Method for detecting internal defects of aviation carbon fiber composite wallboard

Through the automated fusion phased array ultrasonic system, combined with linear array phased array probe and Ω-shaped water-immersed probe boot, the problem of detection of small and medium-sized defects and signal interference is solved, and the carbon fiber composite wall panels are efficient and fast , accurate detection.

CN118980746APending Publication Date: 2024-11-19SHENYANG AIRCRAFT CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411217670.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-02
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The existing ultrasonic detection methods are difficult to effectively detect small-size defects in carbon fiber composite wall panels, and there are signal interference problems caused by water flow injection and mechanical shaft movement, which affects detection efficiency and imaging resolution.

Method used

Adopt an automated fusion phased array ultrasonic system, through the combination of linear array phased array probes and Ω-shaped water-immersed probe boots, the synchronization of electronic scanning and mechanical scanning is achieved, ensuring that the probe and the part curvature match, and a reasonable probe chip is set up. Quantity, water layer thickness and mechanical scanning parameters to improve detection efficiency and imaging resolution.

Benefits of technology

It realizes efficient and rapid detection of carbon fiber composite wall panels, improves the detection sensitivity and imaging resolution of small-sized defects, avoids signal interference caused by water flow and mechanical movement, and meets the real-time online detection requirements for complex structures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118980746A_ABST
    Figure CN118980746A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of wallboard detection, and discloses a method for detecting internal defects of an aviation carbon fiber composite wallboard. The linear array phased array probe is mounted in a probe boot filled with water, the outer edge of the probe boot is in direct contact with the surface of a to-be-detected part, and the curvature of the outer edge is matched with that of the part; the linear array phased array probe electronically controls ultrasonic beams, and water in a probe boot enters a part, so that ultrasonic beam electronic scanning of a probe coverage area is realized; and the mechanical scanning device carries the phased array probe boot to carry out grating type mechanical scanning on the surface of the part to be detected. A good coupling effect is guaranteed, the thickness of the water layer of the probe boot is large enough, and the influence of a water-part secondary interface signal on a part ultrasonic signal is avoided. According to the pulse repetition frequency of a phased array ultrasonic system, the number of probe wafers and phase control parameters, mechanical scanning of an automatic system and mechanical parameters such as the stepping direction, the line stepping, the point stepping and the scanning speed are designed in a fused mode, and it is guaranteed that no data is lost in the scanning process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of wall panel detection, and in particular to a method for detecting internal defects of an aviation carbon fiber composite material wall panel. Background Art

[0002] Carbon fiber composite materials have high specific strength and specific modulus, good fatigue resistance, shock absorption, high temperature resistance, molding processability and damage safety. They are multi-functional and multi-purpose functional materials and structural materials. In recent years, with the increase in the proportion of carbon fiber composite materials in aviation structures and the increasingly complex structure of carbon fiber composite materials, the internal quality of carbon fiber composite materials is closely related to the service safety of aircraft. Aircraft manufacturers have higher requirements for non-destructive testing methods of carbon fiber composite materials: efficient, fast, and suitable for real-time and online detection of complex structures.

[0003] Ultrasonic testing is a commonly used method for non-destructive testing of carbon fiber composite materials. For carbon fiber composite parts in the manufacturing stage, automated imaging testing is preferred. The common ultrasonic automated testing method is the non-contact water spray penetration method, that is, the detection system has two probes, which are placed on both sides of the part. The probes are installed inside the nozzle. The ultrasonic wave emitted by one probe enters the part through the water sprayed from the nozzle, and the other probe receives the ultrasonic wave from the part through the water sprayed from the nozzle. The system strictly matches the received ultrasonic wave with the position information of the inspected part to form a two-dimensional grayscale image with grayscale corresponding to ultrasonic attenuation.

[0004] The above method has the following disadvantages: 1) It can only provide the ultrasonic attenuation characteristics caused by the internal discontinuity of the part, without the depth information of the discontinuity; 2) The splashes formed by the water jet and the recoil on the surface of the part affect the attenuation of the ultrasonic wave, which is easily displayed as abnormal grayscale in the image; 3) When the mechanical axis carries the ultrasonic probe and the probes on both sides are not well aligned, it will affect the attenuation of the ultrasonic signal at the receiving end, which is easy to cause abnormal grayscale in the ultrasonic image; 4) Most importantly, in order to improve the detection efficiency, the nozzle size equipped for water jet detection is generally equivalent to the minimum size defect required to be detected. Due to the diffusion characteristics of ultrasonic propagation, the size of the ultrasonic field entering the part is often larger than the minimum size defect required to be found, making it difficult to find small defects, or the imaging resolution and quantitative accuracy of small defects are not high.

[0005] Phased array ultrasonic testing has become a hot research topic in ultrasonic testing in recent years due to its advantages such as high efficiency and dynamically controllable sound beam. The phased array probe is a combination of a series of small chips, which can realize electronic scanning by electronically controlling multiple chips to transmit and receive signals. Its scanning speed is an order of magnitude faster than the automated mechanical scanning of traditional single-channel probes, which can greatly improve the detection efficiency. Studies have shown that for an array probe containing 128 chips (chip width 0.3mm), the sound beam coverage width of a single-line scan can reach 20mm, and the automated scanning speed is about 300mm / s. In theory, its detection efficiency is 4 times that of the automated mechanical scanning detection efficiency of traditional single-channel probes. And because the phased array sound beam is controllable, a higher imaging resolution can be achieved, which has advantages in the quantification of small-sized defects.

[0006] Aviation carbon fiber composite panels are made of carbon fiber prepregs that are stacked layer by layer according to certain rules and cured in an autoclave. Common internal defects include delamination, pores, debonding, inclusions, etc. Most of the above defects are area defects, and their ultrasonic detection is special. It is necessary to design a phased array ultrasonic detection process based on the part structure and detection characteristics.

[0007] In addition, for large composite wall panel parts, the use of automated fusion phased array ultrasonic detection technology needs to consider the mutual influence of phase control parameters, mechanical motion parameters, and data acquisition parameters. Under the premise of meeting the detection sensitivity, the imaging resolution and thus the quantitative accuracy can be improved, while achieving more efficient automated detection. Summary of the invention

[0008] The present invention proposes a method for detecting internal defects of aviation carbon fiber composite material panels, which realizes internal defect detection of aviation carbon fiber composite material panels based on an automated fusion phased array ultrasonic system. Specifically, an automated-phased array ultrasonic combination technology is used to detect carbon fiber composite material panels, and principles for selecting probes and probe shoes, as well as principles for fusion setting of phased array parameters and mechanical motion parameters are proposed.

[0009] The technical solution of the present invention is as follows: a method for detecting internal defects of aviation carbon fiber composite material wall panels, wherein a linear array phased array probe is installed in a probe boot filled with water, the outer edge of the probe boot is in direct contact with the surface of the part to be inspected and its curvature matches the curvature of the part; an electronically controlled ultrasonic beam emitted by the linear array phased array probe enters the interior of the part through the water inside the probe boot, thereby realizing electronic scanning of the ultrasonic beam in the area covered by the probe; a mechanical scanning device of the automated detection system carries the phased array probe boot to perform a grid-type mechanical scan on the surface of the part to be inspected.

[0010] The linear array phased array probe A is composed of a plurality of probe chips arranged in parallel; the number of probe chips N is selected according to the following formula: N×a+(N-1)×g≤R p / 20; a is the size of a single probe wafer along the wafer arrangement direction, that is, the wafer width; g is the distance between the edges of two adjacent wafers along the wafer arrangement direction; R p is the part curvature.

[0011] The frequency of the linear array phased array probe is 5 MHz.

[0012] The probe shoe 9 is an Ω-shaped water-immersion probe shoe. The curvature of the outer edge of the probe shoe matches the curvature R of the part. The linear array phased array probe is built into the probe shoe. During detection, the inside of the probe shoe is filled with water, and the water layer thickness H w Select according to the following formula: 0.3D w ≤H w ≤0.6D w ;D w is the length of the ultrasonic near field in water.

[0013] The ultrasonic sound beam is a longitudinal wave direct incident sound beam detection, and the scanning mode is set to 0° linear electronic scanning.

[0014] The direction of linear electronic scanning of the sound beam inside the linear array phased array probe (which is also the arrangement direction of the linear array probe chips, and the electronic scanning of the phased array sound beam is performed along the chip arrangement direction) is consistent with the stepping direction of the mechanical scanning device.

[0015] The number of chips n excited at one time in the linear array phased array probe affects the display ratio of defect imaging in the two-dimensional direction and the focal size of the focused acoustic beam. n needs to satisfy the following two formulas at the same time:

[0016]

[0017] [n×a+(n-1)g]×H p ÷4D p ≤Φ min / 2

[0018] Where, b is the length of a single wafer; H p is the thickness of the part; D p is the length of the ultrasonic near field in the part; Φ min The minimum defect size required to be detected on a part.

[0019] The electronic scanning chip step number η setting principle satisfies the following formula: (g+a)×η≤Φ min / 2, the electronic scanning chip step number is the number of chips between two adjacent sound beam groups that perform linear electronic scanning according to sequence excitation.

[0020] The automated inspection system carries a linear array phased array probe to perform grid scanning on the surface of the composite material part, with the scanning direction being the length direction of the part and the stepping direction being the width direction of the part.

[0021] The automated scanning step L of the automated detection system is calculated as follows:

[0022] L=ε×[(g+a)×η]×[(Ν-n)÷η+1]

[0023] Among them, ε is a constant not greater than 1, which is used to eliminate the poor imaging effect caused by the poor edge coupling of the linear array phased array probe;

[0024] The automatic scanning point step S is calculated as follows:

[0025] S=(g+a)×η

[0026] Automatic scanning speed ν s Calculate as follows:

[0027]

[0028] PRF is the pulse repetition frequency of the phased array ultrasound system.

[0029] The beneficial effects of the present invention are as follows: the selected linear array phased array probe is suitable for anisotropic carbon fiber composite materials, the probe frequency and probe size can ensure strong penetration ability, and at the same time, the number of probe chips is large, and the scanning width is large at one time, which can achieve high-efficiency detection of composite material wall panels; the Ω-shaped immersion probe shoe matches the curvature of the part to ensure a good coupling effect, and the thickness of the water layer in the probe shoe is large enough to avoid the influence of the water-part secondary interface signal on the part ultrasonic signal; according to the planned placement direction of the linear array phased array probe and the electronic linear scanning direction, it can match the mechanical scanning direction of the automation system to achieve large-size wall panel parts. Rapid imaging detection; the chip stepping resolution of phased array electronic linear scanning is equivalent to that of automated mechanical scanning, the overall imaging resolution of the parts is uniform, and the imaging is not distorted; the ultrasonic sound beam of phased array electronic linear scanning has focusing characteristics, and the focal size is not greater than half of the minimum required defect size of the part, and has high detection sensitivity; the phased array probe covers a wide area, and combined with the automated detection system, the automated mechanical scanning single-line scanning width is large and the detection efficiency is high; set a reasonable ε value, which is generally between 0.6 and 0.9, so that the edge coupling poor area is removed and a higher detection efficiency can be obtained. The central sound beam is used for imaging detection to avoid poor coupling at the edge of the water boot and ensure excellent imaging effect; the mechanical scanning line stepping ensures scanning coverage, and there is no missed detection between scanning lines; according to the pulse repetition frequency of the phased array ultrasonic system, the number of probe chips, and the phased parameters, the mechanical scanning point stepping and scanning speed of the integrated design automation system can ensure that no data is lost during the scanning process. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1It is a schematic diagram of the placement of the phased array linear array probe and the scanning direction and stepping direction of the grid-type mechanical scanning during detection.

[0031] Figure 2 Schematic diagram of the contact between the probe shoe of the linear array probe and the part.

[0032] Among them: 1 is the direction of arrangement of all ultrasonic chips inside the phased array linear array probe, 2 is the scanning direction of the grid-type mechanical scanning, 3 is the stepping direction of the grid-type mechanical scanning, 4 is the length direction of the part, 5 is the width direction of the part, A is the linear array phased array probe, and B is the composite wall panel part. 6 is the front opening of the probe shoe; 7 is the phased array probe cable; 8 is the water injection hole; 9 is the probe shoe; 10 is the front end of the probe shoe. DETAILED DESCRIPTION

[0033] The method for detecting internal defects of aviation carbon fiber composite wall panels proposed in the present invention is an automated-phased array ultrasonic combination technology. Its coupling method is different from the traditional method of directly using water as a coupling agent. The coupling method in this patent application is a modified water immersion method, specifically: the linear array phased array probe is installed in a probe shoe filled with water, and the outer edge of the probe shoe is in direct contact with the surface of the part and its curvature matches the curvature of the part. The material of the probe shoe is selected to be soft and not easy to wear.

[0034] The linear array phased array probe A is connected to the phased array probe cable 7. The linear array phased array probe A is built into the probe shoe 9. The probe shoe 9 is connected to the water injection system and is ensured to be filled with water at all times through the water injection hole 8 (the ultrasonic wave emitted by the probe is transmitted to the inside of the part through the water); the probe shoe 9 is made of soft plastic and contacts the surface of the composite part B without damaging or scratching the part; the front end 10 of the probe shoe can be replaced to adapt to the curvature of the part.

[0035] The placement direction of the linear array phased array probe A and the mechanical structure perform grid scanning. The grid scanning has a scanning direction 2 and a stepping direction 3 of the grid mechanical scanning, and the two are perpendicular to each other.

[0036] The length of the opening 6 at the front end of the probe shoe is equal to the length of the phased array linear array probe, and the width of the hole is equal to the width of the phased array linear array probe, so that the ultrasonic wave emitted by the probe can be transmitted to the part.

[0037] The electronically controlled ultrasonic beam emitted by the linear array phased array probe enters the part through the water inside the probe shoe, realizing the electronic scanning of the ultrasonic beam in the probe coverage area. The mechanical scanning device of the automated inspection system carries the phased array probe shoe to perform a grid-type mechanical scan on the surface of the part.

[0038] According to the part structure and detection requirements as well as the phased array detection principle, this technical solution is mainly divided into two parts. The first part is to select a suitable phased array probe and probe shoe; the second part is to integrate the setting of phased array parameters and mechanical scanning parameters.

[0039] For the convenience of description, various identifiers used in the present invention and their representative contents are shown in Table 1.

[0040] Table 1 Logo and its representative content

[0041]

[0042] Part 1: Principles for selecting probes and probe shoes

[0043] (1.1) By using a linear array phased array probe, electronic linear scanning of the ultrasonic focused sound beam can be performed along the arrangement direction of the probe chips, realizing rapid imaging detection of aviation carbon fiber composite material sidings.

[0044] (1.2) Probe frequency selection: Carbon fiber composite materials are anisotropic materials with large ultrasonic attenuation, so it is not suitable to use higher frequency detection. However, due to the small thickness of the carbon fiber ply, it is required to be able to distinguish the defect ultrasonic signals between two adjacent layers, which requires a higher longitudinal resolution. Therefore, a frequency of 5 MHz is selected.

[0045] (1.3) Selection of the number of probe chips N: This is mainly related to the curvature of the part. The linear array phased array probe has a large size along the chip arrangement direction. When the curvature of the part surface is too large, the probe edge coupling is poor and the sound beam cannot vertically incident on the part surface, affecting the phased array detection effect. It can be selected according to formula (1):

[0046] N×a+(N-1)×g≤R p / 20 (1)

[0047] (1.4) Selection of probe chip length b: The chip length mainly affects the penetration ability of ultrasound. The longer the chip, the stronger the penetration ability. For composite wall panels with a thickness range of 2mm to 30mm, the chip length b should be about 10mm.

[0048] (1.5) Probe shoe selection: Use an Ω-shaped immersion probe shoe. The curvature of the outer edge of the probe shoe matches the curvature R of the part. The linear array phased array probe is built into the probe shoe. During detection, the inside of the probe shoe is filled with water. The water layer thickness H w According to formula (2), select:

[0049] 0.3D w ≤H w ≤0.6D w (2)

[0050] Part II: Principles for the fusion setting of phase control parameters and mechanical motion parameters

[0051] (2.1) Phased array parameter setting principles:

[0052] For phased array inspection of composite parts, the acoustic field characteristics of the phased array beam and the scanning characteristics of the electronic scanning are important factors affecting the sensitivity of defect detection, imaging resolution, imaging contrast and quantitative accuracy. The relevant phased array parameters mainly include the beam scanning mode, the beam scanning direction (the arrangement direction of the linear array probe wafers), the number of excited wafers, the focus depth, the focal size, and the wafer stepping of the electronic scanning.

[0053] (2.1.1) The composite wall panel is a prepreg layer-by-layer stacking structure. Its internal defects are area defects parallel to the layers. Longitudinal wave direct incident acoustic beam detection is adopted, and the scanning mode is set to 0° linear electronic scanning.

[0054] (2.1.2) Since this patent application adopts phased array-automation fusion technology, it is necessary to combine the characteristics of automated scanning and design the phased array acoustic beam electronic scanning parameters, specifically to make the direction of electronic scanning consistent with the stepping direction of mechanical scanning, such as Figure 1 As shown, 1 is the arrangement direction of the linear array probe chips, which is also the direction of the linear electronic scanning of the sound beam, 2 is the scanning direction of the two-dimensional grid type mechanical scanning, 3 is the stepping direction of the two-dimensional grid type mechanical scanning, 4 is the length direction of the part, and 5 is the width direction of the part.

[0055] (2.1.3) The number of chips excited at one time, n: affects the display ratio of defect imaging in the two-dimensional direction and the focal size of the focused acoustic beam. n needs to satisfy both formula (3) and formula (4):

[0056]

[0057] [n×a+(n-1)g]×H p ÷4D p ≤Φ min / twenty four)

[0058] (2.1.4) Electronic scanning chip step number η: The setting principle satisfies formula (5)

[0059] (g+a) ×η≤Φ min / 2 (5)

[0060] (2.2) The principle of mechanical parameter setting is:

[0061] Mechanical parameters include scanning and stepping direction, line stepping, point stepping, and scanning speed. The mechanical parameter setting of phased array automated detection needs to consider the influence of phased array parameters.

[0062] (2.2.1) The automated inspection system carries a probe to perform grid scanning on the surface of composite parts. The scanning length can be large, so the scanning direction is set to the part length direction 4, and the stepping direction is set to the part width direction 5, such as Figure 1 .

[0063] (2.2.2) Automatic scanning line step L: to ensure the coverage between scanning lines and to avoid missing any part, calculated according to formula (6).

[0064] L=ε×[(g+a)×η]×[(Ν-n)÷η+1] (6)

[0065] (2.2.3) Automatic scanning point step S: In order to ensure that the defect imaging is not distorted, it is calculated according to formula (7):

[0066] S=(g+a) ×η (7)

[0067] (2.2.4) Automated scanning speed ν s : To ensure that data is not lost, formula (8) should be satisfied.

[0068]

[0069] The following is a further explanation using a specific example.

[0070] A carbon fiber composite wall panel with a curvature of about R900mm and a thickness of 20mm was selected. The NUSCAN type automated phased array ultrasonic testing system was used. The system pulse repetition frequency was continuously adjustable within the range of 1 to 20KHz, the automated mechanical scanning line step and point step could be set arbitrarily, and the scanning speed was continuously adjustable within the range of 100mm / s to 1000mm / s.

[0071] 1. Probe and accessories selection:

[0072] One-dimensional linear array phased array probe, specific specifications: 5MHz-L-128-0.3-0.05-W10 one-dimensional linear array straight probe.

[0073] The probe frequency is selected as 5MHz.

[0074] Select the number of probe elements N according to the following rule: N×a+(N-1)×g≤R p / 20, R p The total number of probe chips is 900mm, and the final number of probe chips is 128. Since the number of probe chips is mainly related to the curvature of the part, the linear array phased array probe has a large size along the chip arrangement direction. When the curvature of the part surface is too large, the probe edge is poorly coupled, and the sound beam cannot vertically incident on the part surface, affecting the phased array detection effect.

[0075] The chip width a is selected to be 0.25mm, the distance g between two adjacent chips is 0.05mm, and the chip length is 10mm. The chip length mainly affects the penetration ability of ultrasound. The longer the chip, the stronger the penetration ability. For composite material wall panels with a thickness range of 2mm to 30mm, the chip length b is preferably selected to be about 10mm.

[0076] Ω-shaped immersion probe shoe, the probe shoe curvature is about R800mm.

[0077] According to the formula 0.3D w ≤H w ≤0.6D w , D w The water layer thickness of the probe shoe is approximately 83.3mm and is selected to be 30mm.

[0078] Phased array and automated scanning multi-parameter fusion settings:

[0079] (1) The mechanical scanning device of the automated inspection system can drive the probe shoe to scan the surface of the part and always keep the probe shoe in close contact with the part.

[0080] (2) Use longitudinal wave direct incident acoustic beam detection, and set the scanning mode to 0° linear electronic scanning.

[0081] (3) Adjust the placement of the phased array probe so that the chip arrangement direction is along the Z direction of the automated detection system and the chip length direction is along the X direction of the automated detection system.

[0082] (4) The number of chips excited at one time is based on

[0083] [n×a+(n-1)g]×H p ÷4D p ≤Φ min / 2

[0084] The final selection was 30.

[0085] The chip stepping of electronic scanning is based on (g+a)×η≤Φ min / 2, the final choice is 2.

[0086] (5) The mechanical scanning method is grid scanning, the scanning direction is along the X direction of the automated detection system, and the stepping direction is along the Z direction of the automated detection system.

[0087] (6) The scanning line step is based on L = ε × [(g + a) × η] × [(Ν-n) ÷ η + 1] and is finally selected as 15 mm. The scanning line point step is based on S = (g + a) × η and is finally selected as 0.6 mm. The scanning speed is based on The PRF is 20kHz and the final choice is 200mm / s.

[0088] (7) Take the ε value as 0.6. Set a reasonable ε value and use the central sound beam to detect imaging to avoid poor coupling at the edge of the water shoe and ensure good imaging effect; choose its value as 0.6, that is, take 30% from the center to both sides, and take a total of 60% of the sound beam for imaging. The more central the sound beam, the better the coupling effect, and the more edge the sound beam, the worse the effect.

[0089] Therefore, through the internal defect detection method of aviation carbon fiber composite material panels proposed in this patent application, according to its requirements, the probe and probe shoe selected in this embodiment, the set phased array parameters and automation parameters are obtained, and automated phased array ultrasonic detection of composite carbon fiber panels can be implemented.

[0090] The final test results show that:

[0091] 1. The selected probe is suitable for anisotropic carbon fiber composite materials. For composite wall panels with a thickness of 2mm to 30mm, the probe frequency and probe size can ensure strong penetration ability. At the same time, the number of chips is large and the scanning width is large at one time, which can achieve high-efficiency detection of composite wall panels;

[0092] 2. The Ω-shaped immersion probe shoe matches the curvature of the part to ensure a good coupling effect. The thickness of the water layer in the probe shoe is large enough to avoid the influence of the water-part secondary interface signal on the part ultrasonic signal;

[0093] 3. Press Figure 1 As shown, the planning of the placement direction of the linear array phased array probe and the electronic linear scanning direction can match the mechanical scanning direction of the automation system to achieve rapid imaging detection of large-size wall panel parts;

[0094] 4. The chip stepping resolution of phased array electronic linear scanning is equivalent to the point stepping resolution of automated mechanical scanning, and the overall imaging resolution of the parts is uniform and the imaging is not distorted;

[0095] 5. The ultrasonic sound beam of the phased array electronic linear scanning has a focusing characteristic, and the focal size is no more than half of the minimum defect size required for the part to be detected. It has a high detection sensitivity and meets the detection sensitivity requirement of the minimum defect size of military aircraft of Φ3mm, which is better than the traditional single-chip ultrasonic detection method; the imaging contrast and imaging resolution are high, and the defect quantification is more accurate;

[0096] 6. The phased array probe covers a wide area. Combined with the automated detection system, the automated mechanical scanning single-line scanning width is large and the detection efficiency is high;

[0097] 7. Set a reasonable ε value and use the central acoustic beam to detect imaging to avoid poor coupling at the edge of the water shoe and ensure excellent imaging effect;

[0098] 8. Mechanical scanning line stepping ensures scanning coverage and no missed inspection between scanning lines;

[0099] 9. According to the pulse repetition frequency of the phased array ultrasonic system, the number of probe chips, the phased parameters and the mechanical scanning point stepping of the automation system, the mechanized scanning speed is integrated and designed to ensure that no data is lost during the scanning process.

Claims

1. A method for detecting internal defects of aviation carbon fiber composite material panels, characterized in that: The linear array phased array probe is installed in a probe shoe filled with water. The outer edge of the probe shoe is in direct contact with the surface of the part to be inspected and its curvature matches the curvature of the part. The electronically controlled ultrasonic beam emitted by the linear array phased array probe enters the inside of the part through the water inside the probe shoe, realizing electronic scanning of the ultrasonic beam in the area covered by the probe. The mechanical scanning device of the automated inspection system carries the phased array probe shoe to perform grid-type mechanical scanning on the surface of the part to be inspected.

2. The method for detecting internal defects of aviation carbon fiber composite material panels according to claim 1, characterized in that: The linear array phased array probe (A) is composed of a plurality of probe chips arranged in parallel; the number N of the probe chips is selected according to the following formula: N×a+(N-1)×g≤R p / 20; a is the size of a single probe wafer along the wafer arrangement direction, that is, the wafer width; g is the distance between the edges of two adjacent wafers along the wafer arrangement direction; R p is the part curvature.

3. The method for detecting internal defects of aviation carbon fiber composite material panels according to claim 1 or 2, characterized in that: The frequency of the linear array phased array probe is 5 MHz.

4. The method for detecting internal defects of aviation carbon fiber composite material panels according to claim 1, characterized in that: The probe shoe (9) is an Ω-shaped water-immersion probe shoe, the curvature of the outer edge of the probe shoe matches the curvature R of the part, the linear array phased array probe is built into the probe shoe, and during detection, the inside of the probe shoe is filled with water, and the water layer thickness H w Select according to the following formula: 0.3D w ≤H w ≤0.6D w ;D w is the length of the ultrasonic near field in water.

5. The method for detecting internal defects of aviation carbon fiber composite material panels according to claim 1, 2 or 4, characterized in that: The ultrasonic sound beam is a longitudinal wave direct incident sound beam detection, and the scanning mode is set to 0° linear electronic scanning.

6. The method for detecting internal defects of aviation carbon fiber composite material panels according to claim 5, characterized in that: The direction of linear electronic scanning of the internal acoustic beam of the linear array phased array probe is consistent with the stepping direction of the mechanical scanning device.

7. The method for detecting internal defects of aviation carbon fiber composite material panels according to claim 6, characterized in that: The number of chips n excited at one time in the linear array phased array probe affects the display ratio of defect imaging in the two-dimensional direction and the focal size of the focused acoustic beam. n needs to satisfy the following two formulas at the same time: [n×a+(n-1)g]×H p ÷4D p ≤Φ min / 2 Where, b is the length of a single wafer; H p is the thickness of the part; D p is the length of the ultrasonic near field in the part; Φ min The minimum defect size required to be detected on a part.

8. The method for detecting internal defects of aviation carbon fiber composite material panels according to claim 7, characterized in that: The electronic scanning chip step number η setting principle satisfies the following formula: (g+a)×η≤Φ min / 2, the electronic scanning chip step number is the number of chips between two adjacent sound beam groups that perform linear electronic scanning according to sequence excitation.

9. The method for detecting internal defects of aviation carbon fiber composite material panels according to claim 1, characterized in that: The automated inspection system carries a linear array phased array probe to perform grid scanning on the surface of the composite material part, with the scanning direction being the length direction of the part and the stepping direction being the width direction of the part.

10. The method for detecting internal defects of aviation carbon fiber composite material panels according to claim 9, characterized in that: The automated scanning step L of the automated detection system is calculated as follows: L=ε×[(g+a)×η]×[(Ν-n)÷η+1] Among them, ε is a constant not greater than 1, which is used to eliminate the poor imaging effect caused by the poor edge coupling of the linear array phased array probe; The automatic scanning point step S is calculated as follows: S=(g+a)×η Automatic scanning speed ν s Calculate according to the following formula: PRF is the pulse repetition frequency of the phased array ultrasound system.