Zinc ion battery positive electrode material and preparation method and application thereof

CN118983431AActive Publication Date: 2024-11-19TAN KAH KEE INNOVATION LAB
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411035933.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-19
Estimated Expiration
2044-07-30

AI Technical Summary

Technical Problem

[0004]本发明的主要目的在于提供一种锌离子电池正极材料及其制备方法与应用,以解决锌离子电池正极材料的循环稳定性差的问题

Benefits of technology

[0026] Applying the technical solution of the present invention, by selecting the type of zinc-ion battery cathode material, on the one hand, the energy storage capacity of the cathode material can be improved, on the other hand, its cycle stability can be significantly improved, which is helpful to expand the application of zinc-ion batteries. scope.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118983431A_ABST
    Figure CN118983431A_ABST
Patent Text Reader

Abstract

The invention discloses a zinc ion battery positive electrode material as well as a preparation method and application thereof, and relates to the technical field of secondary batteries. The zinc ion battery positive electrode material disclosed by the invention has a perovskite structure, the chemical formula of the zinc ion battery positive electrode material is LaMnxMoyO3, x is more than or equal to 0.85 and less than or equal to 0.95, y is more than or equal to 0.05 and less than or equal to 0.15, and x + y is equal to 1. According to the invention, the structure of the positive electrode material of the zinc ion battery is selected, a material with a perovskite structure is used as the positive electrode material of the zinc ion battery, Mo is doped in the positive electrode material of the zinc ion battery, and the doping amount of Mo is controlled, so that the cycling stability of the positive electrode material of the zinc ion battery can be remarkably improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of secondary batteries, and in particular to a positive electrode material for a zinc ion battery and a preparation method and application thereof. Background Art

[0002] With the development of society, energy consumption has increased, energy crisis and environmental pollution problems have become increasingly severe, and the demand for clean and renewable energy has become increasingly urgent. Although renewable energy such as solar energy and wind energy is usually easy to obtain, energy storage and transportation are difficult to solve. Therefore, the development of stable and safe energy storage systems has received widespread attention. Batteries are one of the most commonly used energy storage systems and have become an indispensable part of people's daily lives. Among them, lithium-ion batteries have been widely used due to their advantages such as low specific weight, high energy density and long cycle life. However, lithium resources are limited, the cost is high, and most commercial lithium-ion batteries use organic electrolytes, which are prone to safety accidents. These have greatly limited the application of lithium-ion batteries. Aqueous zinc-ion batteries (AZIBs) are considered to be a promising electrochemical energy storage battery due to their low cost, high operating safety and large-scale power storage.

[0003] Cathode materials for aqueous zinc-ion batteries as storage materials for Zn 2+ The host material is the main contributor to battery performance; however, most of the current zinc-ion battery cathode materials cannot meet the requirements of long life, high energy density and power density. Therefore, the design and development of high-performance cathode materials is a hot topic in the field of aqueous zinc-ion batteries. At present, the commonly used cathode materials for AZIBs are manganese-based oxides, which have high energy storage capacity and working voltage, and are low in cost and environmentally friendly; however, manganese-based oxides have poor electronic conductivity and Zn 2+ The transfer kinetics are poor, and the manganese element is easily soluble, resulting in structural collapse, which causes serious capacity decay and poor cycle stability of the positive electrode material, seriously affecting its practical application potential. Therefore, it is urgent to provide a zinc ion battery positive electrode material with both good capacity and cycle stability. Summary of the invention

[0004] The main purpose of the present invention is to provide a zinc ion battery positive electrode material and a preparation method and application thereof, so as to solve the problem of poor cycle stability of the zinc ion battery positive electrode material.

[0005] In order to achieve the above object, according to a first aspect of the present invention, a positive electrode material for a zinc ion battery is provided, wherein the positive electrode material for a zinc ion battery has a perovskite structure and a chemical formula is LaMn x Mo y O3, wherein 0.85≤x≤0.95, 0.05≤y≤0.15, x+y=1.

[0006] Perovskite-structured materials have good electrochemical properties. LaMnO3 has a perovskite structure, excellent room temperature conductivity, small band gap, abundant A-site cation defects, and many oxygen anion vacancies, which are beneficial to improving the electrochemical performance of the material. By doping Mo in LaMnO3 with a perovskite structure and controlling its dosage, the stability of the positive electrode material of zinc-ion batteries can be effectively improved, thereby increasing its application potential.

[0007] Furthermore, the positive electrode material of the zinc ion battery has a popcorn-like structure.

[0008] Furthermore, the specific surface area of ​​the positive electrode material of the zinc ion battery is 5m 2 / g~10m 2 / g; and / or, the porosity of the zinc ion battery positive electrode material is 15% to 28%.

[0009] Controlling the specific surface area or porosity of the positive electrode material of the zinc ion battery within the above range is beneficial to improving the surface energy of the positive electrode material of the zinc ion battery and improving its electrochemical activity; at the same time, its stability is relatively high.

[0010] Furthermore, the positive electrode material of the zinc ion battery is formed by stacking primary particles, and the average particle size of the primary particles is 20nm to 35nm.

[0011] Controlling the average particle size of the primary particles of the zinc ion battery positive electrode material within the above range can shorten the ion diffusion path and improve the specific capacity of the zinc ion battery positive electrode material.

[0012] According to a second aspect of the present invention, there is provided a method for preparing the positive electrode material of a zinc ion battery according to the first aspect of the present invention, comprising the following steps:

[0013] S1, mixing La2O3 powder, MnO2 powder and MoO3 powder to obtain a first mixture;

[0014] S2, ball-milling the first mixture to obtain a second mixture;

[0015] S3, calcining the second mixture to obtain the zinc ion battery positive electrode material.

[0016] The invention adopts a solid phase calcination method to prepare the positive electrode material of the zinc ion battery. The preparation method is simple, has fewer steps, and can realize industrial large-scale production.

[0017] Furthermore, in S1, the La2O3 powder, the MnO2 powder and the MoO3 powder are mixed by grinding.

[0018] Grinding is a high-efficiency, low-cost mixing method. By selecting this method to mix the raw materials, the prepared zinc ion battery positive electrode material can have good uniformity.

[0019] Further, in S2, the ball milling method is:

[0020] The ball milling beads are mixed with the material at a ball-to-material ratio of (15-20):1, and then ethanol is added, and the ball milling is carried out at a rotation speed of 500rpm-700rpm for 2h-4h; the ball milling beads include large beads, medium beads, and small beads, the diameter of the large beads is 15mm-18mm, the diameter of the medium beads is 10mm-12mm, and the diameter of the small beads is 5mm-8mm, and the weight ratio of the large beads, the medium beads, and the small beads is (15-25):(25-35):(45-55).

[0021] Ball milling conditions have a great influence on the physicochemical properties of zinc ion battery positive electrode materials. By controlling the ball milling conditions, the specific surface area, porosity and average particle size of the prepared zinc ion battery positive electrode materials are more moderate, which is conducive to making the zinc ion battery positive electrode materials have both higher specific capacity and cycle stability, thereby improving their application range.

[0022] Furthermore, in S3, the calcination temperature is 700°C to 900°C, and the calcination time is 8h to 12h.

[0023] Calcination conditions have a great influence on the structure of zinc-ion battery positive electrode materials. By controlling the calcination conditions, the zinc-ion battery positive electrode materials have a higher degree of crystallinity and a stable perovskite structure, and the structure is not easy to collapse during the cycle process.

[0024] Furthermore, after calcination, the calcined product is ground and filtered with a sieve to obtain a positive electrode material for a zinc ion battery.

[0025] According to a third aspect of the present invention, there is provided an application of a zinc ion battery positive electrode material obtained by the preparation method of the zinc ion battery positive electrode material according to the first aspect of the present invention or the zinc ion battery positive electrode material according to the second aspect of the present invention in the field of zinc ion batteries, especially aqueous zinc ion batteries.

[0026] By applying the technical solution of the present invention, by selecting the type of positive electrode material for zinc ion batteries, on the one hand, the energy storage capacity of the positive electrode material can be increased, and on the other hand, its cycle stability can be significantly improved, which helps to expand the application range of zinc ion batteries. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 XRD patterns of the positive electrode materials of zinc ion batteries in Examples 1 to 3 and Comparative Examples 1 to 2;

[0028] Figure 2 The energy spectrum and scanning electron microscope image of the positive electrode material of the zinc ion battery in Example 1;

[0029] Figure 3 This is a transmission electron microscope image of primary particles of the positive electrode material of the zinc ion battery in Example 1;

[0030] Figure 4 The nitrogen adsorption and desorption curve of the positive electrode material of the zinc ion battery in Example 1;

[0031] Figure 5 This is the pore size distribution diagram of the positive electrode material of the zinc ion battery in Example 1;

[0032] Figure 6 The battery assembled from the zinc ion battery positive electrode materials in Examples 1 to 3 and Comparative Examples 1 to 2 is 1A·g -1 Electrochemical performance test diagram measured under the following conditions;

[0033] Figure 7 The battery assembled from the zinc ion battery positive electrode materials in Example 1 and Comparative Example 1 is at 0.5A·g -1 Electrochemical performance test diagram measured under the following conditions;

[0034] Figure 8 The battery assembled from the positive electrode material of the zinc ion battery in Example 1 is at 2A·g -1 Electrochemical performance test diagram measured under the following conditions;

[0035] Fig. 9 This is a test diagram of the rate performance of a battery assembled from the zinc ion battery positive electrode material in Example 1 at different current densities. DETAILED DESCRIPTION

[0036] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.

[0037] As described in the background of the present invention, the prior art has the problem that the cycle stability of the positive electrode material of the zinc ion battery is poor. In order to solve the above technical problems, in a typical embodiment of the present invention, a zinc ion battery positive electrode material is provided, which has a perovskite structure, and the chemical formula of the zinc ion battery positive electrode material is LaMn x Mo y O3, wherein 0.85≤x≤0.95, 0.05≤y≤0.15, x+y=1; specifically, LaMn 0.85 Mo0.15 O3、LaMn 0.9 Mo 0.1 O3、LaMn 0.95 Mo 0.05 O3, etc., and may also be other materials within this range.

[0038] LaMn perovskite structure x Mo y O3 has the characteristics of excellent conductivity, small band gap, rich A-site cation defects, and many oxygen anion vacancies, which are beneficial to improving the electrochemical performance. The present invention can inhibit the dissolution of manganese elements by doping Mo into LaMnO3. By controlling the doping amount of Mo, the positive electrode material of the zinc ion battery can have both high capacity and high cycle stability, thereby expanding the application range of the positive electrode material of the zinc ion battery.

[0039] In some embodiments, the zinc ion battery cathode material has a popcorn-like structure.

[0040] The popcorn-like structure helps to expand the specific capacity and specific energy density of the positive electrode material, store more energy, and provide a higher electron transfer rate.

[0041] In some embodiments, 0.88≤x≤0.92, 0.05≤y≤0.12.

[0042] By further optimizing x and y, the specific capacity and stability of the positive electrode material of the zinc ion battery can be further improved.

[0043] In some embodiments, the specific surface area of ​​the zinc ion battery positive electrode material is 5m 2 / g~10m 2 / g, specifically 5m 2 / g, 6m 2 / g, 7m 2 / g, 8m 2 / g, 9m 2 / g, 10m 2 / g, etc., and may also be other values ​​within the range, which are not limited here; and / or, the porosity of the zinc ion battery positive electrode material is 15% to 28%.

[0044] Controlling the specific surface area and porosity of the positive electrode material of zinc ion batteries can help further improve the specific capacity of the positive electrode material, increase its energy density, and help improve its cycle stability.

[0045] In some embodiments, the positive electrode material of the zinc ion battery is formed by stacking primary particles, and the average particle size of the primary particles is 20nm to 35nm, specifically 20nm, 24nm, 26nm, 29nm, 31nm, 33nm, 35nm, etc., or other values ​​within this range, which are not limited here.

[0046] Controlling the average particle size of the primary particles of the positive electrode material of zinc ion batteries can shorten the ion transmission distance, increase the electron transmission rate, and help improve the electrochemical activity of the positive electrode material of zinc ion batteries.

[0047] In a typical embodiment of the present invention, a method for preparing a positive electrode material for a zinc ion battery is provided, which comprises the following steps:

[0048] S1, mixing La2O3 powder, MnO2 powder and MoO3 powder to obtain a first mixture;

[0049] S2, ball milling the first mixture to obtain a second mixture;

[0050] S3, calcining the second mixture to obtain a positive electrode material for a zinc ion battery.

[0051] The invention prepares the zinc ion battery positive electrode material by a solid phase calcination method, has a simple preparation process, does not require special equipment and conditions, and is suitable for industrial production.

[0052] In some embodiments, in S1, La2O3 powder, MnO2 powder and MoO3 powder are mixed by grinding.

[0053] Grinding can increase the contact area between materials, promote the reaction, and improve the reaction rate and efficiency; it can also change the morphology and structure of the materials. In addition, grinding is used for mixing at a faster rate and at a lower cost, making it suitable for large-scale applications.

[0054] In some embodiments, in S2, the ball milling method is: mixing the ball milling beads with the material at a ball-to-material ratio of (15-20):1, then adding ethanol at a material-liquid ratio of 1g:(0.75-2)mL, and ball milling at a speed of 500rpm-700rpm for 2h-4h; the ball milling beads include large beads, medium beads, and small beads, the diameter of the large beads is 15mm-18mm, the diameter of the medium beads is 10mm-12mm, the diameter of the small beads is 5mm-8mm, and the weight ratio of the large beads, the medium beads, and the small beads is (15-25):(25-35):(45-55).

[0055] The purpose of controlling various parameters in the ball milling process is to prepare zinc ion battery positive electrode materials of the required size so that they have good electrochemical activity and cycle stability.

[0056] In some embodiments, the ball milling beads may be made of zirconium oxide, which has high hardness and wear resistance and can effectively grind various materials. In addition, zirconium oxide has good corrosion resistance and can be used stably for a long time in a humid environment. It also has good thermal stability, is pollution-free, and has a long service life.

[0057] In some embodiments, the ball milling process is performed in a planetary ball mill, a drum ball mill, or a vibrating ball mill.

[0058] In some embodiments, in S3, the calcination temperature is 700°C to 900°C, specifically 700°C, 750°C, 800°C, 850°C, 900°C, etc., or other values ​​within the range, which are not limited here; the calcination time is 8h to 12h, specifically 8h, 8.5h, 9h, 10h, 11h, 12h, etc., or other values ​​within the range, which are not limited here.

[0059] The calcination conditions are controlled in order to obtain a zinc ion battery positive electrode material with a complete structure so as to have good stability and improve its cycle performance.

[0060] In some embodiments, the heating rate during calcination is 2°C / min to 5°C / min, specifically 2°C / min, 3°C / min, 4°C / min, 5°C / min, etc., or other values ​​within the range, which are not limited here.

[0061] The purpose of controlling the heating rate is to heat the material evenly and obtain a zinc ion battery positive electrode material with uniform composition.

[0062] In some embodiments, after calcination, the calcined product is ground and filtered with a sieve to obtain a positive electrode material for a zinc ion battery, and filtering can remove large particles of uneven size. Specifically, a 100-mesh sieve can be used for filtering.

[0063] In another typical embodiment of the present invention, there is provided an application of the zinc ion battery positive electrode material in the above embodiment of the present invention or the zinc ion battery positive electrode material prepared by the above preparation method in the field of aqueous zinc ion batteries.

[0064] The present application is further described in detail below in conjunction with specific embodiments. These embodiments should not be construed as limiting the scope of protection claimed in the present application.

[0065]

Zinc-ion battery positive electrode materials

[0066] Example 1

[0067] An embodiment of the positive electrode material of a zinc ion battery of the present invention, the preparation method of the positive electrode material of a zinc ion battery of the present embodiment comprises the following steps:

[0068] S1, adding 1.629 g of La2O3 powder, 0.782 g of MnO2 powder and 0.144 g of MoO3 powder into a quartz mortar, grinding and mixing thoroughly to obtain a first mixture;

[0069] S2, adding the first mixture into a ball mill, adding 50 g of zirconium oxide ball milling beads (the weight ratio of large beads with a diameter of 15 mm, medium beads with a diameter of 10 mm, and small beads with a diameter of 8 mm is 20:30:50), then adding 5 mL of ethanol, placing the ball mill into a planetary ball mill, ball milling at a speed of 600 rpm for 3 h, and drying to obtain a second mixture;

[0070] S3, putting the second mixture into a crucible and compacting it, covering the crucible with a lid and placing the crucible into a muffle furnace for heating at a heating rate of 2°C / min, calcining at 900°C for 10 hours, and after the calcination is completed and naturally cooled, transferring the calcined product into a quartz mortar and grinding it thoroughly, and filtering the unevenly sized powder with a 100-mesh screen to obtain LaMn 0.9 Mo 0.1 O3 powder 2.126g, yield 83.21%.

[0071] Example 2

[0072] An embodiment of the positive electrode material of a zinc ion battery of the present invention, the preparation method of the positive electrode material of a zinc ion battery of the present embodiment comprises the following steps:

[0073] S1, adding 1.629 g of La2O3 powder, 0.826 g of MnO2 powder and 0.072 g of MoO3 powder into a quartz mortar, grinding and mixing thoroughly to obtain a first mixture;

[0074] S2, adding the first mixture into a ball mill, adding 50 g of zirconium oxide ball milling beads (the weight ratio of large beads with a diameter of 15 mm, medium beads with a diameter of 10 mm, and small beads with a diameter of 8 mm is 20:30:50), then adding 5 mL of ethanol, placing the ball mill into a planetary ball mill, ball milling at a speed of 600 rpm for 3 h, and drying to obtain a second mixture;

[0075] S3, putting the second mixture into a crucible and compacting it, covering the crucible with a lid and placing the crucible into a muffle furnace for heating at a heating rate of 2°C / min, calcining at 900°C for 10 hours, and after the calcination is completed and naturally cooled, transferring the calcined product into a quartz mortar and grinding it thoroughly, and filtering the unevenly sized powder with a 100-mesh screen to obtain LaMn 0.95 Mo 0.05O3 powder 2.095g, yield 82.90%.

[0076] Example 3

[0077] An embodiment of the positive electrode material of a zinc ion battery of the present invention, the preparation method of the positive electrode material of a zinc ion battery of the present embodiment comprises the following steps:

[0078] S1, adding 1.629 g of La2O3 powder, 0.739 g of MnO2 powder and 0.216 g of MoO3 powder into a quartz mortar, grinding and mixing thoroughly to obtain a first mixture;

[0079] S2, adding the first mixture into a ball mill, adding 50 g of zirconium oxide ball milling beads (the weight ratio of large beads with a diameter of 15 mm, medium beads with a diameter of 10 mm, and small beads with a diameter of 8 mm is 20:30:50), then adding 5 mL of ethanol, placing the ball mill into a planetary ball mill, ball milling at a speed of 600 rpm for 3 h, and drying to obtain a second mixture;

[0080] S3, putting the second mixture into a crucible and compacting it, covering the crucible with a lid and placing the crucible into a muffle furnace for heating at a heating rate of 2°C / min, calcining at 900°C for 10 hours, and after the calcination is completed and naturally cooled, transferring the calcined product into a quartz mortar and grinding it thoroughly, and filtering the unevenly sized powder with a 100-mesh screen to obtain LaMn 0.85 Mo 0.15 O3 powder 2.276g, yield 88.08%.

[0081] Example 4

[0082] An embodiment of the positive electrode material of a zinc ion battery of the present invention, the preparation method of the positive electrode material of a zinc ion battery of the present embodiment comprises the following steps:

[0083] S1, adding 1.629 g of La2O3 powder, 0.782 g of MnO2 powder and 0.144 g of MoO3 powder into a quartz mortar, grinding and mixing thoroughly to obtain a first mixture;

[0084] S2, adding the first mixture into a ball mill, adding 50 g of zirconium oxide ball milling beads (the weight ratio of large beads with a diameter of 15 mm, medium beads with a diameter of 10 mm, and small beads with a diameter of 8 mm is 30:50:20), then adding 5 mL of ethanol, placing the ball mill into a planetary ball mill, ball milling at a speed of 600 rpm for 3 h, and drying to obtain a second mixture;

[0085] S3, putting the second mixture into a crucible and compacting it, covering the crucible with a lid and placing the crucible into a muffle furnace for heating at a heating rate of 2°C / min, calcining at 900°C for 10 hours, and after the calcination is completed and naturally cooled, transferring the calcined product into a quartz mortar and grinding it thoroughly, and filtering the unevenly sized powder with a 100-mesh screen to obtain LaMn 0.9 Mo 0.1 O3 powder 2.331g, yield 91.23%.

[0086] Example 5

[0087] An embodiment of the positive electrode material of a zinc ion battery of the present invention, the preparation method of the positive electrode material of a zinc ion battery of the present embodiment comprises the following steps:

[0088] S1, adding 1.629 g of La2O3 powder, 0.782 g of MnO2 powder and 0.144 g of MoO3 powder into a quartz mortar, grinding and mixing thoroughly to obtain a first mixture;

[0089] S2, adding the first mixture into a ball mill, adding 50 g of zirconium oxide ball milling beads (the weight ratio of large beads with a diameter of 15 mm, medium beads with a diameter of 10 mm, and small beads with a diameter of 8 mm is 15:20:65), then adding 5 mL of ethanol, placing the ball mill into a planetary ball mill, ball milling at a speed of 600 rpm for 3 h, and drying to obtain a second mixture;

[0090] S3, putting the second mixture into a crucible and compacting it, covering the crucible with a lid and placing the crucible into a muffle furnace for heating at a heating rate of 2°C / min, calcining at 900°C for 10 hours, and after the calcination is completed and naturally cooled, transferring the calcined product into a quartz mortar and grinding it thoroughly, and filtering the unevenly sized powder with a 100-mesh screen to obtain LaMn 0.9 Mo 0.1 O3 powder 2.111g, yield 82.62%.

[0091] Comparative Example 1

[0092] A zinc ion battery positive electrode material, the preparation method of which comprises the following steps:

[0093] S1, adding 1.63 g of La2O3 powder and 0.87 g of MnO2 powder into a quartz mortar, grinding and mixing them thoroughly to obtain a first mixture;

[0094] S2, adding the first mixture into a ball mill, adding 50 g of zirconium oxide ball milling beads (the weight ratio of large beads with a diameter of 15 mm, medium beads with a diameter of 10 mm, and small beads with a diameter of 8 mm is 20:20:60), then adding 5 mL of ethanol, placing the ball mill into a planetary ball mill, ball milling at a speed of 600 rpm for 3 h, and drying to obtain a second mixture;

[0095] S3, put the second mixture into a crucible and compact it. After covering the crucible with a lid, put the crucible into a muffle furnace and heat it at a heating rate of 2°C / min. Calcinate at 900°C for 10 hours. After the calcination is completed and naturally cooled, transfer the calcined product to a quartz mortar and grind it thoroughly. Use a 100-mesh sieve to filter out powders of uneven size to obtain 2.25 g of LaMnO3 powder with a yield of 90%.

[0096] Comparative Example 2

[0097] A zinc ion battery positive electrode material, the preparation method of which comprises the following steps:

[0098] An embodiment of the positive electrode material of a zinc ion battery of the present invention, the preparation method of the positive electrode material of a zinc ion battery of the present embodiment comprises the following steps:

[0099] S1, adding 1.629 g of La2O3 powder, 0.696 g of MnO2 powder and 0.288 g of MoO3 powder into a quartz mortar, grinding and mixing thoroughly to obtain a first mixture;

[0100] S2, adding the first mixture into a ball mill, adding 50 g of zirconium oxide ball milling beads (the weight ratio of large beads with a diameter of 15 mm, medium beads with a diameter of 10 mm, and small beads with a diameter of 8 mm is 20:20:60), then adding 5 mL of ethanol, placing the ball mill into a planetary ball mill, ball milling at a speed of 600 rpm for 3 h, and drying to obtain a second mixture;

[0101] S3, putting the second mixture into a crucible and compacting it, covering the crucible with a lid and placing the crucible into a muffle furnace for heating at a heating rate of 2°C / min, calcining at 900°C for 10 hours, and after the calcination is completed and naturally cooled, transferring the calcined product into a quartz mortar and grinding it thoroughly, and filtering the unevenly sized powder with a 100-mesh screen to obtain LaMn 0.8 Mo 0.2 O3 powder 2.307g, yield 88.29%.

[0102]

Zinc ion battery

[0103] The zinc ion battery positive electrode materials in Examples 1 to 5 and Comparative Examples 1 to 2 are assembled into button batteries, and the preparation method thereof is as follows:

[0104] The positive electrode material, carbon black and PVDF of the zinc ion battery are added to the N-methylpyrrolidone solution in a mass ratio of 7:2:1, stirred for 24 hours to make a slurry, which is coated on a 0.01 mm titanium foil current collector, vacuum dried for 12 hours and cut into discs with a diameter of 12 mm, the 0.1 mm thick zinc foil is cut into discs with a diameter of 17 mm, and the glass fiber diaphragm is cut into discs with a diameter of 19 mm. A 304 stainless steel CR2025 battery shell is used to assemble the battery in the following order: positive electrode shell-positive electrode-100 μL electrolyte-diaphragm-100 μL electrolyte-negative electrode-gasket-wavy spring-negative electrode shell, and finally packaged with a tablet press to obtain an aqueous zinc ion battery; wherein the electrolyte is an aqueous solution with a ZnSO4 concentration of 2 mol / L and a MnSO4 concentration of 0.2 mol / L.

[0105]

Performance test

[0106] 1. Zinc ion battery positive electrode material

[0107] 1) Structure: tested by X-ray diffractometer;

[0108] 2) Morphology: observed by scanning electron microscopy and transmission electron microscopy;

[0109] 3) Specific surface area, porosity, and average particle size: tested using a specific surface area and porosity analyzer.

[0110] 2. Zinc ion battery

[0111] 1) Discharge capacity and cycle performance: at 0.5A·g -1 Cycle 200 times under 1A·g -1 Cycle 500 times under the conditions of 2A·g -1 Cycle 1000 times under the same conditions and test with battery tester system;

[0112] 2) Rate performance: at 0.3A·g -1 , 0.5A·g -1 , 1A·g -1 , 3A g -1 , 5A g -1 , 10A·g -1 The battery tester system was used for testing under the following conditions.

[0113] The performance test results of the zinc ion battery positive electrode material and the zinc ion battery are recorded in Table 1.

[0114] Table 1

[0115]

[0116] It can be seen from Table 1 that the battery made from the positive electrode material of the zinc ion battery in the embodiment has a high discharge specific capacity and good cycle stability. In addition, it can be seen from the test results of Examples 1 to 5 that the specific surface area of ​​the positive electrode material of the zinc ion battery is 5m 2 / g~10m 2 / g, and / or, the porosity of the zinc ion battery positive electrode material is 15% to 28%, and / or, the average particle size of the primary particles of the zinc ion battery positive electrode material is 20nm to 35nm, the electrochemical performance of the zinc ion battery positive electrode material is better, and it has excellent discharge specific capacity and cycle stability.

[0117] Figure 1 3 and 4. The XRD patterns of the positive electrode materials of zinc ion batteries in Examples 1 to 3 and Comparative Examples 1 to 2 show that the positive electrode materials of zinc ion batteries in the examples all have a good perovskite structure; among them, when 0.9≤x≤0.95, the structure of the positive electrode material of zinc ion batteries prepared is almost exactly the same as LaMnO3, but when x≤0.85, an obvious peak of La2MnMoO6 appears in the XRD pattern.

[0118] Figure 2 The energy spectrum diagram and scanning electron microscope diagram of the positive electrode material of the zinc ion battery in Example 1 show that the positive electrode material of the zinc ion battery has a popcorn-like structure, and its energy spectrum diagram shows that each element is evenly distributed in the positive electrode material.

[0119] Figure 3 This is a transmission electron microscope image of the primary particles of the zinc ion battery positive electrode material in Example 1. It can be seen from the figure that the particles of the zinc ion battery positive electrode material prepared by the present invention are fine and uniform, which is beneficial to improving the stability of the positive electrode material.

[0120] Figure 4 This is a nitrogen adsorption-desorption curve of the zinc ion battery positive electrode material in Example 1. It can be seen from the figure that the prepared zinc ion battery positive electrode material has a large specific surface area and a large active area, which is beneficial to improving the electrochemical performance of the positive electrode material.

[0121] Figure 5 This is the pore size distribution diagram of the zinc ion battery positive electrode material in Example 1. It can be seen from the figure that the prepared zinc ion battery positive electrode material has a small particle size and many active sites, which is beneficial to improving the electrochemical performance of the positive electrode material.

[0122] Figure 6 The battery assembled from the zinc ion battery positive electrode materials in Examples 1 to 3 and Comparative Examples 1 to 2 is 1A·g -1 The electrochemical performance test diagram under the conditions of FIG. 2 shows that after 500 cycles, the discharge specific capacity of Examples 1 to 3 changes very little. This result shows that the zinc ion battery prepared with the zinc ion battery positive electrode material disclosed in the present invention has both good discharge specific capacity and cycle stability.

[0123] Figure 7 The battery assembled from the zinc ion battery positive electrode materials in Example 1 and Comparative Example 1 is at 0.5A·g -1 The electrochemical performance test diagram measured under the conditions of 1.5 ℃ and 2.5 ℃ is shown in the figure. It can be seen from the figure that with the increase of the number of cycles, the positive electrode material of the zinc ion battery is gradually activated. After 200 cycles, the discharge capacity of the battery assembled from the positive electrode material of the zinc ion battery in Example 1 reaches 445 mAh·g -1 , which is better than Comparative Example 1. The result shows that the zinc ion battery prepared with the zinc ion battery positive electrode material disclosed in the present invention has excellent discharge specific capacity.

[0124] Figure 8 The battery assembled from the positive electrode material of the zinc ion battery in Example 1 is at 2A·g -1 The electrochemical performance test diagram measured under the conditions is shown in the figure. It can be seen from the figure that the zinc ion battery made with the zinc ion battery positive electrode material disclosed in the present invention also has good electrochemical performance under high rate conditions.

[0125] Fig. 9 This is a rate performance test diagram of a battery assembled from the zinc ion battery positive electrode material in Example 1 at different current densities. It can be seen from the figure that with the increase of current density, the discharge specific capacity of the zinc ion battery decreases approximately linearly. When the current density decreases, the discharge specific capacity of the zinc ion battery can be restored to the initial value, and has good stability.

[0126] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A positive electrode material for a zinc ion battery, characterized in that: The positive electrode material of the zinc ion battery has a perovskite structure, and the chemical formula of the positive electrode material of the zinc ion battery is LaMn x Mo y O3, wherein 0.85≤x≤0.95, 0.05≤y≤0.15, x+y=1.

2. The zinc ion battery cathode material according to claim 1, wherein The zinc ion battery positive electrode material has a popcorn-like structure.

3. The zinc ion battery cathode material according to claim 1, wherein The specific surface area of ​​the positive electrode material of the zinc ion battery is 5m 2 / g~10m 2 / g; and / or, the porosity of the zinc ion battery positive electrode material is 15% to 28%.

4. The zinc ion battery cathode material according to claim 1, wherein The zinc ion battery positive electrode material is formed by stacking primary particles, and the average particle size of the primary particles is 20nm to 35nm.

5. A method for preparing a positive electrode material for a zinc ion battery according to any one of claims 1 to 4, characterized in that: The steps include: S1, mixing La2O3 powder, MnO2 powder and MoO3 powder to obtain a first mixture; S2, ball-milling the first mixture to obtain a second mixture; S3, calcining the second mixture to obtain the zinc ion battery positive electrode material.

6. The method for preparing a positive electrode material for zinc ion batteries according to claim 5, wherein In S1, the La2O3 powder, the MnO2 powder and the MoO3 powder are mixed by grinding.

7. The method for preparing a positive electrode material for zinc ion batteries according to claim 5, wherein The ball milling method is: The ball milling beads are mixed with the material at a ball-to-material ratio of (15-20):1, and then ethanol is added, and the ball milling is carried out at a rotation speed of 500rpm-700rpm for 2h-4h; the ball milling beads include large beads, medium beads, and small beads, the diameter of the large beads is 15mm-18mm, the diameter of the medium beads is 10mm-12mm, and the diameter of the small beads is 5mm-8mm, and the weight ratio of the large beads, the medium beads, and the small beads is (15-25):(25-35):(45-55).

8. The method for preparing a positive electrode material for zinc ion batteries according to claim 5, wherein The calcination temperature is 700° C. to 900° C. and the calcination time is 8 h to 12 h.

9. The method for preparing a positive electrode material for zinc ion batteries according to claim 5, wherein After the calcination, the calcined product is ground and filtered with a sieve to obtain the zinc ion battery positive electrode material.

10. Use of the zinc ion battery positive electrode material according to any one of claims 1 to 4 or the zinc ion battery positive electrode material prepared by the preparation method according to any one of claims 5 to 9 in the field of zinc ion batteries.

Citation Information

Patent Citations

  • Lanthanum-doped high-rate zinc-manganese battery anode material and preparation method thereof

    CN110600728A

  • Sodium ion positive electrode material and preparation and application thereof

    CN116706041A

  • SOFC (Solid Oxide Fuel Cell) double-perovskite type electrode material as well as preparation method and application thereof

    CN117254047A

  • Zinc ion battery positive electrode material, preparation method therefor, and application thereof