Additive manufacturing metal low-cycle fatigue life prediction method based on hole defect characteristics
By constructing an exponential functional relationship based on the characteristics of hole defects, a low-cycle fatigue life prediction model for additively manufactured metals was established, which solved the impact of hole defects on material fatigue performance, and improved prediction accuracy and structural durability.
Patent Information
- Application Number
- CN202411063162.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-11-19
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The prior art cannot effectively eliminate the hole defects in additive manufacturing metals, resulting in a significant impact on the material's fatigue failure ability. There is a lack of effective low-cycle fatigue life prediction methods, which affects structural durability and reliability evaluation.
By comprehensively considering the geometric characteristics of hole defects, the hole defect feature parameter P is proposed, and an exponential functional relationship is established based on this parameter, a fatigue life prediction model based on the hole defect characteristics is constructed, and a low-period fatigue life prediction is carried out in combination with the damage accumulation law.
The accuracy and reliability of low-cycle fatigue life prediction is improved, the dispersion is reduced, and the effective life prediction of additively manufactured metals is achieved.
Smart Images

Figure CN118983034A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of fracture mechanics, and in particular to a method for predicting low-cycle fatigue life of additively manufactured metals based on hole defect characteristics. Background Art
[0002] Compared with traditional manufacturing processes, additive manufacturing technology can achieve complex parts manufacturing and lightweight design with its layer-by-layer manufacturing strategy advantage. Considering that in actual engineering applications, the safe use of parts must not only meet the static strength design, but also be able to withstand the long-term effects of cyclic fatigue loads. Therefore, issues related to fatigue performance have become a key factor in promoting the in-depth application of additively manufactured metal parts.
[0003] Because there is a very complex and interdependent dynamic relationship between laser-powder-melt pool in the additive manufacturing process. From a physical process perspective, additive manufacturing is actually a micro-forging process. Under the combined effect of high cooling rate and high temperature gradient of the deposited layer metal, there are usually a large number of volume defects of various shapes inside the additively manufactured metal specimen. Although current research shows that the process improvement window can be used to cope with the continuous and rapid change of solidification cooling rate, partially eliminate the negative impact of high temperature gradient during laser melting, achieve the process standard of minimizing hole defects, and improve the reliability of the additive manufacturing process, there is currently no effective method to completely eliminate the internal hole defects of additively manufactured metals. At the same time, since fatigue cracks usually originate from stress concentration areas, the material's fatigue failure resistance will be significantly affected by hole defects (such as pores, keyholes, and unfused defects). Therefore, quantitatively establishing the relationship between the internal hole defect characteristics and the fatigue behavior of additively manufactured metals is crucial to improving the structural durability and reliability evaluation accuracy of additively manufactured metals. Summary of the invention
[0004] The purpose of the present invention is to address the deficiencies in the prior art and provide a method for predicting the low-cycle fatigue life of additively manufactured metals based on the geometric characteristics of hole defects; by comprehensively considering the influence of the geometric characteristics of hole defects on the fatigue performance of materials, a hole defect characteristic parameter P is proposed, and the key defects at the fatigue fracture of the material are effectively identified through the characteristic parameter, and based on the exponential function relationship between the constructed hole defect characteristic parameter and the fatigue life of the material under the low-cycle fatigue state, a fatigue life prediction model based on the geometric characteristics of key hole defects in the fatigue fracture area is proposed; compared with the traditional low-cycle fatigue life prediction model, the model proposed by the present invention has higher prediction accuracy and lower dispersion.
[0005] In order to achieve the above technical objectives, the present invention adopts the following technical solutions.
[0006] A method for predicting low-cycle fatigue life of additively manufactured metal based on hole defect characteristics comprises the following steps:
[0007] Step S1, designing the geometric shape of the round bar specimen according to ASTM standard E8 / E8M-13a, and manufacturing the specimen by selective laser melting;
[0008] Step S2, according to the test procedure of ASTM E18, at room temperature and low strain rate conditions, the round bar specimen is tested to obtain the stress-strain curve of the material, and then the elastic-plastic constitutive model parameters of the material are obtained;
[0009] Step S3, using micro-tomography technology to obtain the distribution of hole defects in the sample, generating a cylindrical finite element model with different defect characteristics in ABAQUS according to the scanning results, and using C3D10 unit to perform stress / strain analysis to obtain the law of the change of material plastic deformation size with defect size, defect shape and defect position;
[0010] Step S4, based on the finite element analysis result of step S3, comprehensively considering the relationship between the geometric characteristics of the hole defect and the fatigue performance of the material, and proposing the hole defect characteristic parameter P;
[0011] Step S5, based on the exponential function relationship between the characteristic parameter P of the hole defect and the fatigue life of the material under the low cycle fatigue state, a prediction model for the low cycle fatigue life of additively manufactured metals based on the hole defect characteristics is proposed;
[0012] Step S6: Use the fatigue life prediction model established in step S5 in combination with the damage accumulation law to predict the low cycle fatigue life of the additively manufactured metal, and compare it with the traditional fatigue life prediction model.
[0013] Specifically, the kinematic hardening parameter C of the elastic-plastic constitutive model in step S2 is k and r k The calculation formula is:
[0014]
[0015]
[0016] In the above formula, σ k+1 is the stress value extracted from the K+1th point of the stress-strain curve; σ k is the stress value taken at the Kth point in the stress-strain curve; σ k-1 is the stress value taken at the K-1th point in the stress-strain curve; is the plastic strain value taken at the K+1th point in the stress-strain curve; is the plastic strain value taken at the Kth point of the stress-strain curve; is the plastic strain value taken at the K-1th point of the stress-strain curve.
[0017] Specifically, in step S3, the load magnitude of the material is determined by the stress amplitude ε a Description: The hole defect size adopts the Murakami parameter of the projected area of the defect perpendicular to the maximum stress direction. Description, the hole defect shape is expressed by the aspect ratio R d Description: The position of the hole defect is described by the distance D from the center of the hole defect to the free surface.
[0018] Specifically, the hole characteristic parameter P in step S4 is expressed as:
[0019]
[0020] In the above formula, Y is the shape factor, internal hole defect Y = 0.5, sub-surface hole defect Y = 0.8; ε a is the strain amplitude; is the Murakami parameter; R d is the aspect ratio; D is the distance from the center of the hole defect to the free surface; D d is the major axis length of the hole defect; m and n are material constants.
[0021] Specifically, the additive manufacturing metal low cycle fatigue life prediction model based on the hole defect characteristics in step S5 is expressed as:
[0022] P max =kEXP(μN f ) (4)
[0023] In the above formula, P max is the characteristic parameter of the largest hole inside the material; k and μ are fitting parameters; N f is the material fatigue life.
[0024] Specifically, the calculation formula of the damage accumulation law in step S6 is:
[0025]
[0026] In the above formula, φ is the damage value; q is the damage parameter; N f is the material fatigue life.
[0027] Specifically, in step S6, the traditional fatigue life prediction models include the Manson-Coffin model and the Smith-Watson-Topper model;
[0028] The expression of the Manson-Coffin model is:
[0029]
[0030] The expression of the Smith-Watson-Topper model is:
[0031]
[0032] In the above formula, σ max is the maximum stress; ε a is the strain amplitude; σ' f is the fatigue strength coefficient; ε' f is the fatigue ductility coefficient; b is the fatigue strength index; c is the fatigue ductility index.
[0033] Compared with the prior art, the present invention has the following beneficial effects:
[0034] The method of the present invention considers the important influence of hole defects in fatigue section on the dispersion of fatigue life of additively manufactured metal, analyzes the influence of geometric characteristics of hole defects on fatigue performance of materials, comprehensively considers the influence of geometric characteristics of hole defects on fatigue performance of materials, and proposes hole defect characteristic parameter P, which can effectively identify key defects at fatigue fracture of materials. There is a good exponential relationship between this parameter and material fatigue life. According to the proposed hole defect characteristic parameter, combined with the geometric information of key hole defects at fatigue section, a low-cycle fatigue life prediction model based on hole defect characteristics is established, which can realize the effective prediction of low-cycle fatigue life of additively manufactured metal. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] In order to more clearly illustrate the technical solutions of the embodiments of the present disclosure, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present disclosure and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other relevant drawings can be obtained based on these drawings without paying creative work.
[0036] Figure 1 The present invention is a flow chart of a method for predicting low-cycle fatigue life of additively manufactured metal based on geometric features of hole defects.
[0037] Figure 2 Schematic diagram of the geometric shape of the tested sample in an embodiment of the present invention.
[0038] Figure 3 1 is a uniaxial tensile stress-strain curve diagram of the tested sample in an embodiment of the present invention.
[0039] Figure 4 Schematic diagram of a finite element model containing hole defects with different geometric features that is randomly generated in an embodiment of the present invention.
[0040] Figure 5It is an equivalent replacement diagram of the irregular hole defect in the embodiment of the present invention.
[0041] Figure 6 This is a SEM image of the fatigue fracture in the embodiment of the present invention.
[0042] Figure 7 Graph showing the relationship between hole characteristic parameters and material fatigue life in an embodiment of the present invention.
[0043] Figure 8 Comparison of fatigue life prediction results between the fatigue life prediction model constructed by the method of the present invention and the traditional MC model and SWT model, as well as error analysis diagram. DETAILED DESCRIPTION
[0044] The embodiments of the present invention are described in detail below. The embodiments described with reference to the accompanying drawings are exemplary. It should be understood that the specific embodiments described herein are only used to explain the present application and are not used to limit the present application.
[0045] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art of the technical field of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The terms "including" and "having" and any variations thereof in the specification and claims of the present application and the accompanying drawings are intended to cover non-exclusive inclusions. For example, a series of steps S or units are included, or alternatively, steps S or units not listed are also included, or other steps S or units inherent to these processes, methods, products or devices are also included optionally.
[0046] Only the part relevant to the present application but not all content is shown in the accompanying drawings.Before discussing exemplary embodiments in more detail, it should be mentioned that some exemplary embodiments are described as processing or methods described as flow charts.Although flow charts describe various operations (or step S) as sequential processing, many operations therein can be implemented in parallel, concurrently or simultaneously.In addition, the order of various operations can be rearranged.Described processing can be terminated when its operation is completed, but can also have additional steps S not included in the accompanying drawings.
[0047] Example
[0048] like Figure 1 As shown, the present invention provides a method for predicting low-cycle fatigue life of metal in additive manufacturing based on geometric characteristics of hole defects, comprising the following steps:
[0049] Step S1: Figure 2As shown, the geometry of the round bar specimen was designed according to the ASTM standard E8 / E8M-13a, and the specimen was manufactured by the selective laser melting (SLM) method. The distribution range of Ti6Al4V powder is 13 to 65 um;
[0050] The manufacturing process parameters are: laser power 280W, sintering rate 1200mm / s, layer thickness 40um;
[0051] Step S2: According to the test procedure of ASTM E18, the round bar specimen is tested at room temperature and low strain rate to obtain the stress-strain curve of the material, such as Figure 3 As shown;
[0052] In order to facilitate finite element calculation, in this embodiment, only three points are taken from the stress-strain curve to calibrate the kinematic hardening parameters; the material kinematic hardening parameter C k and r k The calculation formula is:
[0053]
[0054]
[0055] In the above formula, σ k+1 is the stress value extracted from the K+1th point of the stress-strain curve; σ k is the stress value taken at the Kth point in the stress-strain curve; σ k-1 is the stress value taken at the K-1th point in the stress-strain curve; is the plastic strain value taken at the K+1th point in the stress-strain curve; is the plastic strain value taken at the Kth point of the stress-strain curve; is the plastic strain value taken at the K-1th point of the stress-strain curve;
[0056] Step S3, using X-ray micro-tomography technology to obtain the distribution of hole defects in the sample, it is found that the equivalent diameter of the hole defects is between 20-50 μm, the circularity of the hole defects is between 0.6-0.75, and the distance between the hole defects and the free surface is between 500-3500 mm; Figure 4 Shown is a finite element model of a cylinder with different void defects generated based on the statistical information of void defect distribution.
[0057] In order to effectively evaluate the influence of hole defect characteristics on material fatigue properties, such as Figure 5 As shown in the figure, the Murakami method is used to replace the irregular hole defects; finally, the Murakami parameters are used Aspect Ratio dThe hole defect characteristics are parameterized by the distance D from the hole defect center to the free surface.
[0058] In this embodiment, the Murakami parameters is the projection area of the cross-sectional defect in the direction perpendicular to the maximum stress; the aspect ratio R d It is the ratio between the minor axis length and the major axis length of the equivalent ellipse of the cross-sectional defect.
[0059] Step S4: Based on the finite element analysis results of step S3, the relationship between the geometric characteristics of the hole defect and the fatigue performance of the material is comprehensively considered, and a hole defect characteristic parameter P is proposed. The hole characteristic parameter P is expressed as:
[0060]
[0061] In the above formula, Y is the shape factor, internal hole defect Y = 0.5, sub-surface hole defect Y = 0.8; ε a is the strain amplitude; is the Murakami parameter; R d is the aspect ratio; D is the distance from the center of the hole defect to the free surface; D d is the major axis length of the hole defect; m and n are material constants.
[0062] Step S5, based on the exponential function relationship between the characteristic parameters of the hole defect and the fatigue life of the material under the low cycle fatigue state, a prediction model for the low cycle fatigue life of additively manufactured metals based on the hole defect characteristics is proposed;
[0063] In this embodiment, six groups of samples were subjected to fatigue loads with strain amplitudes of 0.8% and 1.2% respectively until the materials broke and failed, and the fatigue fractures were analyzed by SEM (the analysis results are shown in FIG. Figure 6 As shown), the geometric information of the hole defect of the material fatigue fracture is obtained, and then the hole characteristic parameters of all the hole defects in the fatigue fracture crack propagation area are calculated according to the hole characteristic parameters proposed in step S4, where the hole defect with the largest hole characteristic parameter is recorded as the key defect.
[0064] like Figure 7 As shown in the figure, according to the exponential function relationship between the hole characteristic parameters of the key defects and the fatigue life of the material, a low-cycle fatigue life prediction model for additively manufactured metals based on defect characteristics is proposed:
[0065] P max =kEXP(μN f ) (4)
[0066] In the above formula, P max is the characteristic parameter of the largest hole inside the material; k and μ are fitting parameters; N fis the material fatigue life.
[0067] In the above formula, P is the maximum hole characteristic parameter of the material, k and μ are fitting parameters, and N f is the material fatigue life.
[0068] Step S6: Use the fatigue life prediction model established in step S5 in combination with the damage accumulation law to predict the low cycle fatigue life of the additively manufactured metal. The calculation formula of the linear damage accumulation law is:
[0069]
[0070] In the above formula, φ is the damage value; q is the damage parameter; N f is the material fatigue life.
[0071] The prediction results of the low-cycle fatigue life prediction model proposed in the present invention are compared with those of the traditional low-cycle fatigue life prediction models, the Manson-Coffin model and the Smith-Watson-Topper model, where:
[0072] The expression of the Manson-Coffin model is:
[0073]
[0074] The expression of the Smith-Watson-Topper model is:
[0075]
[0076] In the above formula, σ max is the maximum stress; ε a is the strain amplitude; σ' f is the fatigue strength coefficient; ε' f is the fatigue ductility coefficient; b is the fatigue strength index; c is the fatigue ductility index.
[0077] The comparison results are as follows Figure 8 As shown by Figure 8 It can be seen that the prediction results of the low-cycle fatigue life prediction model provided by the present invention all fall within the 1.5-fold error band, indicating that the actual fatigue fracture life of the material is close to the model prediction result, while the prediction results of the traditional MC model and SWT model are partially outside the 1.5-fold error band, indicating that the prediction accuracy of the fatigue life prediction model constructed by the method of the present invention is higher than that of the traditional MC model and SWT model.
[0078] The above is only a preferred embodiment of the present invention, and does not limit the present invention in other forms. Any technician familiar with the profession may use the above disclosed technical content to change or modify it into an equivalent embodiment with equivalent changes. However, any simple modification, equivalent change and modification made to the above embodiment according to the technical essence of the present invention without departing from the technical solution of the present invention still belongs to the protection scope of the technical solution of the present invention.
Claims
1. A method for predicting low-cycle fatigue life of metal in additive manufacturing based on hole defect characteristics, characterized in that: The following steps are involved: Step S1, designing the geometric shape of the round bar specimen according to the American Society for Testing and Materials ASTM standard E8 / E8M-13a, and manufacturing the specimen by selective laser melting; Step S2, according to the test procedure of ASTM E18, at room temperature and low strain rate conditions, the round bar specimen is tested to obtain the stress-strain curve of the material, and then the elastic-plastic constitutive model parameters of the material are obtained; Step S3, using micro-tomography technology to obtain the distribution of hole defects in the sample, generating a cylindrical finite element model with different defect characteristics in ABAQUS according to the scanning results, and using C3D10 unit to perform stress / strain analysis to obtain the law of the change of material plastic deformation size with defect size, defect shape and defect position; Step S4, based on the finite element analysis result of step S3, comprehensively considering the relationship between the geometric characteristics of the hole defect and the fatigue performance of the material, and proposing the hole defect characteristic parameter P; Step S5, based on the exponential function relationship between the characteristic parameter P of the hole defect and the fatigue life of the material under the low cycle fatigue state, a prediction model for the low cycle fatigue life of additively manufactured metals based on the hole defect characteristics is proposed; Step S6: Use the fatigue life prediction model established in step S5 in combination with the damage accumulation law to predict the low cycle fatigue life of the additively manufactured metal, and compare it with the traditional fatigue life prediction model.
2. The method for predicting low-cycle fatigue life of metal in additive manufacturing based on hole defect characteristics according to claim 1 is characterized in that: In step S2, the elastic-plastic constitutive model has a kinematic hardening parameter C k and r k The calculation formulas are: In the above formula, σ k+1 is the stress value extracted from the K+1th point of the stress-strain curve; σ k is the stress value taken at the Kth point in the stress-strain curve; σ k-1 is the stress at the K-1th point in the stress-strain curve. Force value; is the plastic strain value taken at the K+1th point in the stress-strain curve; is the plastic strain value taken at the Kth point of the stress-strain curve; is the plastic strain value taken at the K-1th point of the stress-strain curve.
3. The method for predicting low-cycle fatigue life of metal in additive manufacturing based on hole defect characteristics according to claim 1 is characterized in that: The load magnitude of the material in step S3 is the stress amplitude ε a Description: The hole defect size adopts the Murakami parameter of the projected area of the defect perpendicular to the maximum stress direction. Description, the hole defect shape is expressed by the aspect ratio R d Description: The position of the hole defect is described by the distance D from the center of the hole defect to the free surface.
4. The method for predicting low-cycle fatigue life of metal in additive manufacturing based on hole defect characteristics according to claim 1 is characterized in that: The hole characteristic parameter P in step S4 is expressed as: In the above formula, Y is the shape factor, internal hole defect Y = 0.5, sub-surface hole defect Y = 0.8; ε a is the strain amplitude; is the Murakami parameter; R d is the aspect ratio; D is the distance from the center of the hole defect to the free surface; D d is the major axis length of the hole defect; m and n are material constants.
5. The method for predicting low-cycle fatigue life of metal in additive manufacturing based on hole defect characteristics according to claim 1, characterized in that: The additive manufacturing metal low cycle fatigue life prediction model based on defect characteristics described in step S5 is expressed as: P max =kEXP(μN f ) (4) In the above formula, P max is the characteristic parameter of the largest hole inside the material; k and μ are fitting parameters; N f is the material fatigue life.
6. The method for predicting low-cycle fatigue life of metal in additive manufacturing based on hole defect characteristics according to claim 1 is characterized in that: The calculation formula of the damage accumulation law in step S6 is: In the above formula, φ is the damage value; q is the damage parameter; N f is the material fatigue life.
7. The method for predicting low-cycle fatigue life of metal in additive manufacturing based on hole defect characteristics according to claim 1 is characterized in that: In step S6, the traditional fatigue life prediction models include the Manson-Coffin model and the Smith-Watson-Topper model; The expression of the Manson-Coffin model is: The expression of the Smith-Watson-Topper model is: In the above formula, σ max is the maximum stress; ε a is the strain amplitude; σ' f is the fatigue strength coefficient; ε' f is the fatigue ductility coefficient; b is the fatigue strength index; c is the fatigue ductility index.
Citation Information
Cited By
Metal fatigue crack initiation simulation method for coupling holes and microstructures
CN119864113A