Thin film auxiliary method for improving dry etching precision and dry etching product
By adding a periodic SiO2 mask layer to the surface of the material to be etched, the problem of weak EPD signal in dry etching is solved, enabling precise control and consistent monitoring of the etching process, thus improving etching accuracy and reliability.
Patent Information
- Application Number
- CN202410966953.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-18
- Publication Date
- 2024-11-19
AI Technical Summary
In semiconductor manufacturing, existing dry etching technology is difficult to effectively monitor the etching process in complex or strongly absorbing material systems, resulting in insufficient etching accuracy and reliability, and failing to guarantee the consistency of etching depth.
A SiO2 mask layer with a periodic pattern is added to the surface of the material to be etched. EPD signals are obtained through the etching monitoring area A to optimize the monitoring of the dry etching endpoint and ensure that the etching depth of the device etching area B reaches the preset value.
It improves etching accuracy and reliability, enables real-time monitoring of film thickness changes in complex material systems, and ensures the repeatability and consistency of the etching process.
Smart Images

Figure CN118983300A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of semiconductor manufacturing, and in particular to a thin film auxiliary method and a dry etching product for improving dry etching accuracy. Background Art
[0002] In semiconductor manufacturing and micromachining applications, dry etching technology is a key process step used to accurately remove materials to form tiny circuit patterns. In this process, endpoint monitoring (EPD) technology plays a vital role. EPD technology is based on the principles of optical interference and reflection, and accurately controls the etching process by monitoring the changes in the intensity of interference light generated by the interaction between the laser beam and the processed material. However, when the material system to be etched is complex or has strong absorption of the laser light source, the EPD signal may become complex or weak, or even submerged by noise, making it difficult to effectively monitor the changes in film thickness during the etching process. In this case, the common method is to abandon the use of EPD monitoring and instead control the etching time to control the etching depth. The disadvantage of this method is that it cannot monitor the state of etching in real time and cannot guarantee the repeatability of etching. If the state of the etching equipment (chamber vacuum changes) or the state of the material to be etched (the material surface is not cleaned), the etching rate is likely to change, and the etching time required to etch the same depth will change. Under-etching or over-etching will occur, which will eventually lead to poor process results or even failure. Summary of the invention
[0003] The present application provides a thin film auxiliary method and dry etching product for improving the precision of dry etching, which belongs to a method for optimizing the dry etching endpoint monitoring (EPD) technology by applying a specific mask layer dielectric film. The method of the present invention not only improves the precision and reliability of the dry etching process, but also provides a new technical means for the fine processing of complex material systems, and expands the application scope of the existing dry etching technology.
[0004] In a first aspect, a dry etching product is provided, comprising a stacked material to be etched and a mask layer material; the dry etching product is divided into an etching monitoring area A and a device etching area B, the mask layer pattern applied to the device etching area B is a device pattern, and the mask layer pattern applied to the etching monitoring area A is a periodic pattern;
[0005] The periodic pattern includes a plurality of pattern monomers, each of which is ring-shaped, and the plurality of pattern monomers are arranged in an array of M rows and N columns; the surface of the material to be etched that is not covered by the periodic pattern is completely exposed;
[0006] During the simultaneous etching of the etching monitoring area A and the device etching area B, the etching monitoring area A is used to perform etching monitoring to obtain an EPD signal, and a preset etching endpoint of the EPD signal corresponds to a preset etching depth of the device etching area B.
[0007] In combination with the first aspect, in certain implementations of the first aspect, after etching is completed, the mask layer dielectric film with the periodic pattern is not completely removed.
[0008] In combination with the first aspect, in certain implementations of the first aspect, when etching is completed, the etching depth of the material to be etched is L, and the etching selectivity ratio of the material to be etched and the mask layer dielectric film is r = etching rate of the material to be etched / etching rate of the mask layer dielectric film, then the deposition thickness of the mask layer dielectric film is L / r±150nm.
[0009] In combination with the first aspect, in certain implementations of the first aspect, the area of the EPD spot used for etching monitoring is S, the area of the periodic pattern on the material to be etched that is not covered by the mask layer is s, R = S / s, and within the EPD monitoring area, the number of pattern monomers covered by the EPD laser beam is N ≥ 30, and 10% ≤ R ≤ 80%.
[0010] In combination with the first aspect, in certain implementations of the first aspect, the pattern monomer is in the shape of a circular ring or a polygonal ring.
[0011] In combination with the first aspect, in certain implementations of the first aspect, the area of the etching monitoring region A is ≥ 2S, where S is the area of the EPD spot.
[0012] In combination with the first aspect, in some implementations of the first aspect, the mask layer material is SiO2.
[0013] In a second aspect, a thin film assist method for improving dry etching accuracy is provided, the method comprising:
[0014] A mask layer is deposited on the material to be etched, and a device pattern and a periodic pattern are formed on the mask layer to obtain a dry etching product, wherein the device pattern is located in the device etching area B, and the periodic pattern is located in the etching monitoring area A, and the periodic pattern includes a plurality of pattern monomers, each of which is annular, and the plurality of pattern monomers are arranged in an array of M rows and N columns, and the surface of the material to be etched that is not covered by the periodic pattern is completely exposed;
[0015] Place the dry-etched product into the dry-etching chamber and set the etching program;
[0016] Turn on the EPD laser and adjust the position of the laser spot so that the laser spot covers the periodic pattern of the etching monitoring area A;
[0017] The etching monitoring area A and the device etching area B of the dry etching product are etched simultaneously, and the EPD signal is obtained. When the preset etching end point on the EPD monitoring curve is reached, the etching program is stopped so that the etching depth of the device etching area B reaches the preset etching depth.
[0018] In conjunction with the second aspect, in some implementations of the second aspect, the method further includes:
[0019] Before the formal device etching, etching experiments are carried out on multiple samples of dry etching products to determine the preset etching endpoint on the EPD monitoring curve and the preset etching depth of the corresponding device etching area B.
[0020] In conjunction with the second aspect, in some implementations of the second aspect, the etching experiment includes:
[0021] Etch the target sample of the dry-etched product, and when the EPD monitoring curve of the etching monitoring area A of the target sample reaches the target end point, stop the etching program, take out the target sample, and detect the target etching depth of the device etching area B of the target sample;
[0022] If it is determined that the difference between the target etching depth and the preset etching depth is greater than the preset threshold, the EPD curve end point of the next sample is modified, and the above steps are repeated until the difference between the etching depth of the final sample and the preset etching depth is less than the preset threshold, and the EPD curve end point of the final sample is the preset etching end point.
[0023] In combination with the second aspect, in certain implementations of the second aspect, after etching is completed, the mask layer dielectric film with the periodic pattern is not completely removed.
[0024] In combination with the second aspect, in certain implementations of the second aspect, when etching is completed, the etching depth of the material to be etched is L, and the etching selectivity ratio of the material to be etched and the mask layer dielectric film is r = etching rate of the material to be etched / etching rate of the mask layer dielectric film, then the deposition thickness of the mask layer dielectric film is L / r±150nm.
[0025] In combination with the second aspect, in certain implementations of the second aspect, the area of the EPD spot used for etching monitoring is S, the area of the periodic pattern on the material to be etched that is not covered by the mask layer is s, R = S / s, and within the EPD monitoring area, the number of pattern monomers covered by the EPD laser beam is N ≥ 30, and 10% ≤ R ≤ 80%.
[0026] In combination with the second aspect, in some implementations of the second aspect, the pattern monomer is in the shape of a circular ring or a polygonal ring.
[0027] In combination with the second aspect, in certain implementations of the second aspect, the area of the etching monitoring region A is ≥ 2S, where S is the area of the EPD spot.
[0028] In combination with the second aspect, in some implementations of the second aspect, the mask layer material is SiO2.
[0029] Compared with the prior art, the solution provided by this application includes at least the following beneficial technical effects:
[0030] 1. Optimize EPD signal: By adding a layer of SiO2 film with a periodic pattern on the surface of the material to be etched, the EPD signal is effectively enhanced, especially in complex or strongly absorbing material systems.
[0031] 2. Improve monitoring accuracy: This method can improve the shape and strength of the monitoring curve, so that the changes in film thickness that were previously difficult to monitor can be accurately monitored in real time.
[0032] 3. Wide applicability: This method can be widely used in various complex semiconductor processing and micro-processing scenarios to improve the reliability and consistency of the process. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 :An example of the SiO2 pattern mentioned in this patent is shown. In this example, the periodic pattern is a ring, the side length of the ring is 20μm, the width of the ring is 3.5μm, and the period of the ring is 40μm. The SiO2 in the ring groove is removed to expose the material to be etched, and the rest of the positions are covered with SiO2.
[0034] Figure 2 : Shown Figure 1 In the local enlargement of the SiO2 pattern example, the width of the groove is about 3.5 microns.
[0035] Figure 3 : Shows the EPD monitoring curve of unpatterned SiO2 thin film material.
[0036] Figure 4 :The EPD monitoring curves of materials without SiO2 pattern assistance are shown, where the two curves of patternless 1 and patternless 2 are the EPD monitoring curves of the same material in different etched areas at different times. The peak of the patternless 1 curve near 1500S-2000S is caused by artificial adjustment of signal intensity (EPD signal weakening), which has nothing to do with the material itself. The signal intensity of the other curves is not artificially adjusted.
[0037] Figure 5 : Materials with SiO2 patterns are shown (see Figure 1 ) EPD monitoring curve. SiO2 growth mode and Figure 3 The SiO2 in the same, are PECVD, the material to be etched is Figure 4 The two curves with pattern 1 and pattern 2 are EPD monitoring curves of different etching areas at different times for materials with the same SiO2 pattern.
[0038] Figure 6 :Will Figure 3, Figure 4 and Figure 5 The middle curve is plotted in the same figure for comparison. The horizontal and vertical coordinates in the figure are original data without normalization or other processing. DETAILED DESCRIPTION
[0039] The present application is further described in detail below with reference to the accompanying drawings and specific embodiments.
[0040] The embodiment of the present application provides a thin film auxiliary method and dry etching product for improving the precision of dry etching. Specifically, an etching monitoring area A (located outside the device etching area B) is designed on the surface of the material to be etched. By monitoring the material etching condition of the etching monitoring area A, the material etching condition of the device etching area B is reflected.
[0041] The dry etching product includes applying a mask layer dielectric film (such as SiO2) with a periodic pattern in the etching monitoring area A. Figure 1 and Figure 2 As shown. The periodic pattern includes a plurality of pattern monomers, which are obtained by deposition on the material to be etched. Each pattern monomer can be ring-shaped, and the plurality of pattern monomers are arranged in an array of M rows and N columns to achieve the purpose of optimizing the EPD signal. The surface of the material to be etched that is not covered by the periodic pattern of the mask layer can be completely exposed.
[0042] The etching monitoring area A and the device etching area B are etched simultaneously; by acquiring the EPD signal of the etching monitoring area A, the material etching condition of the etching monitoring area A can be obtained, and then the material etching condition of the device etching area B can be obtained.
[0043] In some embodiments, the mask layer dielectric film with a periodic pattern may be formed by various deposition methods (eg, PECVD) or other techniques.
[0044] In some embodiments, after etching is completed, the dielectric film of the mask layer with the periodic pattern is not completely removed.
[0045] During the etching process of the material to be etched, the mask layer dielectric film is also etched synchronously, and it is necessary to ensure that the mask layer dielectric film is not completely removed when the etching is completed. In one embodiment, when the etching is completed, the etching depth of the material to be etched is L, and the etching selectivity ratio of the material to be etched to the mask layer dielectric film is r = etching rate of the material to be etched / etching rate of the mask layer dielectric film, then the deposition thickness of the mask layer dielectric film can be L / r±150nm.
[0046] In some embodiments, the area of the pattern monomer of the periodic pattern is related to the area of the EPD spot. Assuming that the area of the EPD spot is S, the area of the periodic pattern of the material to be etched that is not covered by the mask layer is s, and R = S / s. Within the EPD monitoring area, the number of pattern monomers covered by the EPD laser beam is N ≥ 30, and 10% ≤ R ≤ 80%.
[0047] The EPD spot is generally circular, and the EPD laser beam covers multiple pattern monomers, which can ensure the repeatability of the EPD signal monitored each time. In addition, the area of the material to be etched that is not covered by the periodic pattern of the mask layer (i.e., the exposed position) and the area of the material to be etched that is covered by the periodic pattern of the mask layer (i.e., the covered position) are in a suitable ratio, which helps to achieve the effect of optimizing the EPD signal, that is, it can achieve the effect of reflecting the material etching situation and modulating and improving the EPD signal, ensuring the repeatability of the EPD signal.
[0048] In some embodiments, the shape of the pattern monomers of the periodic pattern can be various structures such as annular, circular, square or polygonal. In addition, the relative position of each pattern monomer and the surrounding pattern monomers is the same.
[0049] In some embodiments, the area of the etching monitoring region A is ≥ 2S, where S is the area of the EPD spot.
[0050] In order not to affect the etching of the device pattern, the etching monitoring area A is an area independent of the device etching area B, and a periodic pattern is designed in the etching monitoring area A. It should be noted here that since the pattern to be etched in the device etching area B is different from the pattern involved in the etching monitoring area A in size and fineness, the etching speed can be different, and the positional relationship between the device pattern etching depth and the monitoring curve can be calibrated before the formal device etching.
[0051] Usually before material etching, a dielectric layer will be grown on the surface of the material to be etched, which is used as a mask layer for material etching. The present application designs the mask layer of the etching monitoring area A as a mask layer dielectric film with a periodic pattern. During the material etching process, the EPD signal is modulated and amplified by the film with a periodic pattern, thereby enhancing the intensity and analyzability of the EPD signal. By adding a periodic pattern to the surface of the material to be etched, the light reflected from the area covered by the periodic pattern and the area of the material to be etched (uncovered) interferes and superimposes, and is then collected by the EPD. This design of modulating the EPD signal not only improves the morphology of the EPD monitoring curve, but also increases its intensity, making the film thickness changes that were originally difficult to monitor become real-time and accurate monitoring possible.
[0052] Example 1
[0053] The thin film pattern is designed according to the complexity of the material to be etched, the light absorption of the material, etc. This patent gives an example, such as Figure 1 As shown, the thin film material is a SiO2 thin film grown by PECVD on the surface of the material sample to be etched, and the thickness of SiO2 is 500nm. The designed periodic pattern is a ring, the side length of the ring is 20μm, the width of the ring is 3.5μm, and the period of the ring is 40μm.
[0054] The SiO2 pattern can be prepared in the following way: first, a layer of SiO2 is evaporated on the surface of the material sample to be etched by PECVD, and the thickness of SiO2 is 500nm; the designed pattern is transferred to the photoresist on the surface of the SiO2 film by photolithography process. The photoresist used in this example is AZ6130 photoresist; the designed SiO2 pattern is transferred from the photoresist mask to the SiO2 film by combining dry etching or wet etching. RIE dry etching is used in this example; the photoresist on the surface of the film is completely removed by combining organic solvents and plasma glue machine, and the surface is cleaned.
[0055] The etching process may include: placing a material sample with a SiO2 pattern into an ICP dry etching chamber; setting up the etching program, turning on the EPD laser, adjusting the position of the laser spot so that the laser spot covers the SiO2 pattern; running the etching program, monitoring the etching curve, and according to the etching curve, reaching the preset etching end point on the EPD monitoring curve, stopping the etching program, and taking out the sample. Optionally, the remaining SiO2 is removed by dry or wet process means, and the etching depth of the device etching area B is detected by a step profiler or SEM.
[0056] In some embodiments, before the formal device etching, multiple etching experiments can be performed using samples (experimental pieces) with the same structure to calibrate the relationship between the etching depth (h) of the device etching area B and the EPD endpoint monitoring position (p).
[0057] Specifically, when the EPD monitoring curve of the etching monitoring area A reaches the end point p1, the etching program is stopped, the sample is taken out, and the etching depth h1 of the device etching area B is detected. The measured etching depth (h1) of the material in the device etching area B is linked to the end point (p1) of the EPD monitoring curve of the etching monitoring area A, that is, the point p1 of the EPD monitoring curve corresponds to the etching depth h1 of the material in the device etching area B. Afterwards, the above steps are repeated multiple times using the same sample (experimental piece) to obtain the relationship between the etching depths h2, h3, etc. of the material in the device etching area B and the end point monitoring end points p2, p3, etc., respectively. The relationship between the end point (p1, p2, p3, etc.) of the etching curve and the etching depth (h1, h2, h3, etc.) of the material device pattern is recorded, and through this relationship, the position p of the etching end point of the EPD monitoring curve corresponding to the expected etching depth h of the material is finally determined (for example, the peak of the fourth oscillation peak). When etching the subsequent device, the etching is stopped when the EPD monitoring curve reaches the end point, and the expected etching depth can be achieved.
[0058] Although the present invention is disclosed as above in the form of a preferred embodiment, it is not intended to limit the present invention. Any person skilled in the art may make possible changes and modifications without departing from the spirit and scope of the present invention. Therefore, the scope of protection of the present invention shall be based on the scope defined by the claims of the present invention.
Claims
1. A dry etching product, comprising a stacked material to be etched and a mask layer material; It is characterized in that The dry etching product is divided into an etching monitoring area A and a device etching area B. The mask layer pattern applied to the device etching area B is a device pattern, and the mask layer pattern applied to the etching monitoring area A is a periodic pattern. The periodic pattern includes a plurality of pattern monomers, each of which is ring-shaped, and the plurality of pattern monomers are arranged in an array of M rows and N columns; the surface of the material to be etched that is not covered by the periodic pattern is completely exposed; During the simultaneous etching of the etching monitoring area A and the device etching area B, the etching monitoring area A is used to perform etching monitoring to obtain an EPD signal, and a preset etching endpoint of the EPD signal corresponds to a preset etching depth of the device etching area B.
2. The product according to claim 1, It is characterized in that After the etching is completed, the dielectric film of the mask layer with the periodic pattern is not completely removed.
3. The product according to claim 2, It is characterized in that When etching is completed, the etching depth of the material to be etched is L, and the etching selectivity ratio of the material to be etched and the mask layer dielectric film is r = etching rate of the material to be etched / etching rate of the mask layer dielectric film, then the deposition thickness of the mask layer dielectric film is L / r±150nm.
4. The product according to claim 1, It is characterized in that The EPD spot area used for etching monitoring is S, the area of the periodic pattern on the material to be etched that is not covered by the mask layer is s, R=S / s, and within the EPD monitoring area, the number of pattern monomers covered by the EPD laser beam is N≥30, and 10%≤R≤80%.
5. The product according to claim 1, It is characterized in that The pattern monomer is in the shape of a circular ring or a polygonal ring.
6. The product according to claim 1, It is characterized in that The area of the etching monitoring area A is ≥ 2S, where S is the area of the EPD spot.
7. The product according to claim 1, It is characterized in that The mask layer material is SiO 2 .
8. A thin film assisted method for improving dry etching accuracy, It is characterized in that The method comprises: A mask layer is deposited on the material to be etched, and a device pattern and a periodic pattern are formed on the mask layer to obtain a dry etching product, wherein the device pattern is located in the device etching area B, and the periodic pattern is located in the etching monitoring area A, and the periodic pattern includes a plurality of pattern monomers, each of which is annular, and the plurality of pattern monomers are arranged in an array of M rows and N columns, and the surface of the material to be etched that is not covered by the periodic pattern is completely exposed; Place the dry-etched product into the dry-etching chamber and set the etching program; Turn on the EPD laser and adjust the position of the laser spot so that the laser spot covers the periodic pattern of the etching monitoring area A; The etching monitoring area A and the device etching area B of the dry etching product are etched simultaneously, and the EPD signal is obtained. When the preset etching end point on the EPD monitoring curve is reached, the etching program is stopped so that the etching depth of the device etching area B reaches the preset etching depth.
9. The method according to claim 8, It is characterized in that The method further comprises: Before the formal device etching, etching experiments are carried out on multiple samples of dry etching products to determine the preset etching endpoint on the EPD monitoring curve and the preset etching depth of the corresponding device etching area B.
10. The method according to claim 9, It is characterized in that The etching experiment includes: Etch the target sample of the dry-etched product, and when the EPD monitoring curve of the etching monitoring area A of the target sample reaches the target end point, stop the etching program, take out the target sample, and detect the target etching depth of the device etching area B of the target sample; If it is determined that the difference between the target etching depth and the preset etching depth is greater than the preset threshold, the EPD curve end point of the next sample is modified, and the above steps are repeated until the difference between the etching depth of the final sample and the preset etching depth is less than the preset threshold, and the EPD curve end point of the final sample is the preset etching end point.