Holocellulose, preparation method thereof and method for preparing furan chemicals

The biodegradability of lignocellulose is solved by reacting with lignocellulose using a eutectic solvent of lysine and ethanolamine, combined with a temperature-controlled polyacid catalyst and aluminum chloride to catalyze in methyl isobutyl ketone. and the problem of catalyst recycling, achieving efficient conversion into furan chemicals, improving utilization efficiency and reducing costs.

CN118979404AActive Publication Date: 2024-11-19BEIHUA UNIV
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411065111.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-11-19
Estimated Expiration
2044-08-05

AI Technical Summary

Technical Problem

In the prior art, lignocellulose has strong biodegradability and difficult separation, resulting in low utilization efficiency. In addition, traditional catalytic methods have problems such as acid pollution, equipment corrosion and catalyst recovery difficulties, which affects high-value utilization and production. cost.

Method used

The eutectic solvent composed of lysine and ethanolamine reacts with lignocellulose to prepare cellulose, and the temperature-controlled polyacid catalyst is used to catalyze the reaction at high temperature, recover at low temperature, and combine aluminum chloride and water in methyl isobutyl. Catalytic conversion of ketones into furan chemicals, achieving efficient catalysis and catalyst recovery.

Benefits of technology

The purity and removal rate of lignocellulose are improved, and efficient conversion to furan chemicals is achieved. The catalyst remains high performance after five cycles, reducing production costs and environmental pollution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118979404A_ABST
    Figure CN118979404A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of biomass utilization, and provides holocellulose, a preparation method thereof and a method for preparing furan chemicals. The method provided by the invention comprises the following step: reacting a lignocellulose raw material with a deep eutectic solvent (DES) in a mass ratio of (2-6): 60 to obtain holocellulose. Alkaline DES composed of Lys and MEA achieves the optimal treatment effect on the larch raw material, and the high-purity larch holocellulose and lignin removal rate is obtained; a double-acid catalysis system composed of heteropoly acid and AlCl3 catalyzes conversion of larch holocellulose into furan chemicals in a double-phase solvent composed of water and methyl isobutyl ketone (MIBK), efficient conversion of holocellulose is achieved, and the yield of 5-hydroxymethylfurfural (HMF) and furfural (FF) is high; the polyacid catalyst and the aqueous solution of AlCl3 are recycled, and high catalytic performance is still kept after five times of recycling.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of biomass utilization, and in particular to holocellulose and a preparation method thereof, and a method for preparing furan chemicals. Background Art

[0002] A large amount of agricultural and forestry waste is generated during the production process of agriculture and forest product processing industry. At present, the utilization efficiency of these agricultural and forestry wastes rich in lignocellulose is not high. They are mainly used through incineration to generate heat, composting and other methods. The utilization value is low and it will also pollute the environment. Collecting wood resource residues and further transforming them into high value-added products such as liquid fuels, pharmaceutical products and platform chemicals will greatly improve the utilization efficiency of wood resources, effectively avoid resource waste, and also conform to the research trend of coordinated planning of biomass production and utilization efficiency. In order to improve the utilization efficiency of lignocellulose, it is necessary to solve the problems of strong biological resistance to degradation and difficulty in separation of lignocellulose to meet the needs of high-value utilization and development of lignocellulose biomass.

[0003] Among the traditional treatment methods, physical methods are simple to operate, fast in time, and less polluting, especially microwave methods, which greatly shorten the treatment time. However, physical methods have problems such as high equipment cost and energy consumption, as well as potential safety hazards. Biological methods for degrading and separating lignocellulosic components have advantages such as low cost and energy consumption, strong specificity, and mild conditions, but they also have disadvantages such as long treatment cycle, low bioenzyme yield and treatment efficiency. Chemical pretreatment has good treatment effects, but has high requirements for the corrosion resistance of treatment equipment, and solvent recovery is difficult, which can easily cause environmental pollution. Deep eutectic solvents (DES) can overcome the shortcomings of chemical methods, biological methods, and other methods to a certain extent, and can be used to treat lignocellulosic biomass.

[0004] 5-Hydroxymethylfurfural (HMF) is widely considered to be a key factor in narrowing the gap between fossil economy and sustainable economy; furfural (FF) was selected as one of the top 30 biomass-derived platform compounds based on multiple indicators such as raw materials, processing costs, technical complexity and market potential. The traditional method of preparing HMF and FF from biomass is mainly dilute acid catalysis. Dilute acid solutions (such as low-concentration HCl, H2SO4 and other solutions) are suitable for the depolymerization of cellulose and hemicellulose, but they will produce a large amount of acidic pollutants and equipment corrosion. Due to the strong acidity of heteropolyacids (HPA), H3PW 12 O 40 HPA represented by is used to prepare furfural compounds. In addition, homogeneous catalysts have the disadvantage of being difficult to recycle, which is not conducive to controlling production costs; heterogeneous catalysts also have the disadvantage of low mass transfer efficiency.

[0005] Therefore, the temperature-controlled catalyst combined with HPA dissolves at high temperature to achieve homogeneous reaction and precipitates at low temperature to achieve recovery. It is of great significance to achieve catalyst recovery while achieving efficient catalytic reaction. Summary of the invention

[0006] The object of the present invention is to provide a holocellulose and a preparation method thereof and a method for preparing furan chemicals in order to overcome the deficiencies of the prior art.

[0007] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0008] The present invention provides a method for preparing holocellulose, comprising the following steps:

[0009] The lignocellulose raw material and the deep eutectic solvent are reacted to obtain holocellulose;

[0010] The mass ratio of the lignocellulose raw material to the low eutectic solvent is 2-6:60; the low eutectic solvent consists of lysine and ethanolamine.

[0011] Preferably, the reaction temperature is 80-120° C., and the reaction time is 6-9 h.

[0012] Preferably, the reaction mixture obtained from the reaction is subjected to solid-liquid separation, and the filter residue after separation is washed and dried in sequence to obtain holocellulose.

[0013] Preferably, the washing reagents are acetone aqueous solution and water in sequence, and the volume ratio of acetone to water in the acetone aqueous solution is 6-8:2-4; the drying temperature is 70-90°C.

[0014] The invention also provides holocellulose prepared by the preparation method.

[0015] The present invention also provides a method for preparing furan chemicals from the holocellulose, comprising the following steps: reacting holocellulose, aluminum chloride, a polyacid catalyst, water and methyl isobutyl ketone to obtain furan chemicals.

[0016] Preferably, the mass ratio of the holocellulose, aluminum chloride and polyacid catalyst is 1:0.15-0.25:0-3; and the volume ratio of water and methyl isobutyl ketone is 1-4:6-19.

[0017] Preferably, the reaction temperature is 120-170° C., the reaction time is 7-12 h, and the reaction is carried out under stirring at a rate of 400-600 rpm.

[0018] Preferably, the polyacid catalyst is a temperature-controlled polyacid catalyst, and the chemical formula of the temperature-controlled polyacid catalyst is Ch n H3-n PW 12 O 40 , where n is 1, 2 or 3.

[0019] Preferably, the preparation method of the temperature-controlled polyacid catalyst is: adding a choline chloride aqueous solution dropwise to a phosphotungstic acid aqueous solution for reaction to obtain a solid precipitate, washing the solid precipitate and drying it to obtain a temperature-controlled polyacid catalyst;

[0020] The molar ratio of choline chloride to phosphotungstic acid is 1-3:1; the concentration of the choline chloride aqueous solution is 0.15-0.25 mol / L, and the concentration of the phosphotungstic acid aqueous solution is 0.04-0.06 mol / L.

[0021] The beneficial effects of the present invention include the following:

[0022] The method of the present invention uses alkaline DES composed of Lys and MEA to achieve the best treatment effect on larch raw materials, and obtains larch holocellulose with high purity and lignin removal rate; the double acid catalytic system composed of heteropoly acid and AlCl3 catalyzes the conversion of larch holocellulose into furan chemicals in a two-phase solvent composed of water and MIBK, and the holocellulose is efficiently converted, and the HMF and FF yields are high; the polyacid catalyst and the aqueous solution of AlCl3 are recycled and reused, and still maintain a high catalytic performance after five cycles of use. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 These are SEM images of the larch raw material and holocellulose of Example 1, wherein a and c are larch raw materials at different magnifications, and b and d are larch holocellulose at different magnifications;

[0024] Figure 2 This is a cyclic performance diagram of the yield and conversion rate of preparing furan chemicals by catalyzing the temperature-controlled multi-acid catalyst of Example 1 with holocellulose. DETAILED DESCRIPTION

[0025] The present invention provides a method for preparing holocellulose, comprising the following steps:

[0026] The lignocellulose raw material is reacted with a deep eutectic solvent (DES) to obtain holocellulose;

[0027] The mass ratio of the lignocellulose raw material to DES is 2-6:60; and the DES consists of lysine and ethanolamine.

[0028] In the present invention, the mass ratio of the lignocellulose raw material to DES is preferably 3 to 5:60, and more preferably 4:60.

[0029] In the DES of the present invention, the molar ratio of lysine (Lys) to ethanolamine (MEA) is preferably 1:5-7.

[0030] In the present invention, the reaction temperature is preferably 80-120°C, more preferably 90-110°C, and more preferably 100°C; the reaction time is preferably 6-9h, and more preferably 7-8h; and the reaction is carried out under stirring.

[0031] In the present invention, the reaction mixture obtained by the reaction is preferably subjected to solid-liquid separation, and the filter residue after separation is preferably washed and dried in sequence to obtain holocellulose.

[0032] In the present invention, the washing reagents are preferably acetone aqueous solution and water in sequence. In the acetone aqueous solution, the volume ratio of acetone to water is preferably 6-8:2-4, and more preferably 7:3. The purpose of washing with acetone aqueous solution is to remove residual DES, and washing with water makes the filter residue neutral.

[0033] In the present invention, the drying temperature is preferably 70 to 90° C., more preferably 75 to 85° C., and more preferably 80° C.; the drying is preferably vacuum drying.

[0034] The invention also provides holocellulose prepared by the preparation method.

[0035] The present invention also provides a method for preparing furan chemicals from the holocellulose, comprising the following steps: reacting holocellulose, aluminum chloride, a polyacid catalyst, water and methyl isobutyl ketone (MIBK) to obtain furan chemicals.

[0036] In the present invention, the mass ratio of the holocellulose, aluminum chloride and polyacid catalyst is preferably 1:0.15-0.25:0-3, more preferably 1:0.18-0.22:1-2, and more preferably 1:0.2:1.5; the volume ratio of water and MIBK is preferably 1-4:6-19, more preferably 2-3:8-15, and more preferably 2.5:10-13.

[0037] In the present invention, the reaction temperature is preferably 120-170°C, more preferably 130-160°C, more preferably 140-150°C; the reaction time is preferably 7-12h, more preferably 8-11h, more preferably 9-10h; the reaction is preferably carried out under stirring conditions, and the stirring rate is preferably 400-600rpm, more preferably 450-550rpm, more preferably 500rpm.

[0038] In the present invention, the polyacid catalyst is preferably a temperature-controlled polyacid catalyst, and the chemical formula of the temperature-controlled polyacid catalyst is preferably Ch n H 3-n PW12 O 40 , where n is 1, 2 or 3.

[0039] In the present invention, the preparation method of the temperature-controlled polyacid catalyst is as follows: adding a choline chloride aqueous solution dropwise into a phosphotungstic acid aqueous solution for reaction to obtain a solid precipitate, washing the solid precipitate and drying it to obtain a temperature-controlled polyacid catalyst;

[0040] The molar ratio of choline chloride to phosphotungstic acid is preferably 1-3:1, more preferably 1:1, 2:1 or 3:1; the concentration of the choline chloride aqueous solution is preferably 0.15-0.25 mol / L, more preferably 0.18-0.22 mol / L, more preferably 0.2 mol / L; the concentration of the phosphotungstic acid aqueous solution is preferably 0.04-0.06 mol / L, more preferably 0.045-0.055 mol / L, more preferably 0.05 mol / L.

[0041] In the present invention, the reaction temperature is preferably room temperature, the reaction time is preferably 10 to 14 hours, more preferably 11 to 13 hours, more preferably 12 hours; the drying time is preferably 10 to 14 hours, more preferably 11 to 13 hours, more preferably 12 hours.

[0042] In the present invention, the mixture obtained by the reaction is preferably centrifuged to obtain three layers, the upper layer is an organic phase containing furan, the middle layer is an aqueous phase, and the lower layer is a solid residue and a catalyst.

[0043] In the present invention, the solid residue and the catalyst are preferably stirred and then filtered while hot, and the filtered residue is washed and then dried. The stirring temperature is preferably 70 to 90°C, more preferably 75 to 85°C, and even more preferably 80°C.

[0044] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.

[0045] Example 1

[0046] Preparation of alkaline DES: Lys and MEA in a molar ratio of 1:6 were mixed in a round-bottom flask, placed in a constant temperature magnetic stirring bath and stirred at 80°C at a speed of 500 rpm until a uniform transparent liquid was formed. The alkaline DES solvent was cooled to room temperature and stored in a desiccator for use.

[0047] Preparation of larch holocellulose: 4 g larch raw material and 60 g alkaline DES solvent were placed in a round-bottom flask and mixed evenly, and the mixture was stirred at 100 ° C and 500 rpm for 8 h. After the reaction was completed, it was quickly cooled to room temperature, and the reaction mixture was separated from the solid by suction filtration (pressure of 0.5 MPa). The filter residue was fully washed with acetone aqueous solution (the volume ratio of acetone to water was 7:3) to remove the residual DES solvent, and then the filter residue was washed with deionized water until it was neutral. The collected washed filter residue was transferred to a vacuum drying oven (vacuum degree of 0.05 MPa) and dried at 80 ° C to obtain larch holocellulose.

[0048] Temperature controlled polyacid catalyst ChH2PW 12 O 40 Synthesis: Dissolve 1 mmol of choline chloride in 5 mL of deionized water and stir until the choline chloride is completely dissolved. 12 O 40 Dissolve in 20 mL of deionized water and stir until H3PW 12 O 40 The choline chloride aqueous solution was then added dropwise to the H3PW at a rate of 10 mL / min. 12 O 40 The mixture was stirred at room temperature for 12 h, and then filtered to separate the white solid precipitate, which was washed three times with deionized water. The white solid precipitate was placed in a vacuum drying oven (vacuum degree of 0.05 MPa) and dried for 12 h to obtain ChH2PW 12 O 40 catalyst.

[0049] Preparation of furan chemicals: Add 0.1g of holocellulose, 0.02g of AlCl3, 0.15g of catalyst, 10mL of deionized water and MIBK into the reactor (the volume ratio of deionized water to MIBK is 2.5:13), and stir the reaction at 150℃ and 500rpm for 9h. After the reaction, quickly cool to room temperature and centrifuge the mixture. After centrifugation, the reaction mixture is divided into three layers: the upper layer is the organic phase containing the product, the middle layer is the aqueous phase, and the lower layer is the solid residue and catalyst. The solid residue and catalyst are placed in hot water at 85℃, stirred and filtered while hot, and the filter residue is washed, dried, and weighed to calculate the conversion rate of holocellulose. Catalyst precipitation occurs when the hot aqueous solution is cooled to room temperature. The catalyst can be washed and dried for recycling.

[0050] Example 2

[0051] Preparation of alkaline DES: Lys and MEA in a molar ratio of 1:6 were mixed in a round-bottom flask, placed in a constant temperature magnetic stirring bath and stirred at 450 rpm at 80°C until a uniform transparent liquid was formed. The alkaline DES solvent was cooled to room temperature and stored in a desiccator for later use.

[0052] Preparation of larch holocellulose: 3g larch raw material and 60g alkaline DES solvent were placed in a round-bottom flask and mixed evenly, and the mixture was stirred continuously at 90°C and 450rpm for 9h. After the reaction was completed, it was quickly cooled to room temperature, and the reaction mixture was filtered (pressure was 0.5MPa) for solid-liquid separation. The filter residue was fully washed with acetone aqueous solution (volume ratio of acetone to water was 6:2) to remove the residual DES solvent, and then the filter residue was washed with deionized water until it was neutral. The collected washed filter residue was transferred to a vacuum drying oven (vacuum degree was 0.05MPa) and dried at 75°C to obtain larch holocellulose.

[0053] Temperature controlled polyacid catalyst Ch2HPW 12 O 40 Synthesis: Dissolve 2 mmol of choline chloride in 10 mL of deionized water and stir until choline chloride is completely dissolved. 12 O 40 Dissolve in 20 mL of deionized water and stir until H3PW 12 O 40 The choline chloride aqueous solution was then added dropwise to the H3PW at a rate of 10 mL / min. 12 O 40 The mixture was stirred at room temperature for 11 h, and then filtered to separate the white solid precipitate, which was washed 4 times with deionized water. The white solid precipitate was placed in a vacuum drying oven (vacuum degree of 0.05 MPa) and dried for 12 h to obtain Ch2HPW 12 O 40 catalyst.

[0054] Preparation of furan chemicals: Add 0.1g of holocellulose, 0.018g of AlCl3, 0.1g of catalyst, 10mL of deionized water and MIBK into the reactor (the volume ratio of deionized water to MIBK is 2:8), and stir the reaction at 130℃ and 450rpm for 10h. After the reaction, quickly cool to room temperature and centrifuge the mixture. After centrifugation, the reaction mixture is divided into three layers: the upper layer is the organic phase containing the product, the middle layer is the aqueous phase, and the lower layer is the solid residue and catalyst. The solid residue and catalyst are placed in hot water at 80℃, stirred and filtered while hot, and the filter residue is washed, dried, and weighed to calculate the conversion rate of holocellulose. Catalyst precipitation occurs when the hot aqueous solution is cooled to room temperature. The catalyst can be washed and dried for recycling.

[0055] Example 3

[0056] Preparation of alkaline DES: Lys and MEA in a molar ratio of 1:6 were mixed in a round-bottom flask, placed in a constant temperature magnetic stirring bath and stirred at 80°C at a speed of 550 rpm until a uniform transparent liquid was formed. The alkaline DES solvent was cooled to room temperature and stored in a desiccator for use.

[0057] Preparation of larch holocellulose: 5g larch raw material and 60g alkaline DES solvent were placed in a round-bottom flask and mixed evenly, and the mixture was stirred continuously at 110°C and 550rpm for 7h. After the reaction was completed, it was quickly cooled to room temperature, and the reaction mixture was separated from the solid by suction filtration (pressure was 0.5MPa). The filter residue was fully washed with acetone aqueous solution (volume ratio of acetone to water was 7:4) to remove the residual DES solvent, and then the filter residue was washed with deionized water until it was neutral. The collected washed filter residue was transferred to a vacuum drying oven (vacuum degree was 0.05MPa) and dried at 85°C to obtain larch holocellulose.

[0058] Temperature controlled polyacid catalyst Ch3PW 12 O 40 Synthesis: Dissolve 3 mmol of choline chloride in 15 mL of deionized water and stir until choline chloride is completely dissolved. 12 O 40 Dissolve in 20 mL of deionized water and stir until H3PW 12 O 40 The choline chloride aqueous solution was then added dropwise to the H3PW at a rate of 10 mL / min. 12 O 40 The mixture was stirred at room temperature for 13 h, and then filtered to separate the white solid precipitate, which was washed three times with deionized water. The white solid precipitate was placed in a vacuum drying oven (vacuum degree of 0.05 MPa) and dried for 12 h to obtain Ch3PW 12 O 40 catalyst.

[0059] Preparation of furan chemicals: Add 0.1g of holocellulose, 0.022g of AlCl3, 0.2g of catalyst, 10mL of deionized water and MIBK into the reactor (the volume ratio of deionized water to MIBK is 3:15), and stir the reaction at 170℃ and 550rpm for 8h. After the reaction, quickly cool to room temperature and centrifuge the mixture. After centrifugation, the reaction mixture is divided into three layers: the upper layer is the organic phase containing the product, the middle layer is the aqueous phase, and the lower layer is the solid residue and catalyst. The solid residue and catalyst are placed in hot water at 85℃, stirred and filtered while hot, and the filter residue is washed, dried, and weighed to calculate the conversion rate of holocellulose. Catalyst precipitation occurs when the hot aqueous solution is cooled to room temperature. The catalyst can be washed and dried for recycling.

[0060] The SEM images of the larch raw material and holocellulose of Example 1 are as follows: Figure 1 As shown, a and c are larch raw materials at different magnifications, and b and d are larch holocellulose at different magnifications;

[0061] The yield and conversion rate of the preparation of furan chemicals by the temperature-controlled polyacid catalyst of Example 1 are as follows: Figure 2 As shown. Figure 2 It can be seen that the dual acid catalytic system composed of heteropolyacid and AlCl3 catalyzes the conversion of larch holocellulose into furan chemicals in a biphasic solvent composed of water and MIBK. The holocellulose is efficiently converted, and the yields of HMF and FF are high. The polyacid catalyst and the aqueous solution of AlCl3 are recycled and reused, and still maintain a high catalytic performance after five cycles of use.

[0062] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing holocellulose, characterized in that: The following steps are included: The lignocellulose raw material and the deep eutectic solvent are reacted to obtain holocellulose; The mass ratio of the lignocellulose raw material to the low eutectic solvent is 2-6:60; the low eutectic solvent consists of lysine and ethanolamine.

2. The preparation method according to claim 1, characterized in that: The reaction temperature is 80-120° C., and the reaction time is 6-9 hours.

3. The preparation method according to claim 1 or 2, characterized in that: The reaction mixture obtained by the reaction is subjected to solid-liquid separation, and the filter residue after separation is washed and dried in sequence to obtain holocellulose.

4. The preparation method according to claim 3, characterized in that: The washing reagents are acetone aqueous solution and water in sequence, and the volume ratio of acetone to water in the acetone aqueous solution is 6-8:2-4; the drying temperature is 70-90°C.

5. Holocellulose prepared by the preparation method according to any one of claims 1 to 4.

6. The method for preparing furan chemicals from holocellulose according to claim 5, characterized in that: The method comprises the following steps: reacting holocellulose, aluminum chloride, a polyacid catalyst, water and methyl isobutyl ketone to obtain furan chemicals.

7. The method according to claim 6, characterized in that The mass ratio of the holocellulose, aluminum chloride and polyacid catalyst is 1:0.15-0.25:0-3; the volume ratio of water and methyl isobutyl ketone is 1-4:6-19.

8. The method according to claim 6 or 7, characterized in that: The reaction temperature is 120-170° C., the reaction time is 7-12 hours, and the reaction is carried out under stirring conditions at a stirring rate of 400-600 rpm.

9. The method according to claim 8, characterized in that The polyacid catalyst is a temperature-controlled polyacid catalyst, and the chemical formula of the temperature-controlled polyacid catalyst is Ch n H 3-n PW 12 O 40 , where n is 1, 2 or 3.

10. The method according to claim 9, characterized in that The preparation method of the temperature-controlled polyacid catalyst comprises: adding a choline chloride aqueous solution dropwise into a phosphotungstic acid aqueous solution for reaction to obtain a solid precipitate, washing the solid precipitate and drying it to obtain the temperature-controlled polyacid catalyst; The molar ratio of choline chloride to phosphotungstic acid is 1-3:1; the concentration of the choline chloride aqueous solution is 0.15-0.25 mol / L, and the concentration of the phosphotungstic acid aqueous solution is 0.04-0.06 mol / L.

Citation Information

Patent Citations

  • Method for pretreating lignocellulose by adopting alkaline eutectic solvent

    CN108441530A

  • Method for preparing nanocellulose and lignin by adopting biomass one-pot method

    CN116356596A

  • Process for isolating cellulose from cellulosic biomass, isolated cellulose of type i and composite materials comprising same

    US20150361616A1