatment on the rolled steel plate, wherein the two-phase zone sub-temperature quenching temperature is 690° C., the holding time is 36 min, and the cooling method is air cooling;

[0057] (5) The steel plate after two-phase zone quenching is subjected to high-temperature tempering at a temperature lower than Ac1 and air-cooled to room temperature. The tempering temperature is 590°C and the holding time is 18 min to obtain a 1# steel plate.

[0058] Typical rolled SEM microstructure of 1# steel Figure 1 As shown, the final heat treatment structure is as follows Figure 2As shown, the typical tensile engineering stress-strain curve of 1# steel is as follows Figure 3 The niobium-containing 5.5Ni steel plate prepared in this embodiment with excellent room temperature ductility and low temperature impact toughness was subjected to tensile and impact test specimens along the rolling direction and transverse direction. The room temperature tensile strength and -196°C impact energy are shown in Table 1.

[0059] Example 2

[0060] A niobium-containing 5.5Ni steel plate based on a cooling hot rolling process is a 1# steel plate, wherein the chemical composition of the 1# steel plate is as follows by weight: C: 0.045%, Si: 0.112%, Mn: 0.95%, Ni: 5.58%, Mo: 0.216%, Nb: 0.019%, P: 0.005%, S: 0.003%, and the balance is Fe and unavoidable impurities.

[0061] A method for preparing a Nb5.5Ni-containing steel plate based on a cooling hot rolling process comprises the following steps:

[0062] (1) According to the chemical composition design of the niobium-containing 5.5Ni steel plate, a steel ingot is produced by using a vacuum induction melting furnace, the ingot is heated to 1200° C. after the riser is cut off, and the steel ingot is kept at this temperature for 2 hours and then forged into a 2# steel billet with a thickness of 100 mm;

[0063] (2) The steel billet was kept at 1200°C for 2h, and then the 2# steel billet was directly subjected to rough rolling in the austenite dynamic recrystallization zone, with the starting rolling temperature of 1091°C, the final rolling temperature of 942°C, 4 rolling passes, a single-pass reduction rate of 20-22%, and a total reduction rate of 52.0%, and water-cooled after rolling to obtain a rough-rolled steel plate;

[0064] (3) After the rough rolling is completed, multiple passes of finishing rolling are performed, the finishing rolling stage is in the austenite non-recrystallization zone, the finishing rolling stage has three passes, the starting rolling temperature is 870°C, the final rolling temperature is 844°C, the single pass reduction rate is 21-26%, the total reduction rate is 66.7%, and air cooling is performed after rolling to obtain a rolled steel plate;

[0065] (4) performing a two-phase zone quenching heat treatment on the rolled steel plate, wherein the two-phase zone sub-temperature quenching temperature is 690° C., the holding time is 36 min, and the cooling method is air cooling;

[0066] (5) The steel plate after two-phase zone quenching is subjected to high-temperature tempering at a temperature lower than Ac1 and air-cooled to room temperature. The tempering temperature is 590°C and the holding time is 18 min to obtain a 2# steel plate.

[0067] Tensile specimens and impact specimens were taken from the niobium-containing 5.5Ni steel plate prepared in this embodiment with excellent room temperature ductility and low temperature impact toughness along the rolling direction and the transverse direction. The room temperature tensile strength and -196°C impact energy are shown in Table 1.

[0068] Example 3

[0069] A niobium-containing 5.5Ni steel plate based on a cooling hot rolling process is a 1# steel plate, wherein the chemical composition of the 1# steel plate is as follows by weight: C: 0.043%, Si: 0.107%, Mn: 1.01%, Ni: 5.47%, Mo: 0.192%, Nb: 0.01%, P: 0.005%, S: 0.003%, and the remainder is Fe and unavoidable impurities.

[0070] A method for preparing a Nb5.5Ni-containing steel plate based on a cooling hot rolling process comprises the following steps:

[0071] (1) According to the chemical composition design of the niobium-containing 5.5Ni steel plate, a steel ingot was produced by using a vacuum induction melting furnace, and after the riser was removed, it was heated to 1200° C. and kept at this temperature for 2 hours before being forged into a 3# steel billet with a thickness of 100 mm;

[0072] (2) The steel billet was kept at 1200°C for 2h, and then the 3# steel billet was directly subjected to rough rolling in the austenite dynamic recrystallization zone, with the starting rolling temperature of 1103°C, the final rolling temperature of 950°C, the rolling passes of 4 times, the single-pass reduction rate of 20-22%, and the total reduction rate of 52.6%, and water-cooled after rolling to obtain a rough-rolled steel plate;

[0073] (3) After the rough rolling is completed, multiple passes of finishing rolling are performed, the finishing rolling stage is in the austenite non-recrystallization zone, the finishing rolling stage has three passes, the starting rolling temperature is 881°C, the final rolling temperature is 847°C, the single pass reduction rate is 21-26%, the total reduction rate is 67.0%, and air cooling is performed after rolling to obtain a rolled steel plate;

[0074] (4) performing a two-phase zone quenching heat treatment on the rolled steel plate, wherein the two-phase zone sub-temperature quenching temperature is 690° C., the holding time is 36 min, and the cooling method is air cooling;

[0075] (5) The steel plate after two-phase zone quenching was subjected to high-temperature tempering at a temperature lower than Ac1 and air-cooled to room temperature. The tempering temperature was 590°C and the holding time was 18 min to obtain a 3# steel plate.

[0076] Tensile specimens and impact specimens were taken from the niobium-containing 5.5Ni steel plate prepared in this embodiment with excellent room temperature ductility and low temperature impact toughness along the rolling direction and the transverse direction. The room temperature tensile strength and -196°C impact energy are shown in Table 1.

[0077] Example 4

[0078] A niobium-containing 5.5Ni steel plate based on a cooling hot rolling process is a 1# steel plate, wherein the chemical composition of the 1# steel plate is as follows by weight: C: 0.043%, Si: 0.107%, Mn: 1.01%, Ni: 5.47%, Mo: 0.192%, Nb: 0.01%, P: 0.005%, S: 0.003%, and the remainder is Fe and unavoidable impurities.

[0079] A method for preparing a Nb5.5Ni-containing steel plate based on a cooling hot rolling process comprises the following steps:

[0080] (1) According to the chemical composition design of the niobium-containing 5.5Ni steel plate, a steel ingot is produced by using a vacuum induction melting furnace, the steel ingot is heated to 1200° C. after the riser is cut off, and the steel ingot is kept at this temperature for 2 hours and then forged into a 4# steel billet with a thickness of 100 mm;

[0081] (2) The steel billet was kept at 1200°C for 2 hours, and then the 4# steel billet was blown cold to 1000°C for rough rolling in the austenite static recrystallization zone, with the starting rolling temperature of 1011°C, the final rolling temperature of 903°C, 4 rolling passes, a single-pass reduction rate of 20-22%, and a total reduction rate of 52.9%. After rolling, the steel billet was water-cooled to obtain a rough-rolled steel plate;

[0082] (3) After the rough rolling is completed, multiple passes of finishing rolling are performed. The finishing rolling stage is in the austenite non-recrystallization zone. The finishing rolling stage has three passes in total. The starting rolling temperature is 851° C., the final rolling temperature is 817° C., the single pass reduction rate is 20-22%, and the total reduction rate is 67.9%. After rolling, air cooling is performed to obtain a rolled steel plate;

[0083] (4) performing a two-phase zone quenching heat treatment on the rolled steel plate, wherein the two-phase zone sub-temperature quenching temperature is 690° C., the holding time is 36 min, and the cooling method is air cooling;

[0084] (5) The steel plate after two-phase zone quenching was subjected to high-temperature tempering at a temperature lower than Ac1 and air-cooled to room temperature. The tempering temperature was 590°C and the holding time was 18 min to obtain a 4# steel plate.

[0085] Tensile specimens and impact specimens were taken from the niobium-containing 5.5Ni steel plate prepared in this embodiment with excellent room temperature ductility and low temperature impact toughness along the rolling direction and the transverse direction. The room temperature tensile strength and -196°C impact energy are shown in Table 1.

[0086] Example 5

[0087] A niobium-containing 5.5Ni steel plate based on a cooling hot rolling process is a 1# steel plate, wherein the chemical composition of the 1# steel plate is as follows by weight: C: 0.045%, Si: 0.112%, Mn: 0.95%, Ni: 5.58%, Mo: 0.216%, Nb: 0.019%, P: 0.005%, S: 0.003%, and the balance is Fe and unavoidable impurities.

[0088] A method for preparing a Nb5.5Ni-containing steel plate based on a cooling hot rolling process comprises the following steps:

[0089] (1) According to the chemical composition design of the niobium-containing 5.5Ni steel plate, a steel ingot is produced by using a vacuum induction melting furnace, and after the riser is cut off, it is heated to 1200° C. and kept at this temperature for 2 hours before being forged into a 5# steel billet with a thickness of 100 mm;

[0090] (2) The steel billet was kept at 1200°C for 2 hours, and then the 5# steel billet was cooled to 1000°C for rough rolling in the austenite static recrystallization zone, with the starting rolling temperature of 1004°C, the final rolling temperature of 897°C, the rolling passes of 4 times, the single-pass reduction rate of 20-22%, and the total reduction rate of 53.4%, and water-cooled after rolling to obtain a rough-rolled steel plate;

[0091] (3) After the rough rolling is completed, multiple passes of finishing rolling are performed. The finishing rolling stage is in the austenite non-recrystallization zone. The finishing rolling stage has three passes in total. The starting rolling temperature is 846° C., the final rolling temperature is 824° C., the single pass reduction rate is 20-22%, and the total reduction rate is 68.2%. After rolling, air cooling is performed to obtain a rolled steel plate;

[0092] (4) performing a two-phase zone quenching heat treatment on the rolled steel plate, wherein the two-phase zone sub-temperature quenching temperature is 650° C., the holding time is 36 min, and the cooling method is air cooling;

[0093] (5) The steel plate after two-phase zone quenching is subjected to high-temperature tempering at a temperature lower than Ac1 and air-cooled to room temperature. The tempering temperature is 590°C and the holding time is 18 min to obtain a 5# steel plate.

[0094] Tensile specimens and impact specimens were taken from the niobium-containing 5.5Ni steel plate prepared in this embodiment with excellent room temperature ductility and low temperature impact toughness along the rolling direction and the transverse direction. The room temperature tensile strength and -196°C impact energy are shown in Table 1.

[0095] Example 6

[0096] A niobium-containing 5.5Ni steel plate based on a cooling hot rolling process is a 1# steel plate, wherein the chemical composition of the 1# steel plate is as follows by weight: C: 0.045%, Si: 0.112%, Mn: 0.95%, Ni: 5.58%, Mo: 0.216%, Nb: 0.019%, P: 0.005%, S: 0.003%, and the balance is Fe and unavoidable impurities.

[0097] A method for preparing a Nb5.5Ni-containing steel plate based on a cooling hot rolling process comprises the following steps:

[0098] (1) According to the chemical composition design of the niobium-containing 5.5Ni steel plate, a steel ingot is produced by using a vacuum induction melting furnace, and after the riser is cut off, it is heated to 1200° C. and kept at this temperature for 2 hours before being forged into a 5# steel billet with a thickness of 100 mm;

[0099] (2) The steel billet was kept at 1200°C for 2 hours, and then the 5# steel billet was cooled to 1000°C for rough rolling in the austenite static recrystallization zone, with the starting rolling temperature of 1004°C, the final rolling temperature of 897°C, the rolling passes of 4 times, the single-pass reduction rate of 20-22%, and the total reduction rate of 53.4%, and water-cooled after rolling to obtain a rough-rolled steel plate;

[0100] (3) After the rough rolling is completed, multiple passes of finishing rolling are performed. The finishing rolling stage is in the austenite non-recrystallization zone. The finishing rolling stage has three passes in total. The starting rolling temperature is 846° C., the final rolling temperature is 824° C., the single pass reduction rate is 20-22%, and the total reduction rate is 68.2%. After rolling, air cooling is performed to obtain a rolled steel plate;

[0101] (4) performing a two-phase zone quenching heat treatment on the rolled steel plate, wherein the two-phase zone sub-temperature quenching temperature is 730° C., the holding time is 36 min, and the cooling method is air cooling;

[0102] (5) The steel plate after two-phase zone quenching is subjected to high-temperature tempering at a temperature lower than Ac1 and air-cooled to room temperature. The tempering temperature is 590°C and the holding time is 18 min to obtain a 5# steel plate.

[0103] Tensile specimens and impact specimens were taken from the niobium-containing 5.5Ni steel plate prepared in this embodiment with excellent room temperature ductility and low temperature impact toughness along the rolling direction and the transverse direction. The room temperature tensile strength and -196°C impact energy are shown in Table 1.

[0104] The final heat treatment structure of 2#-6# is as follows Figure 4-8 As shown, the longitudinal tensile performance curve is as follows Fig. 9 shown.

[0105] Table 1 Summary of mechanical properties

[0106]

[0107] The results of the examples show that the niobium-containing 5.5Ni steel plate and its preparation method based on the cooling hot rolling process of the present invention can make the niobium-containing 5.5Ni steel plate obtain excellent room temperature strength and plasticity, and -196℃ impact energy while taking into account simplicity, high efficiency and low cost. And by comparing the results of Example 1 and Example 2, it is shown that the cooling hot rolling process can effectively improve the room temperature strength and plasticity, and -196℃ impact energy. By comparing the results of Example 1 and Example 4, it is shown that within an appropriate range, increasing the Nb content can effectively improve the room temperature strength without reducing its room temperature plasticity and -196℃ impact energy. By comparing the results of Example 1 and Example 5 / 6, it is shown that if the annealing temperature in the critical zone is too high or too low, it will lead to a low ferrite content in the critical zone. Although the room temperature strength can be effectively improved, the room temperature plasticity and -196℃ impact energy are greatly reduced.

Claims

1. A niobium-containing 5.5Ni steel plate based on a cooling hot rolling process, characterized in that: The chemical composition of the niobium-containing 5.5Ni steel plate is as follows by weight percentage: C: 0.03-0.06%, Si: 0.05-0.12%, Mn: 0.52-1.10%, Ni: 5.20-5.70%, Mo: 0.10-0.30%, Nb: 0.01-0.02%, P: ≤0.006%, S: ≤0.005%, and the remainder is Fe and unavoidable impurities.

2. The niobium-containing 5.5Ni steel plate based on the temperature reduction hot rolling process according to claim 1, characterized in that: The mechanical properties of the niobium-containing 5.5Ni steel plate are as follows: room temperature yield strength of 585-620MPa, room temperature tensile strength of 700-750MPa, room temperature elongation after fracture of 22-26%, and impact energy of 150J-200J at -196°C.

3. A method for preparing a niobium-containing 5.5Ni steel plate based on a temperature-drop hot rolling process according to any one of claims 1 or 2, characterized in that: The steps include: (1) according to the chemical composition design of the niobium-containing 5.5Ni steel plate, a steel ingot is produced by using a vacuum induction melting furnace, the steel ingot is heated to 1200° C. after the riser is cut off, and the steel ingot is kept at this temperature for 2 hours and then forged into a steel billet; (2) The steel billet is kept at 1200°C for 1.5 to 2.5 hours, and then cooled to 990 to 1020°C for multiple rough rolling. The rough rolling stage is in the static recrystallization zone of austenite to obtain a rough rolled steel plate; (3) subjecting the rough-rolled steel sheet to multiple passes of finish rolling, wherein the finish rolling stage is in the austenite non-recrystallization region to obtain a rolled steel sheet; (4) performing a two-phase zone quenching heat treatment on the rolled steel plate; (5) The steel plate after two-phase region quenching is subjected to high temperature tempering at a temperature lower than Ac1 and air-cooled to room temperature to obtain a niobium-containing 5.5Ni low-temperature steel plate with excellent room temperature strength and plasticity and -196°C impact toughness.

4. The method for preparing a niobium-containing 5.5Ni steel plate based on a temperature-lowering hot rolling process according to claim 3, characterized in that: In the step (1), the thickness of the steel billet is 100-110 mm, and the steel billet is heated in a box-type resistance furnace.

5. The method for preparing a niobium-containing 5.5Ni steel plate based on a temperature reduction hot rolling process according to claim 3, characterized in that: In the step (2), the rough rolling stage has four passes, the reduction rate of each pass is 20-25%, the thickness of the intermediate billet is 45-50 mm, the cumulative reduction rate is 45-50%, and the rough rolling final rolling temperature is 890-930°C.

6. The method for preparing a niobium-containing 5.5Ni steel plate based on a temperature-lowering hot rolling process according to claim 3, characterized in that: In the step (2), the thickness of the rough-rolled steel plate is 45 to 50 mm.

7. The method for preparing a niobium-containing 5.5Ni steel plate based on a temperature-lowering hot rolling process according to claim 3, characterized in that: In the step (3), the finishing rolling stage is performed in three passes, the reduction rate of each pass is 20-25%, the thickness of the rolled steel plate is 6-20 mm, the total reduction rate is ≥65%, the final rolling temperature is 810-830° C., and the steel plate is water-cooled to room temperature after rolling.

8. The method for preparing a niobium-containing 5.5Ni steel plate based on a temperature-lowering hot rolling process according to claim 3, characterized in that: In the step (3), the thickness of the rolled steel plate is 6 to 20 mm.

9. The method for preparing a niobium-containing 5.5Ni steel plate based on a temperature-lowering hot rolling process according to claim 3, characterized in that: The two-phase region sub-temperature quenching temperature described in step (4) is between Ac1 and Ac3, the two-phase region sub-temperature quenching temperature is 670-710°C, and the holding time is 30-40 minutes.

10. The method for preparing a niobium-containing 5.5Ni steel plate based on a temperature reduction hot rolling process according to claim 3, characterized in that: The tempering temperature in step (5) is 570-610° C., and the holding time is 18-30 minutes.

Citation Information

Patent Citations

  • Thick steel plate for ocean platform structure with yield strength of 500MPa grade and manufacture method thereof

    CN102127719A

  • QT (Quenching-Tempering) process-based steel plate for low-nickel LNG (Liquefied Natural Gas) storage tank and preparation method thereof

    CN109136769A

  • Steel plate for low-nickel type liquefied natural gas storage tank and preparation method thereof

    CN109280848A

  • 5% Ni low-temperature steel and manufacturing method thereof

    CN114686649A

  • Nb7Ni-containing ultralow-temperature steel for nickel-saving LNG storage tank and heat treatment process of Nb7Ni-containing ultralow-temperature steel

    CN115747652A

Cited By

  • Forging and rolling method for improving hot rolling edge cracks of ultra-super ferritic stainless steel

    CN119464656A

  • Chromium-rich 5.5 Ni steel plate based on TMCP process and preparation method thereof

    CN120099412A

  • Method for improving impact toughness of 5.5 Ni steel of medium plate

    CN120350203A

  • Method for improving impact toughness of 5.5Ni steel plate

    CN120350203B

  • Method for improving strength and impact toughness of 3.5 Ni steel plate in low-temperature environment

    CN120700405A