Fabric with self-cleaning function and self-repairing effect and preparation method thereof

By forming photocatalytic nanoarray modified nano microspheres on the fabric and combining dopamine-tris and fluorosiloxane-ethanol treatment, fabrics with self-cleaning and self-healing functions are prepared, solving the difficulty of cleaning and durability of traditional fabrics. The poor performance problem has achieved efficient self-cleaning and reuse of fabrics.

CN118979377APending Publication Date: 2024-11-19SHANXI UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411093475.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

After being contaminated by water-soluble and hydrophobic, traditional fabrics are difficult to effectively clean, and the modified fabrics have poor durability and cannot be reused, which limits their large-scale production and multi-functional applications.

Method used

Nanomicrospheres were dispersed into the precursor solution of the photocatalytic nanomaterial, calcined and hydrothermal treatment were performed to form photocatalytic nanoarray modified nanospheres, and treated by dopamine-tris solution and fluorosiloxane-ethanol solution. , fabrics with self-cleaning and self-healing functions were prepared. The fabric produces superoxide radicals under ultraviolet lamps, oxidizes organic pollutants, and returns to superhydrophobic state after being exposed to light or drying.

Benefits of technology

It realizes self-cleaning and self-repair of fabrics, can turn into super-hydrophilic state under ultraviolet lamps to clean pollutants, and restore to super-hydrophobic state after being away from light or drying, extending the service life of the fabrics and is suitable for reuse. and large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118979377A_ABST
    Figure CN118979377A_ABST
Patent Text Reader

Abstract

The invention discloses a fabric with a self-cleaning function and a self-repairing effect and a preparation method thereof, and belongs to the technical field of functional textile preparation. The fabric with a self-cleaning function and a self-repairing effect is finally obtained by loading nano microspheres modified by a photocatalytic nano array on the surface of the fabric and constructing a super-amphiphobic structure through surface fluorination. The prepared fabric has super-amphiphobic property and also has a light-induced self-cleaning effect, the surface is converted into a super-hydrophilic state from a super-hydrophobic state under the irradiation of an ultraviolet lamp, wetting switching and catalysis are carried out, and rapid self-cleaning is realized; meanwhile, the super-amphiphobic performance of the super-hydrophilic fabric can be recovered after the super-hydrophilic fabric is dried for 30-60 minutes or kept away from light for 3-8 days, self-repairing is achieved, reutilization can be achieved, and wide application value is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of functional textile preparation, and in particular relates to a fabric with self-cleaning and self-repairing effects and a preparation method thereof. Background Art

[0002] The main component of traditional fabrics is cellulose. Cellulose is a renewable material and is widely used in the clothing field due to its good comfort. However, due to its hydrophilicity, cellulose is easily infiltrated by water-soluble substances and causes pollution. The most common solution to this problem is to modify the surface of the fabric into a super-amphiphobic surface, making the fabric surface highly liquid-repellent. However, studies have shown that the modified fabrics will still be contaminated by hydrophobic organic matter, such as proteins, dyes, etc. The contaminated fabrics are highly liquid-repellent, resulting in poor cleaning effects with ordinary cleaning methods. Using complex cleaning methods will damage the fabric and shorten its service life. Therefore, the preparation of a multifunctional fabric that can be easily cleaned and reused multiple times has broad application prospects.

[0003] Generally speaking, an ideal fabric surface should be both superhydrophilic and superhydrophobic. Superhydrophobic surfaces are not easily contaminated by hydrophilic substances, while superhydrophilic surfaces can resist hydrophobic pollutants. Therefore, when the fabric surface is in a superhydrophobic state, it can prevent contamination by hydrophilic substances, and when it is converted to a superhydrophilic state, it can clean hydrophobic pollutants. Although it is very difficult to make such a fabric, the emergence of photocatalytic technology has made it possible to solve this problem. Common photocatalytic materials include titanium dioxide, zinc oxide, tin oxide, zirconium dioxide, cadmium sulfide, etc. The superoxide radicals (ROS) generated by photocatalytic materials under light conditions have extremely strong oxidizing properties, which can oxidize organic matter into carbon dioxide and water, and can even completely decompose some inorganic substances. Using this characteristic of photocatalytic materials, self-cleaning of fabrics can be achieved without contact, ensuring the integrity of the fabric surface.

[0004] Karimi et al. generated nano-TiO2 on the surface of cotton fabric by an in-situ growth method, and the degradation rate of methyl orange by the fabric was significantly improved under light conditions. Li et al. loaded the prepared flower-shaped TiO2 onto the surface of cotton fabric by an impregnation method, and prepared a multifunctional cotton fabric with super-amphiphobic and photocatalytic properties. The degradation rate of Reactive Red 195 reached more than 78% under the irradiation of simulated sunlight. Although the above-mentioned prior art has achieved some results and progress, there are still problems that need to be further studied and solved: (1) The in-situ growth method has certain limitations in large-scale production applications; (2) The fabric has poor durability and the modified fabric cannot be reused after being contaminated. Therefore, it is urgent to develop a multifunctional fabric that can be reused and suitable for large-scale production. Summary of the invention

[0005] In order to solve the technical problems existing in the above-mentioned prior art, the present invention provides a fabric with self-cleaning function and self-repairing effect and a preparation method thereof.

[0006] To achieve the above object, the technical solution of the present invention is as follows:

[0007] A first aspect of the present invention is a method for preparing a fabric having a self-cleaning function and a self-repairing effect, comprising the following steps:

[0008] Step 1: dispersing nanospheres into a precursor solution of a photocatalytic nanomaterial, stirring evenly, washing, and drying to obtain a photocatalytic nanocrystalline seed layer; calcining and hydrothermally treating the photocatalytic nanocrystalline seed layer to obtain nanospheres modified with a photocatalytic nanoarray;

[0009] Step 2: soaking the fabric in a dopamine-tris solution, taking it out and drying it, then soaking it in a dispersion of nano-microspheres modified by a photocatalytic nano-array, taking it out and drying it, to obtain a fabric loaded with nano-microspheres modified by a photocatalytic nano-array;

[0010] Step 3: fluorination of the fabric surface is completed by dehydration condensation using a fluorinated silicone-ethanol solution, and the fabric is naturally dried to obtain the fabric having self-cleaning and self-repairing effects.

[0011] Furthermore, in step 1, the nanospheres are at least one of silicon dioxide particles, calcium oxide particles, carbon black particles, calcium carbonate particles, polytetrafluoroethylene particles, polystyrene microspheres, and polypropylene microspheres; the photocatalytic nanomaterial is at least one of titanium dioxide, zinc oxide, ferric oxide, cuprous oxide, tungsten trioxide, tin oxide, zirconium dioxide, cadmium sulfide, and zinc sulfide.

[0012] Furthermore, in step 1, the mass ratio of the nano-microspheres to the photocatalytic nano-material is 1:5-20, and the mass fraction of the precursor solution of the photocatalytic nano-material is 10-50%.

[0013] Furthermore, in step 1, the calcination temperature is 400-700° C., and the calcination time is 2-4 hours; the hydrothermal reaction temperature is 100-200° C., and the hydrothermal reaction time is 4-10 hours.

[0014] Furthermore, the preparation process of the dispersion of nanospheres modified by photocatalytic nanoarrays in step 2 is as follows: the nanospheres modified by photocatalytic nanoarrays are mixed with water in a ratio of (1-3) mg: (2-10) mL, and ultrasonicated for 0.5-1 h.

[0015] Furthermore, in step 2, the concentration of the dopamine-tris solution is 0.2-0.4 g / L, and the fabric is immersed in the dopamine-tris solution for 1-3 hours.

[0016] Furthermore, in step 2, the fabric is immersed in the dispersion of nano-microspheres modified with photocatalytic nano-arrays for 1 to 2 hours.

[0017] Furthermore, the fluorinated silicone in step 3 is at least one of heptadecafluorodecyltrimethylsiloxane, perfluorodecyltriethoxysilane, tridecafluorooctyltriethoxysilane, nonafluorohexyltriethoxysilane, and trifluoropropyltrimethylsiloxane.

[0018] Furthermore, in step 3, the volume fraction of the fluorinated silicone-ethanol solution is 5-20%, and the fluorination time is 2-10 hours.

[0019] The second aspect of the present invention is a fabric with self-cleaning function and self-repairing effect prepared by the preparation method described in the first aspect. The surface of the fabric is loaded with nano-microspheres modified with photocatalytic nano-arrays and has a super-amphiphobic structure. Under the irradiation of ultraviolet light, it produces superoxide free radicals with strong oxidizing properties, which can oxidize organic pollutants and complete self-cleaning. At the same time, the fabric is transformed from a super-hydrophobic state to a super-hydrophilic state. After being protected from light or dried, the fabric is transformed from a super-hydrophilic state to a super-hydrophobic state, achieving self-repair.

[0020] Compared with the prior art, the present invention has the following beneficial effects:

[0021] 1. The present invention prepares a fabric with super amphiphobicity, and the wettability of the fabric changes under the irradiation of ultraviolet light.

[0022] 2. The present invention prepares a fabric with self-cleaning ability. Under the irradiation of ultraviolet light, the oxygen vacancies inside the photocatalytic material are transferred, reacting with lattice oxygen to form oxygen vacancies to adsorb hydroxyl radicals, catalytically degrading pollutants attached to the surface of the fabric. At the same time, the fabric is transformed from a super-hydrophobic state to a super-hydrophilic state, achieving self-cleaning.

[0023] 3. The present invention prepares a fabric with a self-repairing effect. The super-hydrophilic fabric can be restored to a super-hydrophobic state by drying for 30-60 minutes or protecting from light for 3-8 days, achieving self-repair and can be reused. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 The scanning electron microscope images are of the original cotton fabric, the modified cotton fabric prepared in Example 1, and the nano-microspheres modified with the photocatalytic nano-array;

[0025] Figure 2 The wettability of the original cotton fabric and the modified cotton fabric prepared in Example 1 to different liquids;

[0026] Figure 3 This is a graph showing the change of the water contact angle of the modified cotton fabric prepared in Example 1 under ultraviolet light over time;

[0027] Figure 4 This is the UV full scan spectrum of the modified cotton fabric prepared in Example 1 that degrades methyl orange;

[0028] Figure 5 The initial water contact angle of the modified cotton fabric prepared in Example 1 (left), the water contact angle after ultraviolet light irradiation (middle), and the water contact angle after dark recovery (right). DETAILED DESCRIPTION

[0029] In order to facilitate the understanding of the present invention, the present invention will be described more fully below. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present invention more thorough and comprehensive.

[0030] Example 1

[0031] (1) 1 g of silica powder (average particle size 10 μm) was dispersed in 10 g of a 20% mass fraction titanium dioxide precursor solution, and after magnetic stirring for 30 minutes, the material was thoroughly washed with toluene and water, respectively, and completely dried. The washing and drying operations were repeated six times to obtain a titanium dioxide seed layer by a sol-gel method; then, the titanium dioxide seed layer was calcined in a muffle furnace at 600°C for 2 hours, and the calcined material was added to a mixed solution of titanium dioxide precursor solution, hydrochloric acid and water. After mixing, the solution was transferred to a stainless steel autoclave lined with polytetrafluoroethylene and subjected to a hydrothermal reaction at 150°C for 6 hours; finally, the obtained sample was washed with deionized water and dried to obtain titanium dioxide nanoarray-modified silica nanospheres, denoted as STNRs; Figure 1 As shown, a titanium dioxide array was observed to grow vertically on the silicon dioxide surface through a scanning electron microscope. The average length of the titanium dioxide nanoarray was about 3 μm and the diameter was about 25 nm, showing a nanoflower shape.

[0032] (2) Take 20 mg of STNRs obtained in step (1), disperse it in 50 mL of aqueous solution, and ultrasonicate for 1 h before use;

[0033] (3) taking a cotton fabric of 3 cm × 3 cm in size, soaking it in a dopamine-tris (0.2 g / L) solution for 3 h, then taking it out and drying it, thereby completing the pretreatment of the cotton fabric;

[0034] (4) soaking the cotton fabric pre-treated in step (3) in the solution prepared in step (2), stirring magnetically at room temperature for 2 hours, then taking it out and drying it, thereby loading the STNRs onto the cotton fabric;

[0035] (5) The cotton fabric obtained in step (4) is immersed in a 12% by volume perfluorodecyltriethoxysilane (17F)-ethanol solution for 7 hours to complete the fluorination, and then the excess 17F is washed away with ethanol, and the modified cotton fabric is obtained after natural drying.

[0036] pass Figure 1 It can be seen that STNRs can be loaded onto the surface of cotton fabric by the impregnation method.

[0037] Compared with the original cotton fabric, the modified cotton fabric has a high liquid repellency. Figure 2 As shown in the figure, the modified cotton fabrics are hydrophobic to different dye solutions. The wettability of the modified cotton fabrics will change under UV light, such as Figure 3 As shown in the figure, under the irradiation of ultraviolet light, the water contact angle of the modified cotton fabric changed from the initial 150.34° to 7.55°, changing from superhydrophobic to superhydrophilic.

[0038] Modified cotton fabrics have self-cleaning properties, such as Figure 4 As shown in the figure, after the modified cotton fabric was contaminated by methyl orange, its absorbance decreased significantly under ultraviolet light, indicating that the modified cotton fabric can achieve self-cleaning by degrading pollutants under ultraviolet light. And as the irradiation time increases, the absorbance becomes lower and lower, indicating that the longer the irradiation time, the more thorough the degradation of pollutants.

[0039] Modified cotton fabrics have self-repairing effects, e.g. Figure 5 As shown in the figure, the water contact angle of the modified cotton fabric changed from 150.34° to 7.55° after ultraviolet irradiation, indicating that the cotton fabric changed from a superhydrophobic state to a superhydrophilic state; after 5 days of dark treatment, the contact angle of the cotton fabric recovered to 149.33°, indicating that the modified cotton fabric has the performance of superhydrophilic-superhydrophobic conversion and can be reused.

[0040] Example 2

[0041] (1) 1 g of calcium oxide powder was dispersed in 15 g of a titanium dioxide precursor solution with a mass fraction of 15%. After magnetic stirring for 30 minutes, the material was thoroughly washed with toluene and water, respectively, and completely dried. The washing and drying operations were repeated six times to obtain a titanium dioxide seed layer by a sol-gel method. Subsequently, the titanium dioxide seed layer was calcined in a muffle furnace at 500° C. for 3 hours, and the calcined material was added to a mixed solution of a titanium dioxide precursor solution, hydrochloric acid and water. After mixing, the solution was transferred to a stainless steel autoclave lined with polytetrafluoroethylene, and a hydrothermal reaction was carried out at 180° C. for 5 hours. Finally, the obtained sample was washed with deionized water and dried to obtain calcium oxide nanospheres modified with titanium dioxide nanoarrays, which were recorded as CTNRs. A vertically grown titanium dioxide nanoarray was formed on the surface of the calcium oxide nanospheres. The average length of the titanium dioxide nanoarray was about 5 μm, showing a nanostructured state.

[0042] (2) taking 30 mg of the CTNRs obtained in step (1), dispersing it into 50 mL of aqueous solution, and ultrasonicating it for 1 h before use;

[0043] (3) taking a cotton fabric of 3 cm × 3 cm in size, soaking it in a dopamine-tris (0.4 g / L) solution for 2 h, then taking it out and drying it, thereby completing the pretreatment of the cotton fabric;

[0044] (4) soaking the cotton fabric pre-treated in step (3) in the solution prepared in step (2), stirring the solution under magnetic stirring at room temperature for 2 hours, and then taking the solution out to dry, so that the CTNRs are evenly loaded on the cotton fabric;

[0045] (5) The cotton fabric obtained in step (4) is immersed in an 8% by volume solution of tridecafluorooctyltriethoxysilane (13F)-ethanol for 8 hours to complete the fluorination, and then the excess 13F is washed away with ethanol, and the modified cotton fabric is obtained after natural drying.

[0046] Example 3

[0047] (1) 1 g of silica powder (average particle size 2 μm) was dispersed in 5 g of a 40% by mass zinc oxide precursor solution, and after magnetic stirring for 30 minutes, the material was thoroughly washed with toluene and water, respectively, and completely dried. The washing and drying operations were repeated six times to obtain a zinc oxide seed layer by a sol-gel method. Subsequently, the zinc oxide seed layer was calcined in a muffle furnace at 700°C for 2 hours, and the calcined material was added to a mixed solution of zinc oxide precursor solution, hydrochloric acid and water. After mixing, the solution was transferred to a stainless steel autoclave lined with polytetrafluoroethylene, and a hydrothermal reaction was carried out at 140°C for 7 hours. Finally, the obtained sample was washed with deionized water and dried to obtain a zinc oxide nanoarray-modified silica nanosphere, which was denoted as SZnNRs. A vertically grown zinc oxide nanoarray was formed on the surface of the silica nanosphere, and the average length of the zinc oxide nanoarray was about 7 μm.

[0048] (2) Take 10 mg of the SZnNRs obtained in step (1), disperse it in 20 mL of aqueous solution, and ultrasonicate for 0.5 h before use;

[0049] (3) taking a cotton fabric of 2 cm × 2 cm in size, soaking it in a dopamine-tris (0.3 g / L) solution for 2 h, then taking it out and drying it, thereby completing the pretreatment of the cotton fabric;

[0050] (4) soaking the cotton fabric pre-treated in step (3) in the solution prepared in step (2), stirring magnetically at room temperature for 2 hours, then taking it out and drying it, thereby loading SZnNRs onto the cotton fabric;

[0051] (5) The cotton fabric obtained in step (4) is immersed in a 5% by volume nonafluorohexyltriethoxysilane (9F)-ethanol solution for 5 hours to complete the fluorination, and then the excess 9F is washed away with ethanol, and the modified cotton fabric is obtained after natural drying.

[0052] Example 4

[0053] (1) 1 g of carbon black powder was dispersed in 18 g of a 12% tin oxide precursor solution, and after magnetic stirring for 30 minutes, the material was thoroughly washed with toluene and water, respectively, and completely dried. The washing and drying operations were repeated six times, and a tin oxide seed layer was prepared by a sol-gel method; then, the tin oxide seed layer was calcined in a muffle furnace at 400°C for 4 hours, and the calcined material was added to a mixed solution of tin oxide precursor solution, hydrochloric acid and water. After mixing, the solution was transferred to a stainless steel autoclave lined with polytetrafluoroethylene, and a hydrothermal reaction was carried out at 100°C for 10 hours; finally, the obtained sample was washed with deionized water and dried to obtain carbon black nanospheres modified with tin oxide nanoarrays, which were denoted as CSnNRs; vertically grown tin oxide nanoarrays were formed on the surface of the carbon black nanospheres, and the average length of the tin oxide nanoarrays was about 10 μm;

[0054] (2) Take 20 mg of the CSnNRs obtained in step (1), disperse it in 50 mL of aqueous solution, and ultrasonicate for 1 h before use;

[0055] (3) taking a cotton fabric of 2 cm×2 cm in size, soaking it in a dopamine-tris (0.2 g / L) solution for 3 h, then taking it out and drying it, thereby completing the pretreatment of the cotton fabric;

[0056] (4) soaking the cotton fabric pre-treated in step (3) in the solution prepared in step (2), stirring magnetically at room temperature for 2 hours, and then taking it out to dry, so that the CSnNRs are evenly loaded on the cotton fabric;

[0057] (5) The cotton fabric obtained in step (4) is immersed in a 15% by volume tridecafluorooctyltriethoxysilane (13F)-ethanol solution for 8 hours to complete the fluorination, and then the excess 13F is washed away with ethanol, and the modified cotton fabric is obtained after natural drying.

[0058] Example 5

[0059] (1) 1 g of polystyrene microspheres were dispersed in 20 g of a zinc sulfide precursor solution with a mass fraction of 10%, and after magnetic stirring for 30 minutes, the material was thoroughly washed with toluene and water, respectively, and completely dried. The washing and drying operations were repeated six times, and a zinc sulfide seed layer was prepared by a sol-gel method; then, the zinc sulfide seed layer was calcined in a muffle furnace at 650°C for 2 hours, and the calcined material was added to a mixed solution of zinc sulfide precursor solution, hydrochloric acid and water. After mixing, the solution was transferred to a stainless steel autoclave lined with polytetrafluoroethylene, and a hydrothermal reaction was carried out at 120°C for 9 hours; finally, the obtained sample was washed with deionized water and dried to obtain polystyrene nanospheres modified with zinc sulfide nanoarrays, which were recorded as PZnNRs; vertically grown zinc sulfide nanoarrays were formed on the surface of the polystyrene nanospheres, and the average length of the zinc sulfide nanoarrays was about 3 μm;

[0060] (2) Take 10 mg of the PZnNRs obtained in step (1), disperse it in 20 mL of aqueous solution, and ultrasonicate for 0.5 h before use;

[0061] (3) taking a cotton fabric of 2 cm × 2 cm in size, soaking it in a dopamine-tris (0.3 g / L) solution for 2 h, then taking it out and drying it, thereby completing the pretreatment of the cotton fabric;

[0062] (4) soaking the cotton fabric pre-treated in step (3) in the solution prepared in step (2), stirring magnetically at room temperature for 1 hour, and then taking it out to dry, so that the PZnNRs are evenly loaded on the cotton fabric;

[0063] (5) The cotton fabric obtained in step (4) is immersed in a 20% by volume perfluorodecyltriethoxysilane (17F)-ethanol solution for 10 hours to complete the fluorination, and then the excess 17F is washed away with ethanol, and the modified cotton fabric is obtained after natural drying.

[0064] The above description is only for better explaining the embodiments of the present invention, and is not intended to limit the present invention. Any modification or equivalent substitution that does not depart from the spirit and scope of the present invention shall fall within the scope of the present invention.

Claims

1. A method for preparing a fabric having self-cleaning function and self-repairing effect, characterized in that: The following steps are involved: Step 1: dispersing nanospheres into a precursor solution of a photocatalytic nanomaterial, stirring evenly, washing, and drying to obtain a photocatalytic nanocrystalline seed layer; calcining and hydrothermally reacting the photocatalytic nanocrystalline seed layer to obtain nanospheres modified with a photocatalytic nanoarray; Step 2: soaking the fabric in a dopamine-tris solution, taking it out and drying it, then soaking it in a dispersion of nano-microspheres modified by a photocatalytic nano-array, taking it out and drying it, to obtain a fabric loaded with nano-microspheres modified by a photocatalytic nano-array; Step 3: fluorination of the fabric surface is completed by dehydration condensation using a fluorinated silicone-ethanol solution, and the fabric is naturally dried to obtain the fabric having self-cleaning and self-repairing effects.

2. The method for preparing a fabric having self-cleaning and self-repairing effects according to claim 1, characterized in that: The nano-microspheres in step 1 are at least one of silicon dioxide particles, calcium oxide particles, carbon black particles, calcium carbonate particles, polytetrafluoroethylene particles, polystyrene microspheres, and polypropylene microspheres; the photocatalytic nano-material is at least one of titanium dioxide, zinc oxide, ferric oxide, cuprous oxide, tungsten trioxide, tin oxide, zirconium dioxide, cadmium sulfide, and zinc sulfide.

3. The method for preparing a fabric having self-cleaning and self-repairing effects according to claim 1, characterized in that: In the step 1, the mass ratio of the nano-microspheres to the photocatalytic nano-material is 1:5-20, and the mass fraction of the precursor solution of the photocatalytic nano-material is 10-50%.

4. The method for preparing a fabric having self-cleaning and self-repairing effects according to claim 1, characterized in that: In the step 1, the calcination temperature is 400-700° C., and the calcination time is 2-4 hours; the hydrothermal reaction temperature is 100-200° C., and the hydrothermal reaction time is 4-10 hours.

5. The method for preparing a fabric having self-cleaning and self-repairing effects according to claim 1, characterized in that: The preparation process of the photocatalytic nanoarray modified nanosphere dispersion in step 2 is: mixing the photocatalytic nanoarray modified nanospheres with water in a ratio of (1-3) mg: (2-10) mL, and ultrasonicating for 0.5-1 h.

6. The method for preparing a fabric with self-cleaning and self-repairing effects according to claim 1, characterized in that: In the step 2, the concentration of the dopamine-tris solution is 0.2-0.4 g / L, and the fabric is immersed in the dopamine-tris solution for 1-3 hours.

7. The method for preparing a fabric with self-cleaning and self-repairing effects according to claim 1, characterized in that: In step 2, the fabric is immersed in the dispersion of nano-microspheres modified with the photocatalytic nano-array for 1 to 2 hours.

8. The method for preparing a fabric with self-cleaning and self-repairing effects according to claim 1, characterized in that: The fluorine-containing siloxane in step 3 is at least one of heptadecafluorodecyltrimethylsiloxane, perfluorodecyltriethoxysilane, tridecafluorooctyltriethoxysilane, nonafluorohexyltriethoxysilane and trifluoropropyltrimethylsiloxane.

9. The method for preparing a fabric with self-cleaning and self-repairing effects according to claim 1, characterized in that: In step 3, the volume fraction of the fluorinated silicone-ethanol solution is 5-20%, and the fluorination time is 2-10 hours.

10. A fabric with self-cleaning function and self-repairing effect prepared by the preparation method according to any one of claims 1 to 9, characterized in that: The surface of the fabric is loaded with nano-microspheres modified with a photocatalytic nano-array and has a super-amphiphobic structure. Under the irradiation of ultraviolet light, the fabric generates superoxide free radicals with strong oxidizing properties, which can oxidize organic pollutants and complete self-cleaning. At the same time, the fabric changes from a super-hydrophobic state to a super-hydrophilic state. After being protected from light or dried, the fabric changes from a super-hydrophilic state to a super-hydrophobic state, achieving self-repair.