Layered oxide positive electrode single crystal material for sodium ion battery and preparation method of layered oxide positive electrode single crystal material
By using low-copper doped nickel-ferromanganese-based O3 layered positive electrode material in sodium ion batteries, combined with M element co-melting and appropriate sintering conditions, a stable single crystal structure was formed, which solved the problem of NiO heterophase regulation. Significantly improves battery capacity and cycling performance.
Patent Information
- Application Number
- CN202411062414.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-11-19
AI Technical Summary
In sodium ion batteries, it is difficult to achieve a balanced improvement in various performances of the doped elements of nickel-ferromanganese-based layered positive electrode materials, especially the regulation of NiO heterophase has a significant impact on the structural stability and electrochemical properties of the material, resulting in cycling performance decline.
Using low-copper-doped nickel-ferromanganese-based O3 layered positive electrode material as the matrix, the particle size and specific surface area of the material are optimized, the crystallization phase generation and exposure of NiO are controlled, and the appropriate combination of Sintering temperature and time form a stable single crystal structure.
It significantly improves the capacity and cycling performance of the positive electrode material of sodium ion battery, reduces the negative impact of NiO, and improves the electrochemical stability and environmental stability of the battery.
Smart Images

Figure BDA0004978350100000111 
Figure HDA0004978350110000011 
Figure HDA0004978350110000012
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of sodium electric materials, in particular to a sodium ion battery layered oxide positive electrode single crystal material and a preparation method thereof. Background Art
[0002] As a new type of energy storage technology, sodium-ion batteries have attracted widespread attention in recent years due to their advantages such as abundant resources, affordable costs, and environmental friendliness. Researchers have been striving to explore new ways to improve the performance of sodium-ion batteries. In sodium-ion batteries, the positive electrode material is one of the key factors affecting battery performance. Among them, O3-phase layered oxide positive electrode materials have become the research focus of sodium-ion battery positive electrode materials due to their high capacity and good electrochemical properties.
[0003] Single-crystal nickel-iron-manganese-based cathode materials have high structural stability and electrochemical performance. Compared with polycrystalline nickel-iron-manganese-based cathode materials, single-crystal materials usually show better cycle stability and lower interface side reactions due to fewer grain boundaries.
[0004] In nickel-iron-manganese-based laminated cathode materials, certain doping elements are often added to improve their structural stability, electrochemical performance, and synthesis conditions. However, due to factors such as the type and amount of doping elements, it is often difficult to achieve a balanced improvement in multiple aspects of performance. For example, the introduction of doping elements may promote the improvement of ion transmission capacity due to lattice distortion, but it is easy to reduce structural stability and reduce cycle capacity. Copper, as one of the commonly used doping elements, is particularly prominent in improving the electrochemical performance of nickel-iron-manganese-based laminated cathode materials.
[0005] In nickel-iron-manganese-copper-based laminated cathode materials, copper doping will also affect the crystal structure and change the impurity phase. The introduction of copper into the matrix is conducive to the formation of single crystals. Low copper doping may help maintain the stability of the layered structure and provide more suitable ion diffusion channels; however, the low copper content system is prone to increase the content of impurities such as NiO, and the introduction of more impurity phases affects the formation of matrix single crystals. In particular, as a major part of transition metal oxides, the NiO impurity phase has a significant impact on the overall performance of the material. The impact of NiO is multifaceted. It can change the physical structure of the material, cause lattice changes, and indirectly increase the ion diffusion rate, thereby improving the rate performance; but at the same time, as an inactive substance, NiO may occupy active sites and affect the electrochemical activity of battery materials. In addition, the layered oxides in which NiO participates may be difficult to maintain stability under high voltage charging, and the cycle performance is reduced. It is easy to react with moisture and CO2 in the air, affecting the environmental stability and initial capacity of the battery. How to regulate the NiO impurity phase is a challenge faced by nickel-iron-manganese-copper-based laminated cathode materials in terms of material design and synthesis optimization. Summary of the invention
[0006] In view of the above problems in the prior art, the present invention provides a sodium ion battery layered oxide positive electrode single crystal material and a preparation method thereof, and obtains a positive electrode single crystal material with good capacity and cycle performance through the material design of a nickel-iron-manganese-copper-based layered positive electrode material.
[0007] In the first aspect, the sodium ion battery layered oxide positive electrode single crystal material proposed in the present invention has the following general formula: Na x Ni a Cu b Fe c Mn d M y O2, wherein 0.95≤x≤1.05, 0.29≤a≤0.31, 0.02≤b≤0.04, 0.31≤c≤0.35, 0.32≤d≤0.36, 0.001≤y≤0.02, and M is one or more elements selected from Sr, Ca, Ti, Zr, Y, and Bi;
[0008] The particle size D50 of the positive electrode single crystal material satisfies 4μm≤D50≤20μm, and the specific surface area S satisfies S≤0.5m 2 / g;
[0009] In the XRD of the positive electrode single crystal material, the ratio of NiO crystal phase to O3 phase is δ,
[0010] δ=(A(111)+A(200)) / (A(003)+A(104))≤2%, wherein A(111) and A(200) are the peak areas of NiO (111) and (200) peaks in XRD, and A(003) and A(104) are the peak areas of O3 phase positive electrode (003) and (104) peaks in XRD.
[0011] In the above material design scheme of the present invention, a low-copper-doped nickel-iron-manganese-based O3 layered positive electrode is used as the matrix, and a more stable layered structure is formed during the material synthesis process. The addition of M element and the co-fluxing of Cu promote the good formation of a single crystal structure. The particle size range of the material is optimized so that the material forms a good level of particle contact and adhesion during the co-fluxing of the M element, and the specific surface area is effectively controlled during the single crystal formation process. At the same time, the NiO produced by the low-copper system can adjust the sintering temperature and surface structure under the fluxing effect, control the amount of NiO crystalline phase generated, and improve the exposure of the NiO crystalline phase on the material surface through surface regulation. The above materials of the present invention have significant advantages in optimizing and improving the electrical performance of batteries.
[0012] In some embodiments, in the general formula of the sodium-ion battery layered oxide positive electrode single crystal material, 0.03≤b≤0.04, a relatively higher range of copper content within the control range is beneficial to further improve the capacity and cycle performance, which may be related to the further improvement of the single crystal morphology.
[0013] In some embodiments, in the XRD of the positive electrode single crystal material, 0.04%≤δ≤0.3%; δ within this range has good cycle performance and battery capacity, which may be because the lower exposure area of the NiO crystalline phase will reduce the destructive effect on the formation of the single crystal structure, avoiding the inhomogeneity and instability of material performance; it will also reduce side reactions with the electrolyte, thereby improving the capacity and cycle performance of the material.
[0014] In some embodiments, in the sodium-ion battery layered oxide positive electrode single crystal material, the source of sodium is one or more of sodium metal, sodium salt, sodium oxide or sodium hydroxide; as some specific examples: sodium salts include sodium chloride, sodium sulfate, sodium carbonate, sodium bicarbonate, etc., sodium oxides include sodium oxide and sodium peroxide, and sodium hydroxide includes sodium hydroxide.
[0015] In some embodiments, in the sodium ion battery layered oxide positive electrode single crystal material, the additive source of the M element includes corresponding metal oxides, metal salts, hydroxides and other compounds; metal salts include carbonates, sulfates, nitrates, etc.; metal oxides include strontium oxide, calcium oxide, titanium dioxide, zirconium dioxide, yttrium oxide or bismuth trioxide, etc.; hydroxides include strontium hydroxide, calcium hydroxide, titanium hydroxide, zirconium hydroxide, yttrium hydroxide or bismuth hydroxide, etc.
[0016] In some embodiments, in the sodium ion battery layered oxide positive electrode single crystal material, the additive particle size d50 of the M element satisfies 0.03μm≤d50≤2μm.
[0017] Small particle size additives within a suitable range are beneficial to increase the contact area with the precursor material, cause lattice distortion, expand lattice channels, accelerate the rapid transmission of substances in the lattice, and reduce the sintering temperature.
[0018] In order to obtain positive electrode single crystal materials that meet the above-mentioned material design requirements, on the one hand, it is necessary to select precursor materials with suitable specifications, and on the other hand, it is necessary to optimize the sintering system of the materials.
[0019] In some embodiments, the precursor of the sodium ion battery layered oxide positive electrode single crystal material meets the following specifications: Ni a Cu b Fe c Mn d(OH)2, where 0.29≤a≤0.31, 0.02≤b≤0.04, 0.31≤c≤0.35, 0.32≤d≤0.36, the precursor particle size D150 satisfies 4μm≤D150≤11μm, and the specific surface area BET satisfies 10m 2 / g<BET<30m 2 / g.
[0020] The present invention further preferably uses a nickel-iron-manganese-based O3 layered positive electrode doped with low copper content as the matrix, and selects a precursor material with a suitable particle size so that the specific surface area meets 10m 2 / g<BET<30m 2 / g, matching additives with suitable particle sizes to achieve low sintering temperature. Within this range, a stable single crystal structure can be formed with optimal electrochemical stability and cycle performance.
[0021] In some embodiments, the precursor of the sodium ion battery layered oxide positive electrode single crystal material contains an impurity element Y in its raw material, where Y is one or more of Ca, Ti, Zr, Y, Bi, Co, Li, K, Al, Mg, Zn, Sb, Sc, Nb, V, Ga, Sr, Ba, Nd, and Ce, and the content of the impurity element Y is ≤5000ppm;
[0022] In some embodiments, the ratio β of the particle size d50 of the M element additive to the particle size D150 of the precursor (β=d50 / D150) satisfies 0.02≤β≤0.5;
[0023] In a second aspect, the present invention provides a method for preparing a sodium ion battery layered oxide positive electrode single crystal material, the preparation method comprising sintering the sodium ion battery layered oxide positive electrode precursor material, a sodium source, and an M element additive of the present invention; the sintering temperature is 900 to 1000°C, the sintering time is 10 to 20 hours, and the heating rate is controlled to be 1 to 10°C / min.
[0024] The sintering temperature, sintering time and heating rate within this parameter range can work together to make the prepared sodium ion battery layered oxide positive electrode single crystal material have the best electrochemical performance.
[0025] In a third aspect, the present invention further provides a positive electrode plate, which comprises the sodium ion battery layered oxide positive electrode single crystal material obtained by the preparation method of the second aspect of the present invention, a conductive agent and a binder.
[0026] The design of the positive electrode plate is unique and innovative. The positive electrode single crystal material has excellent electrochemical properties and has excellent capacity and cycle stability, which makes the positive electrode plate have broad application prospects in the field of sodium ion batteries, thereby greatly improving the overall performance of the battery and meeting the growing energy demand.
[0027] In a fourth aspect, the present invention provides a sodium ion battery, which includes the positive electrode sheet, negative electrode sheet, electrolyte and separator described in the third aspect. The sodium ion battery with layered oxide positive electrode single crystal material provided by the present invention can be used in multiple fields such as solar power generation, wind power generation, aerospace, distributed power stations, backup power supplies, military equipment or energy storage equipment for communication base stations; it has brought breakthrough progress to the battery industry, making sodium ion batteries a more competitive energy storage solution.
[0028] Compared with the prior art, the present invention has at least the following beneficial effects:
[0029] The present invention adopts a low-copper-doped nickel-iron-manganese-based O3 layered positive electrode as the matrix, selects M element additives and precursor materials of suitable particle size, and improves the fluxing effect of the material in a low-copper system; reduces the sintering temperature within the particle size range optimized by the material, performs reasonable sintering preparation, regulates the amount of NiO crystal phase generated, and further promotes the good formation of a single crystal structure. The above-mentioned materials of the present invention have significant advantages in optimizing and improving the electrical performance of batteries. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0031] Figure 1 The XRD diagram of Example 1 of the present invention is
[0032] Figure 2 This is the SEM image of Example 1 of the present invention.
[0033] Figure 3 This is the SEM image of Comparative Example 5 of the present invention DETAILED DESCRIPTION
[0034] The technical solution of the present application will be described clearly and completely below in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present application, rather than all embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present application.
[0035] In the first aspect, the sodium ion battery layered oxide positive electrode single crystal material proposed in the present invention has the following general formula: Na x Ni a Cu b Fe c Mn d M y O2, wherein 0.95≤x≤1.05, 0.29≤a≤0.31, 0.02≤b≤0.04, 0.31≤c≤0.35, 0.32≤d≤0.36, 0.001≤y≤0.02, and M is one or more elements selected from Sr, Ca, Ti, Zr, Y, and Bi;
[0036] The particle size D50 of the positive electrode single crystal material satisfies 4μm≤D50≤20μm, and the specific surface area S satisfies S≤0.5m 2 / g;
[0037] In the XRD of the positive electrode single crystal material, the ratio of NiO crystal phase to O3 phase is δ,
[0038] δ=(A(111)+A(200)) / (A(003)+A(104))≤2%, wherein A(111) and A(200) are the peak areas of NiO (111) and (200) peaks in XRD, and A(003) and A(104) are the peak areas of O3 phase positive electrode (003) and (104) peaks in XRD.
[0039] A low-copper-doped nickel-iron-manganese-based O3 layered positive electrode is used as the matrix, and a more stable layered structure is formed during the material synthesis process. The addition of M element and the co-fluxing of Cu promote the good formation of a single crystal structure. The particle size range of the material is optimized so that the material forms a good level of particle contact and adhesion during the M element and low-copper fluxing process, and the specific surface area is effectively controlled during the single crystal formation process. At the same time, the NiO produced by the low-copper system can adjust the sintering temperature and surface structure under the fluxing effect, control the amount of NiO crystalline phase generated, and improve the exposure of the NiO crystalline phase on the material surface through surface regulation. The above-mentioned materials of the present invention have significant advantages in optimizing and improving the electrical performance of batteries.
[0040] In the above-mentioned material design scheme of the present invention, a low-copper-doped nickel-iron-manganese-based O3 layered positive electrode is used as the matrix, and a more stable layered structure is formed during the material synthesis process. The addition of M elements and the co-fluxing of Cu further promotes the good formation of a single crystal structure. The particle size range of the material is optimized so that the material forms a good particle contact and adhesion level during the co-fluxing of the M element, and the specific surface area is effectively controlled during the single crystal formation process. At the same time, the NiO produced by the low-copper system is able to adjust the sintering temperature and surface structure under a better fluxing effect, control the amount of NiO crystalline phase generated, and improve the exposure of the NiO crystalline phase on the surface of the material through surface regulation, that is, the content of the NiO crystalline phase and its effect of aggregation on the surface are optimized through the joint regulation of the above-mentioned δ and specific surface area S, reducing the negative effects of NiO, while maximizing the advantages of amorphous NiO and the internal crystalline phase of the particles on the positive electrode material. The above-mentioned materials of the present invention have significant advantages in optimizing and improving the electrical performance of batteries.
[0041] In some embodiments, in the general formula of the sodium-ion battery layered oxide positive electrode single crystal material, 0.03≤b≤0.04, a relatively higher range of copper content within the control range is beneficial to further improve the capacity and cycle performance, which may be related to the further improvement of the single crystal morphology.
[0042] In some embodiments, in the XRD of the positive electrode single crystal material, 0.04%≤δ≤0.3%; the cycle performance and battery capacity of δ within this range are good, which may be because the lower exposure area of the NiO crystalline phase will reduce the destructive effect on the formation of the single crystal structure, avoiding the inhomogeneity and instability of material performance; it will also reduce the side reaction with the electrolyte, thereby improving the capacity, rate and cycle performance of the material.
[0043] In some embodiments, in the sodium-ion battery layered oxide positive electrode single crystal material, the source of sodium is one or more of sodium metal, sodium salt, sodium oxide or sodium hydroxide; as some specific examples: sodium salts include sodium chloride, sodium sulfate, sodium carbonate, sodium bicarbonate, etc., sodium oxides include sodium oxide and sodium peroxide, and sodium hydroxide includes sodium hydroxide.
[0044] In some embodiments, in the sodium ion battery layered oxide positive electrode single crystal material, the additive source of the M element includes corresponding metal oxides, metal salts, hydroxides and other compounds; metal salts include carbonates, sulfates, nitrates, etc.; metal oxides include strontium oxide, calcium oxide, titanium dioxide, zirconium dioxide, yttrium oxide or bismuth trioxide, etc.; hydroxides include strontium hydroxide, calcium hydroxide, titanium hydroxide, zirconium hydroxide, yttrium hydroxide or bismuth hydroxide, etc.
[0045] In some embodiments, in the sodium ion battery layered oxide positive electrode single crystal material, the additive particle size d50 of the M element satisfies 0.03μm≤d50≤2μm.
[0046] Small particle size additives within a suitable range are beneficial to increase the contact area with the precursor material, cause lattice distortion, expand lattice channels, accelerate the rapid transmission of substances in the lattice, and reduce the sintering temperature; when the small particle size additives are different from the precursor particle size, it is beneficial to reduce the activation energy of the lattice, so that atoms can obtain sufficient energy to migrate and rearrange at a lower temperature to achieve sintering.
[0047] In order to obtain positive electrode single crystal materials that meet the above-mentioned material design requirements, on the one hand, it is necessary to select precursor materials with suitable specifications, and on the other hand, it is necessary to optimize the sintering system of the materials.
[0048] In some embodiments, the precursor of the sodium ion battery layered oxide positive electrode single crystal material meets the following specifications: Ni a Cu b Fe c Mn d (OH)2, where 0.29≤a≤0.31, 0.02≤b≤0.04, 0.31≤c≤0.35, 0.32≤d≤0.36, the precursor particle size D150 satisfies 4μm≤D150≤11μm, and the specific surface area BET satisfies 10m 2 / g<BET<30m 2 / g.
[0049] Different metal ion ratios will affect the electrochemical properties of the layered oxide positive electrode single crystal material for sodium ion batteries and the formation of the single crystal structure. The present invention further prefers a nickel-iron-manganese-based O3 layered positive electrode doped with a low copper content as the matrix, and selects a precursor material with a suitable particle size so that the specific surface area meets 10m 2 / g<BET<30m 2 / g, matching additives with appropriate particle sizes, and achieving low sintering temperatures, a stable single crystal structure can be formed within this range. This may be because a smaller specific surface area will reduce the contact between the material and the surrounding environment to produce side reactions, thereby reducing the material's cycle performance. And a smaller specific surface area usually means fewer grain boundaries, which can form a stable single crystal structure; at the same time, low sintering temperatures will reduce the amount of NiO generated, reduce the exposure range of the NiO crystalline phase on the O3 phase surface, and improve the electrochemical performance of single crystal structure materials.
[0050] In some embodiments, the precursor of the sodium ion battery layered oxide positive electrode single crystal material contains an impurity element Y in its raw material, where Y is one or more of Ca, Ti, Zr, Y, Bi, Co, Li, K, Al, Mg, Zn, Sb, Sc, Nb, V, Ga, Sr, Ba, Nd, and Ce, and the content of the impurity element Y is ≤5000ppm;
[0051] In some embodiments, the ratio β of the particle size d50 of the M element additive to the particle size D150 of the precursor (β=d50 / D150) satisfies 0.02≤β≤0.5; within this range, good single crystal materials can be obtained more quickly through synergistic Cu co-fluxing.
[0052] In a second aspect, the present invention provides a method for sintering a sodium ion battery layered oxide positive electrode single crystal material, the preparation method comprising sintering the sodium ion battery layered oxide positive electrode precursor material, a sodium source, and an M element additive of the present invention; the sintering temperature is 900 to 1000°C, the sintering time is 10 to 20 hours, and the heating rate is controlled to be 1 to 10°C / min.
[0053] The present invention adopts a nickel-iron-manganese-based material doped with a low copper system combined with a precursor material of suitable particle size and an additive, which has a better fluxing effect and reduces the sintering temperature. The present invention selects a lower sintering temperature range, combined with an appropriate sintering time, and can control the heating rate within the range of 1 to 10°C / min. When the precursor material within this range is sintered, it can avoid the problems of uneven crystal structure growth, increased grain boundaries or lattice distortion, and form an excellent single crystal structure, thereby having good battery stability and cycle performance. In addition, controlling a lower sintering temperature is also beneficial to reducing the generation of NiO crystalline phase, thereby reducing its exposure range on the surface of the material, reducing the side reaction with the electrolyte, and avoiding the possible NiO crystalline phase on the surface of the material. The surface reconstruction has an adverse effect on the single crystal structure. The sintering temperature, sintering time and heating rate in this parameter range can be coordinated to make the prepared sodium ion battery layered oxide positive electrode single crystal material have the best electrochemical performance.
[0054] In a third aspect, the present invention further provides a positive electrode plate, which is made of the sodium ion battery layered oxide positive electrode single crystal material, a conductive agent and a binder as described in the present invention.
[0055] The present invention does not particularly limit the type of conductive agent, as long as it has the function of enhancing the conductivity of the positive electrode and does not adversely affect the performance of the doped layered oxide positive electrode single crystal material. Those skilled in the art can select the conductive agent commonly used in the art according to actual needs. As some specific examples, the conductive agent used to prepare the positive electrode plate can be selected from carbon blacks such as acetylene black and conductive carbon black, conductive polymers such as carbon nanotubes, graphene, graphite, polyaniline, polythiophene, tin oxide, zinc oxide and other metal oxide conductive agents and carbon nanofiber conductive agents, etc.
[0056] The present invention does not particularly limit the type of binder, as long as it has the effect of enhancing the adhesion between the positive electrode active material particles and does not adversely affect the performance of the doped layered oxide positive electrode single crystal material. Those skilled in the art can choose according to actual needs. As some specific examples, the binder used to prepare the positive electrode plate includes polyvinylidene fluoride, polyvinylidene fluoride, polytetrafluoroethylene, polyvinyl alcohol, polyimide, polystyrene sulfonic acid, polyacrylonitrile, polycarbonate or polyetherimide ketone, etc.
[0057] The design of the positive electrode plate is unique and innovative. The positive electrode single crystal material has excellent electrochemical properties and has excellent capacity and cycle stability, which makes the positive electrode plate have broad application prospects in the field of sodium ion batteries, thereby greatly improving the overall performance of the battery and meeting the growing energy demand.
[0058] In a fourth aspect, the present invention provides a sodium ion battery, which includes the positive electrode sheet, negative electrode sheet, electrolyte and separator described in the third aspect. The sodium ion battery with layered oxide positive electrode single crystal material provided by the present invention can be used in multiple fields such as solar power generation, wind power generation, aerospace, distributed power stations, backup power supplies, military equipment or energy storage equipment for communication base stations; it has brought breakthrough progress to the battery industry, making sodium ion batteries a more competitive energy storage solution.
[0059] The following provides specific implementation cases to further fully illustrate the present invention.
[0060] Example 1
[0061] Preparation of O3-type Na 1.0 Ni 0.29 Cu 0.04 Fe 0.31 Mn 0.36 Bi 0.001 O2, weigh 2.34kg Na2CO3, 4kg specific characteristic spherical precursor Ni 0.29 Cu 0.04 Fe 0.31 Mn 0.36(OH)2 (D150 = 6.5 μm), 10.24 g Bi2O3 (d50 = 0.5 μm) and other raw materials were mixed at high speed and sintered at 900 ° C in a compressed air atmosphere for 20 h at a heating rate of 2 ° C / min. After crushing, a layered oxide positive electrode single crystal material (D50 = 8.6 μm) was obtained, which is recorded as Example 1; its XRD pattern is shown in Figure 1 As shown in the SEM images Figure 2 shown.
[0062] Embodiment 2:
[0063] Preparation of O3-type Na 1.03 Ni 0.31 Cu 0.03 Fe 0.33 Mn 0.33 Sr 0.005 Ca 0.005 O2, weigh 2.36kgNa2CO3, 4kg specific characteristic spherical precursor Ni 0.31 Cu 0.03 Fe 0.33 Mn 0.33 (OH)2 (D150 = 7.5 μm), 32.56 g SrCO3 (d50 = 0.55 μm) and 22.08 g CaCO3 (d50 = 0.55 μm) and other raw materials were mixed at high speed and sintered at 950 ° C in a compressed air atmosphere for 18 h at a heating rate of 2 ° C / min. After crushing, a layered oxide positive electrode single crystal material (D50 = 9.6 μm) was obtained, which is recorded as Example 2;
[0064] Embodiment 3:
[0065] Preparation of O3-type Na 0.95 Ni 0.31 Cu 0.02 Fe 0.35 Mn 0.32 Sr 0.0025 Ti 0.0025 O2, weigh 2.22kgNa2CO3, 4kg specific characteristic spherical precursor Ni 0.31 Cu 0.02 Fe 0.35 Mn 0.32 (OH)2 (D150 = 7.3 μm), 16.30 g SrCO3 (d50 = 0.8 μm) and 8.81 g TiO2 (d50 = 0.8 μm) and other raw materials were mixed at high speed and sintered at 970 ° C in a compressed air atmosphere for 15 h at a heating rate of 2 ° C / min. After crushing, a layered oxide positive electrode single crystal material (D50 = 8.4 μm) was obtained, which is recorded as Example 3;
[0066] Embodiment 4:
[0067] Preparation of O3-type Na 1.05 Ni 0.3 Cu 0.03 Fe 0.33 Mn 0.34 Sr 0.005 Y 0.005 Zr 0.005 O2, weigh 2.46kgNa2CO3, 4kg specific characteristic spherical precursor Ni 0.3 Cu 0.03 Fe 0.33 Mn 0.34 Raw materials such as (OH)2 (D150 = 4 μm), 26.06 g SrCO3 (d50 = 2 μm), 19.93 g Y2O3 (d50 = 2 μm) and 21.76 g ZrO2 (d50 = 2 μm) were mixed at high speed and sintered at 980°C in a compressed air atmosphere for 12 h at a heating rate of 2°C / min. After crushing, a layered oxide positive electrode single crystal material (D50 = 8.5 μm) was obtained, which is recorded as Example 4;
[0068] Embodiment 5:
[0069] Preparation of O3-type Na 1.02 Ni 0.3 Cu 0.03 Fe 0.33 Mn 0.34 Ti 0.01 Zr 0.01 O2, weigh 2.39kg Na2CO3, 4kg specific characteristic spherical precursor Ni 0.3 Cu 0.03 Fe 0.33 Mn 0.34 Raw materials such as (OH)2 (D150 = 10 μm), 35.25 g TiO2 (d50 = 0.2 μm) and 54.39 g ZrO2 (d50 = 0.2 μm) were mixed at high speed and sintered at 1000°C in a compressed air atmosphere for 10 h at a heating rate of 2°C / min. After crushing, a layered oxide positive electrode single crystal material (D50 = 12.1 μm) was obtained, which is recorded as Example 5;
[0070] Comparative Example 1:
[0071] The preparation steps are the same as those in Example 1, except that Bi2O3 is not added, and the layered oxide positive electrode single crystal material (D50=9.1 μm) is obtained and is recorded as Comparative Example 1;
[0072] Comparative Example 2:
[0073] The preparation steps are the same as those in Example 1, except that the d50 of the additive is 5 μm, and the obtained layered oxide positive electrode single crystal material (D50=9.4 μm) is recorded as Comparative Example 2;
[0074] Comparative Example 3:
[0075] The preparation steps are the same as those in Example 2, except that the D150 of the precursor material is 2 μm, and the obtained layered oxide positive electrode single crystal material (D50=3.4 μm) is recorded as Comparative Example 3;
[0076] Comparative Example 4:
[0077] The preparation steps are the same as those in Example 3, except that the D150 of the precursor material is 13.2 μm, and the obtained layered oxide positive electrode single crystal material (D50=20.4 μm) is recorded as Comparative Example 4;
[0078] Comparative Example 5:
[0079] The preparation steps are the same as those in Example 4, except that the sintering time is 8 h, and the obtained layered oxide positive electrode single crystal material (D50 = 7.3 μm) is recorded as Comparative Example 5; its SEM image is as follows Figure 3 shown.
[0080] Comparative Example 6:
[0081] The preparation steps are the same as those of Example 5, except that the sintering temperature is 1100° C. and the sintering time is 30 h, and the obtained layered oxide positive electrode single crystal material (D50=13.2 μm) is recorded as Comparative Example 6;
[0082] Test conditions and methods:
[0083] XRD test: Bruker D8 ADVANCE equipment was used for testing with a scanning range of 10-80. Jade, X-Ray, Highscore and other analysis software were used to calculate the peak area ratio.
[0084] Specific surface area test: The specific surface area of the material was tested using a precision Gaobo specific surface area analyzer, with reference to GB / T19587-2017 "Determination of the specific surface area of solid substances by gas adsorption BET method". The specific surface area of the material was tested using a precision Gaobo JW-DX dynamic adsorption specific surface area analyzer. 1g of sample was weighed, the heating temperature was set to 150°C, the degassing time was 60min, and the specific surface area data output after calculation by the software was recorded.
[0085] Button cell assembly: layered oxide positive electrode material, conductive agent Super P, and adhesive PVDF were used in a mass ratio of 90:5:5 to prepare positive electrode material slurry using a degassing machine. After adjusting the solid content of the slurry to 39% with N-methylpyrrolidone (NMP), the adjusted slurry was coated on aluminum foil using an automatic coating machine, dried at 120°C in a vacuum drying oven, rolled on a roller press, and punched with a slicer. After that, button 2032 batteries were assembled in a glove box. The electrolyte was 1.2 mol / L NaPF6, in which the solvent was EC:PC:EMC=1:1:1 (volume ratio), plus 2 wt.% FEC, the diaphragm was a glass fiber diaphragm, and a metal sodium sheet was used as the counter electrode.
[0086] Electrochemical test: The button half-cell was charged and discharged on a Xinwei tester in the voltage range of 2.5 to 4.05 V. 0.1C charge and discharge were performed three times, and then 1C charge and discharge test was performed to test the 0.1C first discharge capacity and first cycle charge and discharge efficiency, as well as the capacity retention rate after 50 cycles at 1C.
[0087] The above test results are listed in Tables 1-2 and Figure 1-2 middle.
[0088] Table 1
[0089]
[0090]
[0091] Table 2
[0092] sample Morphology 0.1C Capacity 1C rate 1C cycle / % Example 1 Single Crystal 142.3 93.2 96.30% Example 2 Single Crystal 141.1 92.1 94.40% Example 3 Single Crystal 138.9 92.7 93.30% Example 4 Single Crystal 143.4 91.8 95.30% Example 5 Single Crystal 140.3 92 94.60% Comparative Example 1 Single Crystal 137.8 87.9 86.60% Comparative Example 2 Single Crystal 137.1 86.9 82.60% Comparative Example 3 Single Crystal 136.3 84.1 82.40% Comparative Example 4 Single Crystal 139.1 85.7 82.90% Comparative Example 5 Single crystal 136.4 87.1 81.2% Comparative Example 6 Single Crystal 139.1 90.1 83.90%
[0093] It can be seen from the data in Table 1 that when the reasonably designed precursor, additives and sintering system of the present invention are selected, a crystalline material with a lower specific surface area can be obtained, and its δ value meets the requirements.
[0094] It can be seen from the data in Table 2 that Examples 1-5 generally have higher battery capacity, rate and battery cycle performance than Comparative Examples 1-4. This is because the product particle size and product specific surface area within the optimization range of the present invention are conducive to synergistically improving the fluxing effect of the material in a low copper system, reducing the sintering temperature, forming a good particle contact and adhesion level during the fluxing process, promoting the growth of the single crystal structure, and forming a stable single crystal structure. The high conductivity and electrochemical stability of the single crystal structure are helpful to improve the charge and discharge efficiency and cycle life of the battery; and the limited δ value indicates that the NiO crystalline phase is less exposed on the surface of the O3 phase, which is conducive to avoiding side reactions between the NiO crystalline phase and the electrolyte, affecting the environmental stability and initial capacity of the battery, thereby improving the battery capacity, rate and cycle performance of the material.
[0095] Examples 1-5 and Comparative Example 1 illustrate that the present invention can significantly reduce the exposure range of the NiO crystalline phase on the O3 phase surface by adding additives, improve the cycle performance of the material, and increase the capacity of the battery. This is because the addition of additives can further promote the formation of a good single crystal structure by improving the fluxing effect in a low copper system. The lower specific surface area also proves that the additives cooperate with the co-fluxing effect of copper to reduce the grain boundaries and reduce the interface side reactions, thereby having better cycle stability. It can be seen from Example 1 and Comparative Example 2 that selecting an additive with a suitable particle size will have better electrochemical performance. This is because the fluxing effect is poor in a low copper system. Selecting an additive with a suitable particle size range is conducive to more complete contact with the precursor material, causing lattice anomalies, accelerating the transmission rate of substances in the lattice, and reducing the sintering temperature; regulating the generation of NiO crystalline phases, reducing side reactions, and improving electrochemical performance.
[0096] It can be seen from Examples 2-3 and Comparative Examples 3-4 that Example 2-3 selects a suitable particle size range to have better battery capacity, rate and cycle performance; the present invention has a good fluxing effect through reasonable doping. When prepared within a suitable sintering time and sintering temperature range, a particle size that is too small will lead to abnormal crystallization, while a particle size that is too large will lead to insufficient crystallization, which is not conducive to forming a good single crystal structure; thereby reducing the capacity and cycle performance of the battery.
[0097] It can be seen from Examples 1 and 2-4 that within the low copper system range, a higher copper content is more conducive to reducing the exposure range of the NiO crystalline phase on the O3 phase surface, so that the copper-doped nickel-iron-manganese-based material has a higher fluxing effect, reducing the sintering temperature, and combining with a suitable sintering time, which is conducive to regulating the amount of NiO generated and obtaining the best performance sodium ion battery layered oxide positive electrode single crystal material.
[0098] It can be seen from Examples 4-5 and Comparative Examples 5-6 that when the sintering temperature is high and the sintering time is too long or too short, it is not conducive to improving the electrochemical performance of the battery, especially when the sintering time is too short, it forms a single-crystal-like morphology, this is because when the sintering time is too short, its crystal growth may be incomplete, and the particle rearrangement is insufficient, so that a uniform and continuous single crystal structure cannot be formed, and the polycrystalline structure will also provide more active sites due to the high specific surface area, resulting in the NiO crystalline phase having more exposure range on the O3 phase surface, increasing the side reaction with the electrolyte, and reducing the battery rate and cycle performance. And the higher sintering temperature will cause the grains to grow abnormally, and this abnormality will destroy the uniformity and continuity of the crystal, and will also cause the NiO crystalline phase to increase abnormally, so that the battery capacity, rate and cycle performance of the battery are reduced. The precursor material of the present invention has a higher fluxing effect by reasonable doping, and is selected in the range of reasonable sintering temperature, sintering time and heating rate, so that it has a better battery rate, capacity and cycle performance.
[0099] Depend on Figure 2 and Figure 3 It can be seen that Example 1 forms a uniform and continuous single crystal structure, while Comparative Example 5 forms an uneven single crystal-like structure. Figure 1 It can be seen that there is a clear and high diffraction peak, combined with Figure 1 It can be seen that the material has good crystal structure integrity, the crystals are arranged in an orderly manner and have high symmetry, forming a good single crystal structure.
[0100] The technical features of the above-described embodiments can be combined arbitrarily. In order to make the description concise, all possible combinations of the technical features in the above-described embodiments are not described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification. Although the embodiments of the present invention have been shown and described above, it can be understood that the above-described embodiments are exemplary and cannot be understood as limitations of the present invention. Those of ordinary skill in the art can change, modify, replace and deform the above-described embodiments within the scope of the present invention. In addition, those of ordinary skill in the art can combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples without contradiction.
Claims
1. A sodium ion battery layered oxide positive electrode single crystal material, the sodium ion battery layered oxide positive electrode single crystal material having the following general formula: Na x Ni a Cu b Fe c Mn d M y O2, where 0.95≤x≤1.05, 0.29≤a≤0.31, 0.02≤b≤0.04, 0.31≤c≤0.35, 0.32≤d≤0.36, 0.001≤y≤0.02, M is one or more elements selected from Sr, Ca, Ti, Zr, Y, and Bi; The particle size D50 of the positive electrode single crystal material satisfies 4μm≤D50≤20μm, and the specific surface area S satisfies S≤0.5m 2 / g; In the XRD of the positive electrode single crystal material, the ratio of NiO crystal phase to O3 phase is δ, δ=(A(111)+A(200)) / (A(003)+A(104))≤2%, wherein A(111) and A(200) are the peak areas of NiO (111) and (200) peaks in XRD, and A(003) and A(104) are the peak areas of O3 phase positive electrode (003) and (104) peaks in XRD.
2. The sodium ion battery layered oxide positive electrode single crystal material according to claim 1, characterized in that: In the general formula, 0.03≤b≤0.
04.
3. The sodium ion battery layered oxide positive electrode single crystal material according to claim 1, characterized in that: In the XRD of the positive electrode single crystal material, 0.04%≤δ≤0.3%.
4. The sodium ion battery layered oxide positive electrode single crystal material according to claim 1, characterized in that: The source of sodium is one or more of sodium metal, sodium salt, sodium oxide or sodium hydroxide.
5. The sodium ion battery layered oxide positive electrode single crystal material according to claim 1, characterized in that: The additive source of the M element includes one or more compounds of corresponding metal oxides, metal salts, and hydroxides; Furthermore, the particle size d50 of the additive of the M element satisfies 0.03 μm≤d50≤2 μm.
6. The sodium ion battery layered oxide positive electrode single crystal material according to claim 1, characterized in that: The precursor material of the sodium ion battery layered oxide positive electrode single crystal material meets the following specifications: Ni a Cu b Fe c Mn d (OH)2, where 0.29≤a≤0.31, 0.02≤b≤0.04, 0.31≤c≤0.35, 0.32≤d≤0.36, The precursor particle size D150 satisfies 4μm≤D150≤11μm, and the specific surface area BET satisfies 10m 2 / g<BET<30m 2 / g.
7. The sodium ion battery layered oxide positive electrode single crystal material according to claim 1, characterized in that: The sodium ion battery layered oxide positive electrode single crystal material, its precursor material contains impurity element Y, Y is one or more of Ca, Ti, Zr, Y, Bi, Co, Li, K, Al, Mg, Zn, Sb, Sc, Nb, V, Ga, Sr, Ba, Nd, Ce, and the content of impurity element Y is ≤5000ppm.
8. The sodium ion battery layered oxide positive electrode single crystal material according to claim 1, characterized in that: The ratio β of the additive particle size d50 of the M element to the precursor material particle size D150 (β=d50 / D150) satisfies 0.02≤β≤0.
5.
9. A method for preparing a sodium ion battery layered oxide positive electrode single crystal material, the preparation method comprising sintering a precursor material of the sodium ion battery layered oxide positive electrode single crystal material according to any one of claims 4 to 8, a sodium source, and an M element additive, the sintering temperature being 900 to 1000° C., the sintering time being 10 to 20 hours, and the heating rate being controlled to be 1 to 10° C. / min.
10. A sodium ion battery comprising a positive electrode sheet, a negative electrode sheet, an electrolyte and a separator, characterized in that: The active material in the positive electrode comprises the sodium ion battery layered oxide positive electrode single crystal material according to any one of claims 1 to 8 or the sodium ion battery layered oxide positive electrode single crystal material obtained by the preparation method of claim 9.
Citation Information
Cited By
Sodium ion battery monomer, battery device and electric equipment
CN121149372A
Sodium-ion battery cell, battery device, and electric device
CN121149372B