Test structure, failure positioning method and failure analysis method
By introducing positioning structures and dummy metal wires into the chain test structure, combining the voltage contrast principle and scale lines, the problem of low positioning efficiency of breakpoints of super-large chain structures is solved, and fast and accurate failure positioning and analysis are achieved.
Patent Information
- Application Number
- CN202411037918.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-11-19
AI Technical Summary
The prior art cannot accurately locate the circuit breaker of the ultra-large chain test structure, and it requires multiple entry and exit of the nanoprobe machine, reducing the failure positioning efficiency.
A test structure is designed, including chain structure and dummy metal wire. By setting a positioning structure between the chain structure and dummy metal wire, the positioning structure corresponds to the number of metal layers in the chain structure and the number of rows. The failure position is quickly positioned and the coordinates of the failure position are determined through electron beam scanning and scale marks.
The efficiency and accuracy of failure positioning are improved, and the number of times when marking near the break point and returning to the test machine to confirm the relative position is reduced. It directly enters the FIB machine for TEM sample preparation to determine the cause of failure.
Smart Images

Figure CN118983301A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of semiconductor production, and in particular to a test structure, a failure location method and a failure analysis method. Background Art
[0002] Open circuit failure is the most common failure phenomenon in the semiconductor manufacturing process. It is mainly caused by design problems and / or process problems. A large voltage drop will occur at the open circuit, blocking the normal operation of the entire circuit. In order to monitor or evaluate process stability and design reliability, it is usually necessary to extract the structure with open circuit risk and use this structure to form a repeated, large-area, and easy-to-test structure for testing. Open circuit test is a common test item in wafer process control detection (Wafer Acceptable Test, WAT). It has a variety of different test structures, involving almost all levels in the semiconductor manufacturing process, and should have the characteristics of easy testing and easy failure analysis. However, when designing the test structure, designers often ignore the characteristics that the structure should be easy to locate and analyze failures. The test structure area is designed to be larger and larger, which increases the difficulty of locating, slicing, and analyzing the failure point.
[0003] There are many large-area test structures for monitoring circuit breaks. The most common structure is the chain test structure, such as Figures 1 to 3 As shown in the figure, the resistance of the entire chain structure is tested to determine whether the metal circuit has a short circuit failure. If a short circuit failure occurs, the structure needs to be analyzed for failure, that is, the short circuit point is found by using electrical and physical analysis methods and the physical manifestation of the metal short circuit is determined, and finally the root cause of the metal short circuit is deduced. Among them, the location of the short circuit failure point by using electrical analysis methods is the most critical step in the entire analysis process.
[0004] At present, Active Voltage Contrast (AVC) is the most commonly used method to locate the short circuit failure point of a super-large chain test structure. AVC is a function of a nanoprobe machine, which uses the nanoprobe machine to artificially set one end of the chain test structure to a positive potential and the other end to a negative potential. At this time, the structure where the short circuit failure occurs will be divided into a positive potential structure and a negative potential structure with the short circuit point as the dividing point. Then the entire chain structure is scanned by an electron beam, and positive charges accumulate on the surface of the positive potential structure. Since the positive charges will attract secondary electrons escaping from the sample surface, the number of secondary electrons collected by the scanning electron microscope (SEM) probe will decrease; negative charges accumulate on the surface of the negative potential structure, and the negative charges will repel secondary electrons escaping from the sample surface, so that the number of secondary electrons collected by the SEM probe will increase. In this way, the number of secondary electrons collected by the SEM probe at the negative potential structure is greater than that at the positive potential structure, and the brightness displayed by the negative potential structure will be greater than that displayed by the positive potential structure. Therefore, the entire chain structure will show obvious light and dark differences with the break point as the dividing line, and the light and dark intersection point is the break failure point.
[0005] At present, a major disadvantage of using AVC to locate the failure point of the circuit breaker of a super-large chain test structure is that the AVC function can only be implemented in the nanoprobe machine. In this way, the test structure that needs to use AVC to locate the failure point of the circuit breaker can only show the difference in light and dark in the nanoprobe machine. Once the sample is taken out of the nanoprobe machine, the circuit breaker cannot be seen. If the circuit breaker is located at the edge of the test structure, the AVC image can be scanned and stored, and then the circuit breaker can be located by the digital structure and slice analysis can be performed. However, if the area of the test structure is extremely large and the circuit breaker is located in the middle of the test structure, it is still very difficult to perform a slice analysis on the circuit breaker. Although it is possible to make a mark near the circuit breaker and then return to the test machine to confirm the relative position of the mark and the circuit breaker, thereby achieving the precise positioning requirements of FIB (Focused Ion Beam) sample preparation, this requires at least 2 to 3 times of entering and exiting the nanoprobe machine.
[0006] Based on this, how to quickly locate the breaking point of the super-large chain test structure and reduce the number of times the sample enters and exits the nanoprobe machine has become a technical problem that technicians in this field need to solve. Summary of the invention
[0007] The purpose of the present invention is to provide a test structure, a failure location method and a failure analysis method to solve the problem in the prior art that the breaking point of the ultra-large chain test structure cannot be accurately located and the nanoprobe machine needs to be entered and exited multiple times, thereby reducing the failure location efficiency.
[0008] In order to achieve the above object, the present invention provides a test structure, including: a chain structure and a dummy metal wire;
[0009] The chain structure includes a first metal layer, a second metal layer and a through hole, wherein the first metal layer is located one level above the second metal layer, and the first metal layer is connected to the second metal layer through the through hole; the first metal layer is arranged at intervals along a first direction to form a plurality of columns, and is arranged at intervals along a second direction to form a plurality of rows;
[0010] The dummy metal wire is filled around the chain structure;
[0011] A positioning structure is arranged between the chain structure and the dummy metal wire. The positioning structure is arranged corresponding to the number of columns and rows of the first metal layer and is used to locate a position of a certain first metal layer in the chain structure.
[0012] Optionally, the chain structure has a relative first side and a second side along the first direction, and the positioning structure is arranged on the first side and / or the second side; the chain structure has a relative third side and a fourth side along the second direction, and the positioning structure is arranged on the third side and / or the fourth side.
[0013] Optionally, the positioning structure is aligned with the middle of the corresponding first metal layer.
[0014] Optionally, the positioning structure includes a first positioning ruler and a second positioning ruler;
[0015] The first positioning ruler extends along the first direction, and first scale lines are arranged at intervals along the first direction, and the distance between two adjacent first scale lines matches the distance between two adjacent first metal layers along the first direction, or the distance between two adjacent first scale lines matches the distance between a plurality of adjacent first metal layers along the first direction;
[0016] The second positioning ruler extends along the second direction, and second scale lines are arranged at intervals along the second direction, and the distance between two adjacent second scale lines is adapted to the distance between two adjacent first metal layers along the second direction, or the distance between two adjacent second scale lines is adapted to the distance between several adjacent first metal layers along the second direction.
[0017] Optionally, the first scale lines extend along the second direction, and some of the first scale lines have different extension lengths along the second direction, and the distance between two adjacent first scale lines having the same extension length along the second direction matches the distance between two adjacent first metal layers along the first direction, or the distance between two adjacent first scale lines having the same extension length along the second direction matches the distance between a plurality of adjacent first metal layers along the first direction;
[0018] The second scale lines extend along the first direction, and some of the second scale lines have different extension lengths along the first direction. The distance between two adjacent second scale lines having the same extension length along the first direction matches the distance between two adjacent first metal layers along the second direction, or the distance between two adjacent second scale lines having the same extension length along the first direction matches the distance between several adjacent first metal layers along the second direction.
[0019] Optionally, scale marks are provided on one side of the first scale line and the second scale line, and the scale marks are used to determine the positions corresponding to the first scale line and the second scale line.
[0020] Optionally, the positioning structure and the chain structure are integrally etched and formed.
[0021] In order to achieve the above object, the present invention also provides a failure location method, comprising:
[0022] Providing a sample having the test structure as described above, wherein the sample has a failure position;
[0023] The first metal layer has a silicon carbide layer therein, the sample is ground to the silicon carbide layer of the first metal layer, and the sample is subjected to electron beam scanning to determine that the boundary between light and dark is the failure position;
[0024] Moving the field of view of the test machine along the first direction, and determining the coordinates of the failure position along the second direction by means of the positioning structure;
[0025] Return to the failure position, move the field of view of the test platform along the second direction, and determine the coordinates of the failure position along the first direction through the positioning structure.
[0026] Optionally, determining the coordinates of the failure position by using the positioning structure includes:
[0027] The corresponding coordinates of the failure position are determined by the scale marks on the first scale line and the second scale line.
[0028] In order to achieve the above object, the present invention also provides a failure analysis method, comprising:
[0029] Using the failure analysis method as described above, the failure position is located;
[0030] TEM sample preparation is performed based on the coordinates of the failure location to determine the cause of the failure.
[0031] Compared with the existing test structure, the test structure, failure location method and failure analysis method provided by this application have the following advantages:
[0032] The test structure provided in the present application adds a positioning structure between the chain structure and the dummy metal wire, and sets the positioning structure corresponding to the number of rows and columns of the first metal layer in the chain structure. This allows the operator to locate the failure position through the positioning structure after discovering the failure position when testing the ultra-large area chain structure, thereby avoiding the prior art of marking near the break point and returning to the test machine multiple times to confirm the relative position of the mark and the break point, thereby improving the efficiency and accuracy of failure location.
[0033] The failure location method provided in the present application uses the above-mentioned test structure. After the operator finds the boundary between light and dark as the failure location through the voltage contrast principle, the test platform can be moved in the first direction and the second direction respectively, and the coordinates of the failure location can be confirmed in combination with the positioning structure, thereby avoiding returning to the platform multiple times to determine the relative position of the breakpoint, thereby improving the efficiency and accuracy of failure location.
[0034] The failure analysis method provided in the present application, by using the above-mentioned failure location method, can directly enter the FIB machine and prepare TEM samples according to the coordinates of the failure position, and finally determine the failure mechanism leading to the failure through the TEM machine, thereby further improving the efficiency and accuracy of failure analysis. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 is a schematic diagram of a test structure in the prior art;
[0036] Figure 2 It is a schematic diagram of a chain structure in the prior art;
[0037] Figure 3 It is a cross-sectional view of a chain structure in the prior art;
[0038] Figure 4 A schematic diagram of a first test structure provided by an embodiment of the present invention;
[0039] Figure 5 A schematic diagram of a second test structure provided by an embodiment of the present invention;
[0040] Figure 6 A schematic diagram of a third test structure provided by an embodiment of the present invention;
[0041] Figure 7 A flowchart of a failure location method provided by an embodiment of the present invention;
[0042] Figure 8 A schematic diagram of a test structure provided by an embodiment of the present invention during a failure location process;
[0043] Fig. 9 A schematic diagram of reading coordinates of a test structure provided by an embodiment of the present invention during a failure location process;
[0044] Fig.10 A flowchart of a failure analysis method provided by an embodiment of the present invention;
[0045] The description of each reference numeral is as follows:
[0046] 1-chain structure; 10-first metal layer; 11-second metal layer; 12-through hole; 13-first side; 14-second side; 15-third side; 16-fourth side;
[0047] 2-dummy metal wire;
[0048] 3-positioning structure; 30-first positioning ruler; 31-second positioning ruler; 300-first scale line; 310-second scale line;
[0049] X-first direction; Y-second direction. DETAILED DESCRIPTION
[0050] In order to make the purpose, advantages and features of the present invention clearer, the present invention is further described in detail below in conjunction with the accompanying drawings and specific embodiments. It should be noted that the drawings are all in a very simplified form and are not drawn to scale, and are only used to conveniently and clearly assist in explaining the purpose of the embodiments of the present invention. In addition, the structure shown in the drawings is often a part of the actual structure. In particular, the emphasis of each drawing is different, and sometimes different scales are used.
[0051] As used in this specification, the singular forms "a", "an" and "the" include plural objects, the term "or" is generally used to include the meaning of "and / or", the term "several" is generally used to include the meaning of "at least one", and the term "at least two" is generally used to include the meaning of "two or more". In addition, the terms "first", "second" and "third" are used for descriptive purposes only and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Therefore, the features defined as "first", "second" and "third" may explicitly or implicitly include one or at least two of the features, "one end" and "the other end" and "the proximal end" and "the distal end" generally refer to two corresponding parts, which include not only the endpoints, and the terms "installed", "connected" and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral body; it can be directly connected or indirectly connected through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements. In addition, as used in this specification, an element disposed on another element generally only indicates that there is a connection, coupling, cooperation or transmission relationship between the two elements, and the connection, coupling, cooperation or transmission between the two elements may be direct or indirect through an intermediate element, and it cannot be understood as indicating or implying the spatial position relationship between the two elements, that is, one element may be in any orientation such as inside, outside, above, below or on one side of another element, unless the content clearly indicates otherwise. The terms "upper", "lower", "top" and "bottom" are generally relative position relationships arranged in the direction of gravity; the terms "vertical, vertical direction" generally refer to the direction of gravity, which is generally perpendicular to the ground, and "horizontal, horizontal plane direction" generally refers to the direction parallel to the ground; for ordinary technicians in this field, the specific meanings of the above terms in this specification can be understood according to specific circumstances.
[0052] The purpose of the present invention is to provide a test structure, a failure location method and a failure analysis method to solve the problem in the prior art that the breaking point of the ultra-large chain test structure cannot be accurately located and the nanoprobe machine needs to be entered and exited multiple times, thereby reducing the failure location efficiency.
[0053] Those skilled in the art can understand, please refer to Figures 1 to 3In the existing testing process of ultra-large area chain structures, nanoprobe machines are often used and the AVC (Active Voltage Contrast) function is used to make the ultra-large area chain structure show the light and dark contrast difference. However, due to the large area of the chain structure, there is no characteristic pattern near the intersection of the light and dark difference. Once the nanoprobe machine is left, the specific position of the intersection of the light and dark difference cannot be observed. Therefore, the operator is required to form a mark near the intersection of the light and dark difference, and repeatedly confirm the relative position between the intersection of the light and dark difference and the mark through the nanoprobe machine, so as to locate the failure position. This method has high repeatability and is time-consuming, which seriously affects the efficiency and accuracy of failure analysis. Based on this, the present application adds a positioning structure between the chain structure and the dummy metal wire, so that the operator can quickly read the coordinates of the failure position, avoid the phenomenon of repeatedly entering the machine to obtain the relative position, and improve the efficiency and accuracy of failure positioning.
[0054] For further information, please refer to Figures 1 to 6 , it can be understood by those skilled in the art that dummy (pseudo device) refers to a semiconductor element or structure without function, generally refers to a structure used to fill unused areas in a chip to ensure that the structure and performance of other parts can be maintained. These fillers are usually made of the same material as the chip, but will not be used for any circuit or logic function. Dummy has the functions of filling blank areas in the chip manufacturing process, ensuring manufacturability, and avoiding the influence of clutter on key signals in the chip. In addition, dummy can also be used to test the performance and reliability of the chip. The dummy metal wire 2 in the present embodiment is used to fill the blank areas.
[0055] Please continue to refer to Figures 1 to 6 The present invention provides a test structure, including: a chain structure 1 and a dummy metal wire 2; the chain structure 1 includes a first metal layer 10, a second metal layer 11 and a through hole 12, the first metal layer 10 is located at the upper level of the second metal layer 11, and the first metal layer 10 is connected to the second metal layer 11 through the through hole 12; the first metal layer 10 is arranged in a first direction X to form a plurality of columns, and is arranged in a second direction Y to form a plurality of rows; the dummy metal wire 2 is filled around the chain structure 1; a positioning structure 3 is arranged between the chain structure 1 and the dummy metal wire 2, and the positioning structure 3 is arranged corresponding to the number of columns and rows of the first metal layer 10, and is used to locate the position of a first metal layer 10 in the chain structure 1. For explanation, please refer to Figure 3In this embodiment, the first metal layer 10 and the second metal layer 11 are both short sections of metal wires, and the two ends of the metal wires along the first direction X are connected to the two ends of the metal wires of another layer through the through holes 12 in a one-to-one correspondence, and the metal wires are sequentially connected along the first direction X to form a row of chain structures 1, and the two ends of each row of chain structures 1 along the first direction X are connected to chain structures 1 in a second direction Y, thereby forming multiple rows of chain structures 1. At the same time, in each row of chain structures 1, each metal wire forms multiple columns of chain structures 1, and the metal wires in each row are arranged in a one-to-one correspondence, forming a structure as shown in FIG. Figure 4 The chain structure 1 is shown. The first direction X and the second direction Y are perpendicular to each other. Of course, in other embodiments, the first direction X and the second direction Y can also be set at other angles. Please continue to refer to Figure 4 In this embodiment, a positioning structure 3 is provided between the chain structure 1 and the dummy metal wires 2 located around it. The positioning structure 3 in this embodiment is a positioning scale with scale lines provided thereon, and each scale line corresponds to the position of the first metal layer 10. In an optional embodiment, the positioning structure 3 and the chain structure 1 are integrally etched.
[0056] As an optional embodiment, in Figures 4 to 6 In the illustrated embodiment, the positioning structure 3 is aligned with the middle of the first metal layer 10, that is, the scale line is aligned with the center of the metal line. In other embodiments, the positioning structure 3 may also be aligned with the edge of the first metal layer 10, or the positioning structure 3 may also be aligned with the position of the through hole 12. Those skilled in the art may reasonably configure the relative position between the positioning structure 3 and the first metal layer 10 according to actual conditions, and this embodiment does not limit this.
[0057] In this configuration, by adding a positioning structure 3 between the chain structure 1 and the dummy metal wire 2, and setting the positioning structure 3 corresponding to the number of rows and columns of the first metal layer 10 in the chain structure 1, the operator can locate the failure position through the positioning structure 3 after discovering the failure position when testing the ultra-large area chain structure 1, thereby avoiding the prior art of marking near the break point and returning to the test machine multiple times to confirm the relative position of the mark and the break point, thereby improving the efficiency and accuracy of failure location.
[0058] Please refer to Figures 4 to 5 As an optional embodiment, the chain structure 1 has a first side 13 and a second side 14 opposite to each other along the first direction X, and the positioning structure 3 is arranged on the first side 13 and / or the second side 14; the chain structure 1 has a third side 15 and a fourth side 16 opposite to each other along the second direction Y, and the positioning structure 3 is arranged on the third side 15 and / or the fourth side 16. Figure 4In the illustrated example, the positioning structure 3 is only disposed on the first side 13 and the third side 15 of the chain structure 1. In other embodiments, the positioning structure 3 may also be disposed on the second side 14 and the third side 15 of the chain structure 1, or the first side 13 and the fourth side 16, or the second side 14 and the fourth side 16. It is only necessary to dispose the positioning structure 3 on at least one side of the chain structure 1 along the first direction X and one side of the chain structure 1 along the second direction Y. In other embodiments, if the number of columns of the chain structure 1 along the first direction X or the number of rows along the second direction Y is too large, it is also possible to consider disposing the positioning structure 3 on both sides of the chain structure 1 along the first direction X or both sides of the chain structure 1 along the second direction Y, so as to facilitate the operator to observe the positioning. As a preferred embodiment, please refer to Figure 5 The positioning structure 3 can also be set on both sides of the chain structure 1 along the first direction X, and on both sides of the chain structure 1 along the second direction Y. With this configuration, the operator can determine the moving direction of the test machine according to the area where the light and dark contrast intersection point is located, so that the positioning structure 3 can be observed after moving a short distance, further improving the efficiency of failure location.
[0059] Please refer to Figure 4 and Figure 6 The positioning structure 3 includes a first positioning ruler 30 and a second positioning ruler 31; the first positioning ruler 30 extends along the first direction X, and first scale lines 300 are arranged at intervals along the first direction X, and the distance between two adjacent first scale lines 300 is adapted to the distance between two adjacent first metal layers 10 along the first direction X, or the distance between two adjacent first scale lines 300 is adapted to the distance between several adjacent first metal layers 10 along the first direction X; the second positioning ruler 31 extends along the second direction Y, and second scale lines 310 are arranged at intervals along the second direction Y, and the distance between two adjacent second scale lines 310 is adapted to the distance between two adjacent first metal layers 10 along the second direction Y, or the distance between two adjacent second scale lines 310 is adapted to the distance between several adjacent first metal layers 10 along the second direction Y. Figure 4 In the illustrated example, the first scale lines 300 on the first positioning ruler 30 are arranged in one-to-one correspondence with the first metal layers 10 in the chain structure 1 in a row, and the distance between two adjacent first scale lines 300 is equal to the distance between two adjacent first metal layers 10; the second scale lines 310 on the second positioning ruler 31 are arranged in one-to-one correspondence with the first metal layers 10 in the chain structure 1 in a column, and the distance between two adjacent second scale lines 310 is equal to the distance between two adjacent first metal layers 10. Figure 6In the illustrated example, the first scale lines 300 on the first positioning ruler 30 are spaced apart by one first metal layer 10, i.e., the distance between two adjacent first scale lines 300 is equal to the distance between three first metal layers 10; similarly, the second scale lines 310 on the second positioning ruler 31 are spaced apart by one first metal layer 10, i.e., the distance between two adjacent second scale lines 310 is equal to the distance between three first metal layers 10. It should be noted that Figure 6 In the figure, the distance between the three first metal layers 10 is the distance between the middle of the first first metal layer 10 and the middle of the third first metal layer 10. In other embodiments, two adjacent scale lines may be separated by two first metal layers 10, three first metal layers 10 or even more first metal layers 10. Those skilled in the art may reasonably configure the scale lines according to the area of the chain structure 1, and this embodiment does not limit this.
[0060] For further information, please continue to refer to Figure 4 and Figure 6 , the first scale lines 300 extend along the second direction Y, and some of the first scale lines 300 have different extension lengths along the second direction Y, and the distance between two adjacent first scale lines 300 having the same extension length along the second direction Y matches the distance between two adjacent first metal layers 10 along the first direction X, or, the distance between two adjacent first scale lines 300 having the same extension length along the second direction Y matches the distance between several adjacent first metal layers 10 along the first direction X; the second scale lines 310 extend along the first direction X, and some of the second scale lines 310 have different extension lengths along the first direction X, and the distance between two adjacent second scale lines 310 having the same extension length along the first direction X matches the distance between two adjacent first metal layers 10 along the second direction Y, or, the distance between two adjacent second scale lines 310 having the same extension length along the first direction X matches the distance between several adjacent first metal layers 10 along the second direction Y. Figure 4 In the illustrated example, five first metal layers 10 are spaced between first scale lines 300 with a longer extension length along the second direction Y, and the spacing between first scale lines 300 with a shorter extension length along the second direction Y is equal to the spacing between two adjacent first metal layers 10; five first metal layers 10 are spaced between second scale lines 310 with a longer extension length along the first direction X, and the spacing between second scale lines 310 with a shorter extension length along the first direction X is equal to the spacing between two adjacent first metal layers 10. Figure 6In the illustrated example, ten first metal layers 10 are spaced between first scale lines 300 with longer extension lengths along the second direction Y, and two first metal layers 10 are spaced between first scale lines 300 with shorter extension lengths along the second direction Y; ten first metal layers 10 are spaced between second scale lines 310 with longer extension lengths along the first direction X, and two first metal layers 10 are spaced between second scale lines 310 with shorter extension lengths along the first direction X. In other embodiments, more first metal layers 10 may be spaced between scale lines of different lengths, and those skilled in the art may reasonably configure the setting of the scale lines according to the area of the chain structure 1, and this embodiment does not limit this.
[0061] As an optional embodiment, a scale mark (not shown in the figure) is set on one side of the first scale line 300 and the second scale line 310, and the scale mark is used to determine the position corresponding to the first scale line 300 and the second scale line 310. It should be noted that the scale mark can be a digital mark or a shape mark, and the scale mark can be set at any position around the scale line as long as it is not confused with the scale marks of other scale lines. The digital mark can be an Arabic numeral or a Roman numeral. For example, in Figure 4 A "0" or "1" is marked near the first scale line 300 corresponding to the first column of the first metal layer 10; the shape mark can be a marking point, a marking line or a marking figure (such as a rectangle, a circle, a triangle or other irregular figures, etc.), for example, Figure 4 A point is marked near the second scale line 310 corresponding to the first row of the first metal layer 10, two points are marked near the second scale line 310 corresponding to the fifth row of the first metal layer 10, and so on. Those skilled in the art can configure the scale markings according to actual conditions.
[0062] In another embodiment, please refer to Figures 4 to 9 The present invention also provides a failure location method, comprising:
[0063] Step S1: Provide a sample having the test structure as described above, the sample having a failure position (such as Figures 4 to 6 shown);
[0064] Step S2: The first metal layer 10 has a silicon carbide layer (not shown in the figure), the sample is ground to the silicon carbide layer of the first metal layer 10, and the sample is scanned by an electron beam to determine that the bright and dark junction is the failure position (such as Figure 8 shown);
[0065] Step S3: Move the field of view of the test machine along the first direction X, and determine the coordinates of the failure position along the second direction Y (such as Fig. 9 shown);
[0066] Step S4: Return to the failure position, move the field of view of the test machine along the second direction Y, and determine the coordinates of the failure position along the first direction X (such as Fig. 9 shown).
[0067] It should be noted that in step S2, the sample is ground to the silicon carbide layer of the first metal layer 10, and the two ends of the test structure are ground out using the FIB machine to facilitate the insertion of the nanoprobe, and then the ground sample is placed in the nanoprobe machine, and two nanoprobes are respectively inserted into the two ends of the test structure that have been ground out, one end is placed at a high potential, and the other end is placed at a point, and after the voltage difference is constructed, the sample is scanned using the electron beam in the nanoprobe machine, and the boundary between light and dark is found using the voltage contrast principle, which is the failure position of the sample. In steps S3 and S4, it is only necessary to move the field of view of the nanoprobe machine to the edge area of the test structure along the first direction X and the second direction Y respectively, and the coordinates of the failure position can be accurately located by the first positioning ruler 30 and the second positioning ruler 31.
[0068] With such configuration, by using the above-mentioned test structure, after the operator finds the boundary between light and dark as the failure position through the voltage contrast principle, the test platform can be moved along the first direction X and the second direction Y respectively, and the coordinates of the failure position can be confirmed in combination with the positioning structure 3, thereby avoiding returning to the platform multiple times to determine the relative position of the breakpoint, thereby improving the efficiency and accuracy of failure location.
[0069] Furthermore, the coordinates of the failure position are determined by the positioning structure 3, including:
[0070] Step S3 - 1 : Determine the corresponding coordinates of the failure position through the scale marks on the first scale line 300 and the second scale line 310 .
[0071] It should be noted that in the above steps S3 and S4, after the operator moves the field of view of the nanoprobe machine to the edge area of the test structure, the first scale line 300 and the second scale line 310 corresponding to the failure position can be determined. At this time, the corresponding coordinates of the failure position can be determined by the scale marks (numbers or corresponding graphics, etc.) set nearby. For example, Fig. 9 In the illustrated example, the failure position is located at the connection position between the two first metal layers 10 at the coordinate points (17, 18) and (18, 18), so that the failure position can be accurately located.
[0072] In another embodiment, please refer to Fig.10 The present invention also provides a failure analysis method, comprising:
[0073] Step S10: locating the failure position by the failure analysis method as described above;
[0074] Step S20: TEM sample preparation is performed based on the coordinates of the failure position to determine the failure cause.
[0075] As can be understood by those skilled in the art, TEM (Transmission Electron Microscope) is generally used to analyze sample morphology, metallographic structure and sample composition. TEM uses electron beams to bombard samples. Some electrons can penetrate the sample surface. The detector located under the sample collects the electrons that penetrate the sample to form an image, thereby analyzing the failure mechanism of the sample based on the impact. It should be noted that when preparing TEM samples, it is necessary to use a FIB machine to perform fixed-point sampling and extraction of the sample.
[0076] With such configuration, by using the above-mentioned failure location method, it is possible to directly enter the FIB machine and prepare the TEM sample according to the coordinates of the failure position, and finally determine the failure mechanism leading to the failure through the TEM machine, further improving the efficiency and accuracy of failure analysis.
[0077] In summary, in the test structure, failure location method and failure analysis method provided in the embodiments of the present invention, the test structure includes: a chain structure and a dummy metal wire; the chain structure includes a first metal layer, a second metal layer and a through hole, the first metal layer is located at the upper level of the second metal layer, and the first metal layer is connected to the second metal layer through the through hole; the first metal layer is arranged at intervals along the first direction to form a plurality of columns, and is arranged at intervals along the second direction to form a plurality of rows; the dummy metal wire is filled around the chain structure; a positioning structure is arranged between the chain structure and the dummy metal wire, and the positioning structure is arranged corresponding to the number of columns and rows of the first metal layer, and is used to locate the position of a certain first metal layer in the chain structure.
[0078] With such a configuration, by adding a positioning structure between the chain structure and the dummy metal wire, and setting the positioning structure corresponding to the number of rows and columns of the first metal layer in the chain structure, the operator can locate the failure position through the positioning structure after discovering the failure position when testing the ultra-large area chain structure, thereby avoiding the prior art of marking near the break point and returning to the test machine multiple times to confirm the relative position of the mark and the break point, thereby improving the efficiency and accuracy of failure location.
[0079] Furthermore, by using the above-mentioned test structure, after the operator finds the boundary between light and dark as the failure position through the voltage contrast principle, the test machine can be moved in the first direction and the second direction respectively, and the coordinates of the failure position can be confirmed in combination with the positioning structure, thereby avoiding returning to the machine multiple times to determine the relative position of the breakpoint, thereby improving the efficiency and accuracy of failure location.
[0080] Furthermore, by using the above-mentioned failure location method, it is possible to directly enter the FIB machine and prepare TEM samples according to the coordinates of the failure position, and finally determine the failure mechanism leading to the failure through the TEM machine, further improving the efficiency and accuracy of failure analysis.
[0081] The above description is only a description of the preferred embodiments of the present invention, and is not intended to limit the scope of the present invention. Any changes or modifications made by a person skilled in the art in the field of the present invention based on the above disclosure shall fall within the scope of protection of the claims.
Claims
1. A test structure, characterized in that: include: Chain structure and dummy metal wire; The chain structure includes a first metal layer, a second metal layer and a through hole, wherein the first metal layer is located one level above the second metal layer, and the first metal layer is connected to the second metal layer through the through hole; the first metal layer is arranged at intervals along a first direction to form a plurality of columns, and is arranged at intervals along a second direction to form a plurality of rows; The dummy metal wire is filled around the chain structure; A positioning structure is arranged between the chain structure and the dummy metal wire. The positioning structure is arranged corresponding to the number of columns and rows of the first metal layer and is used to locate a position of a certain first metal layer in the chain structure.
2. The test structure according to claim 1, characterized in that The chain structure has a first side and a second side relative to each other along the first direction, and the positioning structure is arranged on the first side and / or the second side; the chain structure has a third side and a fourth side relative to each other along the second direction, and the positioning structure is arranged on the third side and / or the fourth side.
3. The test structure according to claim 1, characterized in that: The positioning structure is aligned with the middle portion of the corresponding first metal layer.
4. The test structure according to claim 1, characterized in that: The positioning structure includes a first positioning ruler and a second positioning ruler; The first positioning ruler extends along the first direction, and first scale lines are arranged at intervals along the first direction, and the distance between two adjacent first scale lines matches the distance between two adjacent first metal layers along the first direction, or the distance between two adjacent first scale lines matches the distance between a plurality of adjacent first metal layers along the first direction; The second positioning ruler extends along the second direction, and second scale lines are arranged at intervals along the second direction, and the distance between two adjacent second scale lines is adapted to the distance between two adjacent first metal layers along the second direction, or the distance between two adjacent second scale lines is adapted to the distance between several adjacent first metal layers along the second direction.
5. The test structure according to claim 4, characterized in that: The first scale lines extend along the second direction, some of the first scale lines have different extension lengths along the second direction, the distance between two adjacent first scale lines having the same extension length along the second direction matches the distance between two adjacent first metal layers along the first direction, or the distance between two adjacent first scale lines having the same extension length along the second direction matches the distance between a plurality of adjacent first metal layers along the first direction; The second scale lines extend along the first direction, and some of the second scale lines have different extension lengths along the first direction. The distance between two adjacent second scale lines having the same extension length along the first direction matches the distance between two adjacent first metal layers along the second direction, or the distance between two adjacent second scale lines having the same extension length along the first direction matches the distance between several adjacent first metal layers along the second direction.
6. The test structure according to claim 4 or 5, characterized in that: A scale mark is disposed on one side of each of the first scale mark and the second scale mark, and the scale mark is used to determine the positions corresponding to the first scale mark and the second scale mark.
7. The test structure according to claim 1, characterized in that: The positioning structure and the chain structure are integrally etched and formed.
8. A failure location method, characterized in that: include: Providing a sample having a test structure as claimed in any one of claims 1 to 7, wherein the sample has a failure position; The first metal layer has a silicon carbide layer therein, the sample is ground to the silicon carbide layer of the first metal layer, and the sample is subjected to electron beam scanning to determine that the boundary between light and dark is the failure position; Moving the field of view of the test machine along the first direction, and determining the coordinates of the failure position along the second direction by means of the positioning structure; Return to the failure position, move the field of view of the test platform along the second direction, and determine the coordinates of the failure position along the first direction through the positioning structure.
9. The failure location method according to claim 8, characterized in that: The determining the coordinates of the failure position by the positioning structure includes: The corresponding coordinates of the failure position are determined by the scale marks on the first scale line and the second scale line.
10. A failure analysis method, characterized in that: include: Locating the failure position by the failure analysis method according to any one of claims 8 to 9; TEM sample preparation is performed based on the coordinates of the failure location to determine the cause of the failure.