Electrode plate and preparation method thereof, ion battery and vehicle
By using a pore-making composition composed of high boiling point organic solvent and water, the drying process is controlled to ensure that the electrode sheet maintains porosity after rolling, solving the problem of the electrode sheet reducing porosity after rolling, and improving the performance of the battery stability.
Patent Information
- Application Number
- CN202411058059.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-02
- Publication Date
- 2024-11-19
AI Technical Summary
The pore-making effect of the electrode sheet is affected during the rolling process, and the porosity is reduced, especially the formation of closed openings on the coating surface, which affects the performance of the battery.
The pore-making composition consisting of high boiling point organic solvent and water is controlled to control the first drying temperature below the boiling point of the pore-making composition to ensure that water evaporates and retains the organic solvent. After rolling, the organic solvent is evaporated by the second drying. Pores are formed so as to maintain porosity at high compaction density.
Ensure that the electrode sheet maintains the proper porosity under high compaction density, improves the cycle stability and power density of the battery, and reduces the risk of cracking.
Smart Images

Figure BDA0004976993910000121
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of batteries, and in particular to an electrode sheet and a preparation method thereof, an ion battery and a vehicle. Background Art
[0002] The preparation process of electrode sheets generally includes homogenization, coating, drying, rolling and slicing. At present, pore-forming agents such as ammonium carbonate, ammonium chloride and ammonium bicarbonate are usually added during the homogenization process and decomposed to form pores during the drying process of the coating, so that the coating has abundant pores. However, the pores left by the decomposition of the pore-forming agent during the drying process will have a reduced porosity after rolling, especially on the surface of the coating, or closed holes will be formed after rolling, which will affect the pore-forming effect. Summary of the invention
[0003] Based on this, it is necessary to provide an electrode sheet and a preparation method thereof, an ion battery and a vehicle to address the above problems. The preparation method will not affect the pore-forming effect due to the rolling process, so that the electrode sheet can maintain the proper porosity while having a high compaction density.
[0004] A method for preparing an electrode sheet comprises the following steps:
[0005] The active layer material is mixed with a pore-forming composition to obtain a slurry, wherein the pore-forming composition comprises water and an organic solvent miscible with water, and the boiling point of the organic solvent is higher than that of water by more than 25° C.;
[0006] The slurry is coated on a current collector, and then subjected to a first drying, rolling and a second drying to obtain an electrode sheet, wherein the temperature of the first drying is lower than the boiling point of the pore-forming composition.
[0007] In one embodiment, the preparation method further satisfies at least one of the following conditions:
[0008] (1) The boiling point of the organic solvent is at least 30°C higher than that of water;
[0009] (2) the boiling point of the pore-forming composition is greater than or equal to 100° C.;
[0010] (3) the temperature of the first drying is at least 10° C. lower than the boiling point of the pore-forming composition;
[0011] (4) The second drying is vacuum drying.
[0012] In one embodiment, the preparation method further satisfies at least one of the following conditions:
[0013] (1) The boiling point of the pore-forming composition is 100°C-130°C;
[0014] (2) The boiling point of the organic solvent is 140°C-220°C;
[0015] (3) the temperature of the first drying is 10°C to 40°C lower than the boiling point of the pore-forming composition;
[0016] (4) The vacuum drying is carried out at a temperature of 90°C to 140°C and for a time of 20 min to 60 min.
[0017] In one embodiment, the organic solvent is selected from at least one of N-methylpyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, N-methylformamide, 1,2-propylene glycol, and ethylene glycol.
[0018] In one embodiment, the steps include:
[0019] Mixing the first graphite, the silicon-based material, the conductive agent, the binder and the pore-forming composition to obtain a first slurry;
[0020] Mixing a second graphite, a conductive agent, a binder and the pore-forming composition to obtain a second slurry;
[0021] The first slurry is coated on the current collector to form a first slurry layer, and the second slurry is coated on the first slurry layer to form a second slurry layer, and then the electrode sheet is obtained through a first drying, rolling, a second drying and slicing.
[0022] In one embodiment, the energy density of the first graphite active material is greater than the energy density of the second graphite active material, and the fast charging capability of the first graphite active material is less than the fast charging capability of the second graphite active material.
[0023] In one embodiment, the preparation method also meets at least one of the following conditions:
[0024] (1) The energy density of the first graphite is 355 mAh / g-365 mAh / g, and the upper limit of compaction density is 1.65 g / cm 3 -1.80g / cm 3 , fast charging capability is 1.5C-2C;
[0025] (2) The energy density of the second graphite is 340 mAh / g-355 mAh / g, and the upper limit of compaction density is 1.55 g / cm 3 -1.65g / cm 3 , fast charging capability is 4C-6C;
[0026] (3) The mass ratio of the silicon-based material, the first graphite, the conductive agent, the binder and the organic solvent in the first slurry is (3-8): (82-93): (1-2): (2-4): (1-4);
[0027] (4) The mass ratio of the second graphite, the conductive agent, the binder and the organic solvent in the second slurry is (92-98):(0.1-1):(1-3):(0.9-4);
[0028] (5) The silicon-based material is selected from at least one of pre-lithiation silicon oxygen, nano silicon or gas phase silicon carbon;
[0029] (6) the conductive agent in the first slurry and the second slurry is independently selected from at least one of conductive carbon black, conductive graphite, graphene, and single-walled / multi-walled carbon nanotubes;
[0030] (7) The binders in the first slurry and the second slurry are independently selected from at least one of styrene-butadiene rubber, sodium carboxymethyl cellulose, lithium carboxymethyl cellulose, lithium polyacrylate and sodium polyacrylate.
[0031] An electrode sheet obtained by the preparation method comprises a current collector and an active layer attached to at least one surface of the current collector.
[0032] In one embodiment, the electrode sheet includes a current collector and a first negative electrode active layer and a second negative electrode active layer sequentially attached to at least one surface of the current collector, wherein the first negative electrode active layer includes a first graphite, a silicon-based material, a conductive agent and a binder, and the second negative electrode active layer includes a second graphite, a conductive agent and a binder.
[0033] An ion battery comprises the electrode sheet.
[0034] A vehicle using the ion battery.
[0035] The present invention selects an organic solvent with a suitable boiling point and miscible with water to form a pore-forming composition with water, and controls the temperature in the first drying process to be lower than the boiling point of the pore-forming composition, thereby ensuring that only water is evaporated and removed while the organic solvent is retained in the first drying process, and the organic solvent is evaporated through a second drying after rolling to produce pores, so that the pore-forming effect is not affected by the rolling process, so that the electrode sheet can maintain a desired porosity under the condition of a high compaction density. DETAILED DESCRIPTION
[0036] For ease of understanding of the present invention, the present invention will be described in more detail below. However, it should be understood that the present invention can be implemented in many different forms and is not limited to the embodiments or examples described herein. On the contrary, the purpose of providing these embodiments or examples is to make the understanding of the disclosure of the present invention more thorough and comprehensive.
[0037] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific implementation methods or embodiments, and are not intended to limit the present invention. The optional scope of the term "and / or" used herein includes any one of two or more related listed items, and also includes any and all combinations of related listed items, and the combinations include any two related listed items, any more related listed items, or all related listed items.
[0038] The method for preparing an electrode sheet provided by the present invention comprises the following steps:
[0039] The active layer material is mixed with a pore-forming composition to obtain a slurry, wherein the pore-forming composition comprises water and an organic solvent miscible with water, and the boiling point of the organic solvent is higher than that of water by more than 20° C.;
[0040] The slurry is coated on a current collector, and then subjected to a first drying, rolling and a second drying to obtain an electrode sheet, wherein the temperature of the first drying is lower than the boiling point of the pore-forming composition.
[0041] After an organic solvent having a boiling point greater than that of water and miscible with water is combined with water to form a pore-forming composition, the temperature during the drying process is controlled to achieve the effect of evaporating water and organic solvent in sequence. However, if the boiling points of the organic solvent and water are too close, part of the organic solvent will evaporate along with the water. Therefore, in the preparation method of the electrode sheet of the present invention, by selecting an organic solvent miscible with water and having a boiling point 20°C higher than that of water to form a pore-forming composition with water, and controlling the temperature during the first drying process to be lower than the boiling point of the pore-forming composition, it is possible to ensure that only water is evaporated and removed during the first drying process while retaining the organic solvent, and the organic solvent is evaporated by the second drying after rolling to produce pores, so that the pore-forming effect will not be affected by the rolling process, so that the electrode sheet can maintain the proper porosity under the condition of high compaction density.
[0042] In addition, the organic solvent can also be used as a plasticizer to make the binder molecular chain in the active layer material softer, thereby improving the flexibility and plasticity of the electrode sheet and reducing the occurrence of cracking of the electrode sheet.
[0043] Furthermore, the boiling point of the organic solvent is preferably higher than the boiling point of water by more than 30°C, more preferably higher than 40°C, and / or the boiling point of the pore-forming composition is preferably greater than or equal to 100°C, more preferably 100°C-130°C, and / or the temperature of the first drying is preferably lower than the boiling point of the pore-forming composition by more than 10°C, more preferably 10°C-40°C, so as to be more conducive to evaporating only water and retaining the organic solvent during the first drying process, and at the same time, to improve the preparation efficiency.
[0044] Furthermore, the boiling point of the organic solvent is preferably less than or equal to 220°C. In this way, the organic solvent can be evaporated and removed without using an excessively high temperature during the second drying process. There will be no additional impurities introduced due to incomplete removal of the organic solvent that may affect the performance of the electrode sheet, and there will be no impact on the performance of components such as the binder due to excessively high temperature or problems such as cracking of the electrode sheet.
[0045] Furthermore, the boiling point of the organic solvent is preferably 140°C-220°C.
[0046] Optionally, the organic solvent is selected from at least one of N-methylpyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, N-methylformamide, 1,2-propylene glycol, and ethylene glycol.
[0047] Generally, the lower the gas pressure, the lower the boiling point of the solvent. Compared with normal pressure drying, in a vacuum environment, the solvent can be evaporated using a lower drying temperature and a shorter drying time, thereby avoiding adverse effects on the electrode sheet due to excessively high temperature or excessively long drying time. Therefore, the second drying is preferably vacuum drying. Furthermore, the vacuum drying temperature is preferably 90°C-140°C, and the time is preferably 20min-60min.
[0048] The preparation method of the electrode sheet of the present invention is applicable to the preparation method of the positive electrode sheet and the preparation method of the negative electrode sheet. If it is the preparation method of the positive electrode sheet, the active layer material generally includes components such as positive electrode active material, conductive agent, binder, dispersant, etc., and the composition and proportion are conventionally selected. If it is the preparation method of the negative electrode sheet, the active layer material generally includes costs such as negative electrode active material, conductive agent, binder, dispersant, etc., and the composition and proportion are also conventionally selected. The present invention does not make any special restrictions. In addition, in the slurry obtained by mixing the active layer material and the pore-forming composition, the amount of the pore-forming composition can be selected according to the requirements of the porosity. When the slurry is coated, it can be coated in a single layer, or in a double layer or multiple layers. When it is coated in a double layer or multiple layers, the pore-forming composition can be added to any slurry as needed, or the pore-forming composition can be added to all slurries. The present invention does not make any specific restrictions.
[0049] For example, in terms of negative electrode materials, silicon-based materials have extremely high theoretical specific capacity, as well as advantages such as abundant resources and moderate working potential. They are considered to be the most likely negative electrode active materials to replace graphite as the next generation of lithium-ion batteries. However, silicon-based materials undergo great volume changes during the lithium insertion / extraction process, which can lead to rapid degradation of battery performance. In response to this, the present invention uses the above-mentioned preparation method to provide a method for preparing an electrode sheet using silicon-based materials as negative electrode active materials, which specifically includes the following steps:
[0050] Mixing the first graphite, the silicon-based material, the conductive agent, the binder and the pore-forming composition to obtain a first slurry;
[0051] Mixing a second graphite, a conductive agent, a binder and the pore-forming composition to obtain a second slurry;
[0052] The first slurry is coated on the current collector to form a first slurry layer, and the second slurry is coated on the first slurry layer to form a second slurry layer, and then the electrode sheet is obtained through a first drying, rolling, a second drying and slicing.
[0053] Specifically, the electrode sheet includes a current collector and a first negative electrode active layer and a second negative electrode active layer sequentially stacked on the surface of the current collector.
[0054] In the present invention, the negative electrode active layer is provided in a double layer, and the silicon-based material is used only in the first negative electrode active layer, which can not only improve the energy density but also improve the stability of the electrode sheet.
[0055] At the same time, through the pore-forming composition, the first negative electrode active layer has abundant pores, which can accommodate the volume expansion of the silicon-based material, thereby improving the cycle stability of the battery. The second negative electrode active layer has abundant pores, which can accelerate the infiltration of the electrolyte in the electrode sheet and ion conduction, and help to improve the power density of the battery.
[0056] Furthermore, it is preferred that the energy density of the first graphite active material is greater than the energy density of the second graphite active material, and the fast charging capability of the first graphite active material is less than the fast charging capability of the second graphite active material, which is beneficial to simultaneously improve the fast charging capability and energy density of the battery.
[0057] Furthermore, it is preferred that the energy density of the first graphite is 355 mAh / g-365 mAh / g, and the upper limit of the compaction density is 1.65 g / cm 3 -1.80g / cm 3 , the fast charging capacity is 1.5C-2C; preferably, the energy density of the second graphite is 340mAh / g-355mAh / g, and the upper limit of the compaction density is 1.55g / cm 3 -1.65g / cm3 , the fast charging capacity is 4C-6C.
[0058] Furthermore, the mass ratio of the silicon-based material, the first graphite, the conductive agent, the binder and the organic solvent in the first slurry is (3-8):(82-93):(1-2):(2-4):(1-4); the mass ratio of the second graphite, the conductive agent, the binder and the organic solvent in the second slurry is (92-98):(0.1-1):(1-3):(0.9-4).
[0059] The present invention does not limit the selection of silicon-based materials, conductive agents and binders. Preferably, the silicon-based material is selected from at least one of pre-lithiated silicon oxide, nano silicon or gas phase silicon carbon; the conductive agents in the first slurry and the second slurry are independently selected from at least one of conductive carbon black, conductive graphite, graphene, and single-walled / multi-walled carbon nanotubes; the binders in the first slurry and the second slurry are independently selected from at least one of styrene-butadiene rubber, sodium carboxymethyl cellulose, lithium carboxymethyl cellulose, lithium polyacrylate and sodium polyacrylate.
[0060] Furthermore, the thickness of the first negative electrode active layer and the second negative electrode active layer are independently selected from 50 μm to 200 μm, and the compaction density of the electrode sheet is 1.55 g / cm 2 -1.7g / cm 2 .
[0061] The present invention utilizes cheap and readily available organic solvents and water to form a composition to create pores in the electrode sheet, does not require additional equipment support, has low cost, and the pore-making process is compatible with the current electrode sheet manufacturing process, and the method is scalable.
[0062] The present invention also provides an electrode sheet obtained by the preparation method, wherein the electrode sheet comprises a current collector and an active layer attached to at least one surface of the current collector.
[0063] It should be noted that the electrode sheet can be a positive electrode sheet or a negative electrode sheet, and the electrode sheet can maintain a proper porosity when having a high compaction density. For example, a silicon-based material is used as a negative electrode active material, and the electrode sheet obtained by the above preparation method includes a current collector and a first negative electrode active layer and a second negative electrode active layer sequentially attached to at least one surface of the current collector, wherein the first negative electrode active layer includes a first graphite, a silicon-based material, a conductive agent, and a binder, and the second negative electrode active layer includes a second graphite, a conductive agent, and a binder.
[0064] The present invention also provides an ion battery, which comprises the electrode sheet. The electrode sheet of the present invention can improve the wettability of the electrode sheet and enhance the ion transmission dynamics in the electrode sheet.
[0065] The present invention also provides a vehicle, wherein the vehicle uses the ion battery.
[0066] Hereinafter, the electrode sheet and its preparation method, the ion battery and the vehicle will be further described through the following specific embodiments.
[0067] Example 1
[0068] Artificial graphite (energy density is 355mAh / g, compaction density upper limit is 1.65g / cm 3 , fast charging capacity 2C), pre-lithiated silicon oxide, conductive carbon black, single-walled carbon nanotubes, carboxymethyl cellulose lithium, styrene-butadiene rubber, polyacrylate lithium, N,N-dimethylacetamide and deionized water are mixed uniformly in a mass ratio of 82:8:1.5:0.5:1:1:2:4:96 to obtain a first slurry. Among them, the boiling point of the pore-forming composition composed of N,N-dimethylacetamide and deionized water is 105°C.
[0069] Artificial graphite (energy density is 340mAh / g, compaction density upper limit is 1.55g / cm 3 , fast charging capacity 6C), conductive carbon black, lithium carboxymethyl cellulose, styrene butadiene rubber, N,N-dimethylacetamide and deionized water are mixed uniformly in a mass ratio of 92:1:1:2:4:96 to obtain a second slurry. Among them, the boiling point of the pore-forming composition composed of N,N-dimethylacetamide and deionized water is 105°C.
[0070] Through the double-layer coating technology, the first slurry is introduced into the lower die head, and the second slurry is introduced into the upper die head, and coated on the copper current collector at the same time, then dried in an oven at 90°C, and then rolled, and finally vacuum dried in an oven at 120°C, and sliced to obtain electrode sheets.
[0071] The electrode sheet obtained in this embodiment includes a current collector and a first negative electrode active layer and a second negative electrode active layer stacked in sequence on the surface of the current collector, wherein the thickness of the first negative electrode active layer is 50 μm, the thickness of the second negative electrode active layer is 200 μm, and the compaction of the electrode sheet is 1.7 g / cm 3 .
[0072] Example 2
[0073] Artificial graphite (energy density is 365mAh / g, compaction density upper limit is 1.8g / cm 3, fast charging capacity 1.5C), nano silicon, conductive carbon black, single-walled carbon nanotubes, lithium carboxymethyl cellulose, styrene-butadiene rubber, lithium polyacrylate, N-methylformamide and deionized water are mixed uniformly in a mass ratio of 93:3:0.5:0.5:0.5:0.5:1:1:99 to obtain a first slurry. Among them, the boiling point of the pore-forming composition composed of N-methylformamide and deionized water is 102°C.
[0074] Artificial graphite (energy density is 355mAh / g, compaction density upper limit is 1.65g / cm 3 , fast charging capacity 4C), conductive carbon black, lithium carboxymethyl cellulose, styrene butadiene rubber, N-methylformamide and deionized water are mixed uniformly in a mass ratio of 98:0.1:0.5:0.5:1:99 to obtain a second slurry. Among them, the boiling point of the pore-forming composition composed of N-methylformamide and deionized water is 102°C.
[0075] Through the double-layer coating technology, the first slurry is introduced into the lower die head, and the second slurry is introduced into the upper die head, and coated on the copper current collector at the same time, then dried in an oven at 85°C, and then rolled, and finally vacuum dried in an oven at 115°C, and sliced to obtain electrode sheets.
[0076] The electrode sheet obtained in this embodiment includes a current collector and a first negative electrode active layer and a second negative electrode active layer stacked in sequence on the surface of the current collector, wherein the thickness of the first negative electrode active layer is 200 μm, the thickness of the second negative electrode active layer is 50 μm, and the compaction of the electrode sheet is 1.55 g / cm 3 .
[0077] Example 3
[0078] Artificial graphite (energy density is 360mAh / g, compaction density upper limit is 1.7g / cm 3 , fast charging capacity 1.8C), fumed silicon carbon, conductive carbon black, single-walled carbon nanotubes, lithium carboxymethyl cellulose, styrene-butadiene rubber, lithium polyacrylate, dimethyl sulfoxide and deionized water are mixed uniformly in a mass ratio of 86:5:1:0.5:0.8:0.5:1.2:3:97 to obtain a first slurry. Among them, the boiling point of the pore-forming composition composed of dimethyl sulfoxide and deionized water is 103°C.
[0079] Artificial graphite (energy density is 350mAh / g, compaction density upper limit is 1.6g / cm 3 , fast charging capacity 5C), conductive carbon black, lithium carboxymethyl cellulose, styrene-butadiene rubber, dimethyl sulfoxide and deionized water are mixed uniformly in a mass ratio of 95:0.5:1:0.5:3:97 to obtain a second slurry. Among them, the boiling point of the pore-forming composition composed of dimethyl sulfoxide and deionized water is 103°C.
[0080] Through the double-layer coating technology, the first slurry is introduced into the lower die head, and the second slurry is introduced into the upper die head, and coated on the copper current collector at the same time, then dried in an oven at 80°C, and then rolled, and finally vacuum dried in an oven at 110°C, and sliced to obtain electrode sheets.
[0081] The electrode sheet obtained in this embodiment includes a current collector and a first negative electrode active layer and a second negative electrode active layer stacked in sequence on the surface of the current collector, wherein the thickness of the first negative electrode active layer is 100 μm, the thickness of the second negative electrode active layer is 100 μm, and the compaction of the electrode sheet is 1.6 g / cm 3 .
[0082] Comparative Example 1
[0083] The only difference between Comparative Example 1 and Example 1 is that the N,N-dimethylacetamide in the second slurry is replaced by ammonium bicarbonate.
[0084] Comparative Example 2
[0085] The only difference between Comparative Example 2 and Example 1 is that the N,N-dimethylacetamide in the first slurry is replaced by ammonium bicarbonate.
[0086] Comparative Example 3
[0087] The only difference between Comparative Example 3 and Example 1 is that N,N-dimethylacetamide in the first slurry and the second slurry is replaced by ammonium bicarbonate at the same time.
[0088] Comparative Example 4
[0089] The only difference between Comparative Example 4 and Example 1 is that the N,N-dimethylacetamide in the first slurry and the second slurry is replaced by ammonium bicarbonate at the same time, and the drying temperature is set to 60°C and the vacuum drying temperature is set to 100°C.
[0090] Comparative Example 5
[0091] The only difference between Comparative Example 5 and Example 1 is that N,N-dimethylacetamide in the second slurry is replaced by n-butanol.
[0092] Comparative Example 6
[0093] The only difference between Comparative Example 6 and Example 1 is that N,N-dimethylacetamide in the second slurry is replaced by ethylene glycol diethyl ether.
[0094] Lithium ion button half-cells were assembled using the electrode sheets prepared in Examples 1-3 and Comparative Examples 1-6:
[0095] Place the electrode sheet moistened with electrolyte, the diaphragm, the lithium sheet, the gasket, and the spring sheet in the middle of the positive terminal of the stainless steel battery shell, align them strictly, then drip an appropriate amount of electrolyte, cover the negative battery shell and press it with tweezers, and use a sealing machine to seal it. The entire assembly process is carried out in a sealed glove box filled with high-purity argon (O2<0.1ppm, H2O<0.1ppm). The experiment uses metallic lithium as the counter electrode, 1mol / LLiPF6 EC / DEC (volume ratio of 1:1) mixed solution as the electrolyte, and Celgard-2400 polypropylene PP film as the diaphragm. The assembled button battery is placed for 12 hours to allow the electrode material to be fully infiltrated by the electrolyte before the battery performance test.
[0096] The relevant performance of the obtained lithium-ion button half-cell was tested, and the results are shown in Table 1.
[0097] The relevant test conditions are as follows:
[0098] First discharge capacity, first charge capacity and first coulombic efficiency: 25±2℃, 0.33C constant current and constant voltage discharge to 0.005V, record the first discharge capacity as D1; then, 0.33C constant current charge to 2.0V, record the first charge capacity as C1, and record the first coulombic efficiency as C1 / D1;
[0099] Normal temperature 0.33C cycle: 25±2℃, 0.33C constant current and constant voltage discharge to 0.005V, 0.33C constant current charge to 2.0V, cycle 50 times;
[0100] Rate discharge: 25±2℃, after the first cycle at 0.33C, discharge at 0.33C constant current and constant voltage to 0.005V, and record the discharge specific capacity as D1; then charge at 0.33C to 2.0V, discharge at 2C constant current and constant voltage to 0.005V, record the discharge specific capacity as D2, and the rate charging performance is characterized by D2 / D1.
[0101] Table 1
[0102]
[0103] It can be seen from Table 1 that the lithium ion battery using the electrode sheets prepared in Examples 1-3 has relatively higher gram capacity and first efficiency, better cycle performance and better rate discharge capability.
[0104] In Comparative Example 1, ammonium bicarbonate was decomposed before rolling. After rolling, the pores of the second negative electrode active layer were reduced and even closed, which affected the infiltration of the electrolyte and the Li + In Comparative Example 2, ammonium bicarbonate was also decomposed before rolling. After rolling, the porosity of the first negative electrode active layer was reduced, which affected the Li +ion transport, and at the same time, it cannot better accommodate the volume expansion of the silicon oxide material; in Comparative Example 3, ammonium bicarbonate has also been decomposed before rolling. After rolling, the porosity in the first negative electrode active layer and the second negative electrode active layer is reduced, which not only affects the infiltration of the electrolyte and Li + transmission, and cannot better accommodate the volume expansion of silicon-based materials; therefore, the performance of lithium-ion batteries prepared using the electrode sheets of Comparative Examples 1-3 is reduced.
[0105] In comparative example 4, after coating, the electrode was dried in an oven at 60°C, and after rolling, a semi-dried electrode was obtained. Subsequently, the semi-dried electrode was vacuum dried in an oven at 100°C to remove the ammonium bicarbonate. However, due to the low decomposition temperature of ammonium bicarbonate, the ammonium bicarbonate in the semi-dried electrode has been partially decomposed. At the same time, since the surface of the electrode has a larger contact area with the hot air during drying, the ammonium bicarbonate on the surface is easier to decompose. After rolling, the pores on the surface of the electrode are reduced, and even closed, which still affects the infiltration of the electrolyte and the Li + Therefore, the performance of the lithium-ion battery using the electrode sheet prepared in Comparative Example 4 also declined.
[0106] In Comparative Examples 5 and 6, an organic solvent with a lower boiling point (100°C-125°C) was used in the second slurry, which had partially evaporated before rolling. After rolling, the porosity of the second negative electrode active layer was reduced, which affected the electrolyte infiltration and Li + Ion transport, therefore, the performance of lithium-ion batteries prepared using the electrode sheets of Comparative Examples 5 and 6 is reduced.
[0107] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0108] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A method for preparing an electrode sheet, characterized in that: The following steps are involved: The active layer material is mixed with a pore-forming composition to obtain a slurry, wherein the pore-forming composition comprises water and an organic solvent miscible with water, and the boiling point of the organic solvent is higher than that of water by more than 25° C.; The slurry is coated on a current collector, and then subjected to a first drying, rolling and a second drying to obtain an electrode sheet, wherein the temperature of the first drying is lower than the boiling point of the pore-forming composition.
2. The method for preparing an electrode sheet according to claim 1, characterized in that: The preparation method also satisfies at least one of the following conditions: (1) The boiling point of the organic solvent is at least 30°C higher than that of water; (2) the boiling point of the pore-forming composition is greater than or equal to 100° C.; (3) the temperature of the first drying is at least 10° C. lower than the boiling point of the pore-forming composition; (4) The second drying is vacuum drying.
3. The method for preparing an electrode sheet according to claim 2, characterized in that: The preparation method also satisfies at least one of the following conditions: (1) The boiling point of the pore-forming composition is 100°C-130°C; (2) The boiling point of the organic solvent is 140°C-220°C; (3) the temperature of the first drying is 10°C to 40°C lower than the boiling point of the pore-forming composition; (4) The vacuum drying is carried out at a temperature of 90°C to 140°C and for a time of 20 min to 60 min.
4. The method for preparing an electrode sheet according to claim 3, characterized in that: The organic solvent is selected from at least one of N-methylpyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, N-methylformamide, 1,2-propylene glycol, and ethylene glycol.
5. The method for preparing an electrode sheet according to any one of claims 1 to 4, characterized in that: The following steps are involved: Mixing the first graphite, the silicon-based material, the conductive agent, the binder and the pore-forming composition to obtain a first slurry; Mixing a second graphite, a conductive agent, a binder and the pore-forming composition to obtain a second slurry; The first slurry is coated on the current collector to form a first slurry layer, and the second slurry is coated on the first slurry layer to form a second slurry layer, and then the electrode sheet is obtained through a first drying, rolling, a second drying and slicing.
6. The method for preparing an electrode sheet according to claim 5, characterized in that: The energy density of the first graphite active material is greater than the energy density of the second graphite active material, and the fast charging capability of the first graphite active material is less than the fast charging capability of the second graphite active material.
7. The method for preparing an electrode sheet according to claim 6, characterized in that: The preparation method also meets at least one of the following conditions: (1) The energy density of the first graphite is 355 mAh / g-365 mAh / g, and the upper limit of compaction density is 1.65 g / cm 3 -1.80g / cm 3 , fast charging capability is 1.5C-2C; (2) The energy density of the second graphite is 340 mAh / g-355 mAh / g, and the upper limit of compaction density is 1.55 g / cm 3 -1.65g / cm 3 , fast charging capability is 4C-6C; (3) The mass ratio of the silicon-based material, the first graphite, the conductive agent, the binder and the organic solvent in the first slurry is (3-8): (82-93): (1-2): (2-4): (1-4); (4) The mass ratio of the second graphite, the conductive agent, the binder and the organic solvent in the second slurry is (92-98):(0.1-1):(1-3):(0.9-4); (5) The silicon-based material is selected from at least one of pre-lithiation silicon oxygen, nano silicon or gas phase silicon carbon; (6) the conductive agent in the first slurry and the second slurry is independently selected from at least one of conductive carbon black, conductive graphite, graphene, and single-walled / multi-walled carbon nanotubes; (7) The binders in the first slurry and the second slurry are independently selected from at least one of styrene-butadiene rubber, sodium carboxymethyl cellulose, lithium carboxymethyl cellulose, lithium polyacrylate and sodium polyacrylate.
8. An electrode sheet obtained by the preparation method according to any one of claims 1 to 7, characterized in that: The electrode sheet includes a current collector and an active layer attached to at least one surface of the current collector.
9. The electrode sheet according to claim 8, characterized in that: The electrode sheet includes a current collector and a first negative electrode active layer and a second negative electrode active layer sequentially attached to at least one surface of the current collector, wherein the first negative electrode active layer includes a first graphite, a silicon-based material, a conductive agent and a binder, and the second negative electrode active layer includes a second graphite, a conductive agent and a binder.
10. An ion battery, characterized in that: The ion battery comprises the electrode sheet as claimed in claim 8 or 9.
11. A vehicle, characterized in that: The vehicle uses the ion battery as claimed in claim 10.