Electrolyte combination, secondary liquid injection method and lithium ion battery
By using a combination of two injection electrolytes in lithium-ion batteries, a stable SEI layer is formed using lithium salt, vinylene carbonate and fluoropropanesulfonolide organic matter, which solves the vinylene carbonate in the electrolyte The problem of uneven ester dispersion improves the cycle life and high temperature stability of lithium-ion batteries, achieving the goal of 10,000 cycles.
Patent Information
- Application Number
- CN202411064401.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-11-19
AI Technical Summary
The cycle life of existing lithium-ion batteries is insufficient, especially under high cycle times, the uneven dispersion of vinylene carbonate additives in the electrolyte leads to poor consistency of the SEI film, resulting in a dip in the battery cell capacity and deterioration of the cycle life.
Using an electrolyte combination, including the first electrolyte for the first injection and the second electrolyte for the second injection, by adding lithium salt, vinylene carbonate and fluorophosphoric acid to the first injection The organic substances of ylpropane sulfolide form a stable SEI layer to avoid an increase in DC resistance of the battery cell, and increase the amount of vinylene carbonate in the second injection to compensate for damage to the SEI film.
Without increasing the DC internal resistance of the battery cell, the cycle life of the lithium-ion battery is improved, and the goal of 0.5C is achieved, which avoids the problems of high viscosity of the electrolyte and uneven distribution of additives, ensuring the battery High temperature stability and cycling performance.
Smart Images

Figure CN118983519A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium ion batteries, and in particular to an electrolyte combination, a secondary liquid injection method and a lithium ion battery. Background Art
[0002] Lithium-ion batteries have the advantages of low self-discharge, high specific energy, specific power, charge and discharge efficiency, output voltage, and long service life. They have an absolute advantage in new energy storage installations and are an ideal energy storage technology. With the reduction of manufacturing costs, lithium-ion batteries are being installed on a large scale in the field of electrochemical energy storage, with strong growth momentum. With the popularization of lithium-ion battery applications, higher requirements are placed on the cycle life and capacity of lithium-ion battery energy storage, and the demand for large-capacity and long-life aluminum-shell iron-lithium energy storage batteries continues to increase.
[0003] Generally speaking, to extend the life of lithium-ion batteries, it is necessary to slow down the attenuation of battery capacity. The reasons for the capacity attenuation of lithium-ion batteries can be divided into two categories: 1) loss of active Li; 2) loss of positive and negative active materials. At the same time, the capacity attenuation of lithium-ion batteries is often accompanied by an increase in battery internal resistance and consumption of electrolyte (including the consumption of additives in the electrolyte). Therefore, it is necessary to reduce the loss of active Li when the SEI film (solid electrolyte interface film) is formed in the early stage of the cycle, and to prevent the co-embedding of solvent molecules by forming a dense and thermodynamically stable SEI film, avoid the damage to the electrode material by the interface side reaction, and reduce the loss of positive and negative active materials during the cycle, thereby improving the cycle life of lithium-ion batteries.
[0004] In lithium iron batteries, vinyl carbonate additives can effectively reduce the thickness of the SEI film, improve the battery's cycle stability and high-temperature performance, and are a mature and indispensable additive. When the amount of vinyl carbonate additive added to the electrolyte is too low, it cannot meet the necessary consumption required for repairing the SEI film in the late stage of a long cycle. If a sufficient amount of vinyl carbonate additive is added to the electrolyte at one time to meet the requirements of a long cycle life of the battery cell, the total amount of vinyl carbonate additive in the electrolyte is high at this time, the DCIR (direct current internal resistance) of the battery cell will increase significantly, the power performance will be poor, and the risk of lithium deposition and capacity drop in the battery cell will also increase.
[0005] At present, the main solutions to improve the cycle life are: 1) positive / negative lithium supplementation; 2) secondary injection. The secondary injection increases the total amount of vinyl carbonate added to the electrolyte by two separate injections, compensates for the damage caused by SEI decomposition during the cycle, and extends the cycle life of the battery. In the secondary injection scheme, the injection volume of the first injection is larger, and the proportion of vinyl carbonate additives is lower, avoiding the problem of large DCIR of the battery cell caused by the high addition of vinyl carbonate additives; the second injection volume is lower and contains a higher proportion of vinyl carbonate, which increases the ratio of vinyl carbonate in the overall electrolyte, plays the role of decomposing and compensating SEI in the middle and late stages of the cycle, thereby improving the cycle life performance of the battery cell. Usually, the vinyl carbonate additive is used in combination with a low-impedance film-forming additive during the first injection to further reduce the DCIR of the battery cell. At the same time, the concentration of vinyl carbonate in the second injection is higher, which increases the difficulty of wettability and uniformity of the injection.
[0006] With the demand for lithium-ion batteries to have a life of 10,000 cycles, the conventional secondary injection scheme with a total vinylene carbonate addition of 4wt% or less does not meet the requirements for cycle performance, storage performance, DCIR, etc., and it is necessary to further increase the amount of vinylene carbonate added. While keeping the amount of vinylene carbonate added in the first injection unchanged, the increase in the total amount of vinylene carbonate added will further increase the amount of vinylene carbonate additive in the second injection, significantly increase the viscosity of the electrolyte, increase the difficulty of injection, increase the difficulty of wetting the battery cell, and increase the difficulty of dispersing vinylene carbonate. The uneven dispersion of vinylene carbonate will make the consistency of SEI film formation poor, deteriorate the cycle performance of the battery cell, lead to cyclic lithium precipitation, cause the battery cell capacity to dive, and other serious deterioration of the cycle life of lithium-ion batteries.
[0007] Patent CN113904071B introduces a secondary injection electrolyte solution for lithium-ion batteries with lithium iron phosphate positive electrodes. In the first injection, vinylene carbonate and DTD (vinyl sulfate) are used together to reduce the DCIR of the battery. In the second injection, FB (fluorobenzene) is added to improve the dispersion and wetting problems caused by high concentrations of additives. Although additives such as FB can reduce the viscosity of the electrolyte and improve the wettability of the electrolyte, it is impossible to optimize the dispersion uniformity of vinylene carbonate after injection, and there is still a problem of poor consistency of SEI film formation caused by uneven dispersion of additives. Summary of the invention
[0008] The present invention provides an electrolyte combination. The present invention takes secondary injection, lithium salt, vinylene carbonate and fluorophosphate propane sultone organic matter as a basic scheme, and increases the content of vinylene carbonate during the first injection without increasing the DC internal resistance of the battery cell, thereby avoiding the problem of uneven distribution of additives after injection caused by only increasing the content of vinylene carbonate during the second injection.
[0009] The present invention discloses an electrolyte combination suitable for secondary injection, comprising a first electrolyte for the first injection and a second electrolyte for the second injection;
[0010] The first electrolyte contains 5-19wt% lithium salt, 3-3.5wt% vinylene carbonate, 0.1-0.6wt% fluorophosphate propane sultone organic compound additive, 0-5wt% positive and negative electrode film-forming additives and the balance non-aqueous organic solvent;
[0011] The second electrolyte contains 5-19wt% lithium salt, 13-25wt% vinylene carbonate and the balance non-aqueous organic solvent;
[0012] The weight ratio of the first electrolyte to the second electrolyte is 75-92:8-25.
[0013] Preferably, the weight ratio of the first electrolyte to the second electrolyte is 80-85:15-20. The battery cell of the lithium-ion battery can be fully wetted.
[0014] Preferably, the amount of the positive and negative electrode film-forming additives added is 0.1-4.5 wt %.
[0015] A higher proportion of vinylene carbonate is added to the first electrolyte, and fluorophosphate propane sultone organic compounds and positive and negative electrode film-forming additives are used together to partially inhibit the decomposition of vinylene carbonate while assisting in the formation of a stable SEI layer, thereby reducing the DC internal resistance of the battery cell.
[0016] If the amount of the fluorophosphate propane sultone organic compound added is less than 0.1wt%, it cannot play its due role; if the amount added is greater than 0.6wt%, the reaction degree of vinylene carbonate will be insufficient, which will have a deteriorating effect on SEI.
[0017] The lithium salt is selected from one or more of lithium hexafluorophosphate, lithium bis(trifluoromethanesulfonyl)imide, lithium perchlorate, lithium hexafluoroarsenate, and lithium 4,5-dicyano-2-(trifluoromethyl)isopyrazole.
[0018] The non-aqueous organic solvent is selected from dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, ethylene carbonate, propylene carbonate, methyl acetate, ethyl acetate, ethyl propionate, propyl propionate, fluorobenzene, fluoroethylene carbonate, fluoroethyl methyl carbonate, fluorodimethyl carbonate, and fluorodiethyl carbonate; the additive is one or more combinations of propane sultone, vinyl sulfate, methylene methanedisulfonate, vinyl sulfite, propylene sultone, tris(trimethylsilane) phosphate, propylene sulfate, tris(trimethylsilane) borate, lithium bis(oxalatoborate), lithium tetrafluoroborate, lithium difluorooxalatoborate, lithium difluorophosphate, lithium difluorooxalatophosphate, vinylene carbonate, fluoroethylene carbonate, vinylethylene carbonate, and 1,4-butane sultone.
[0019] The decomposition potential of the fluorophosphate propane sultone organic compound additive is lower than that of vinyl carbonate, and it is preferentially decomposed in the pre-charging formation stage, reducing the degree of decomposition of vinyl carbonate into film, thereby reducing the high internal resistance caused by the large amount of decomposition of vinyl carbonate into film. Fluorophosphate propane sultone organic compounds have sulfonate groups, have a lower decomposition voltage, and the decomposition film products have strong ion conductivity, which has the effect of reducing internal resistance; the fluorinated group is beneficial to improve the stability of the electrolyte and alleviate the decomposition and consumption of the electrolyte during the cycle; the phosphate group can inhibit the chromaticity change of the electrolyte, improve the stability of the electrolyte when it is shelved at high temperature, and also help to form a stable SEI to avoid the occurrence of side reactions during the cycle.
[0020] The first innovative point of the present invention is: after two injections, the amount of vinylene carbonate added to the electrolyte is greater than 5wt%, wherein the first injection adds more than 3.0wt% of vinylene carbonate, the positive and negative electrode film-forming agents are used in combination, and the fluorophosphate propane sultone organic compound is added to avoid the increase of the DC internal resistance of the battery in the first cycle, the cycle drop, and the rapid increase of the DC internal resistance, thereby achieving the goal of 10,000 cycles of lithium-ion batteries at 0.5C. The second innovative point is: by increasing the amount of vinylene carbonate added in the two injections at the same time, the problem of high electrolyte viscosity and difficulty in injection caused by increasing the amount of vinylene carbonate added only in the second injection is avoided, and the problem of uneven distribution of additives after injection due to excessive difference in the concentration of vinylene carbonate in the two injections is avoided, and the resulting poor film formation uniformity and battery cycle capacity drop are avoided. The third innovation point is: through the preferential film formation of the new fluorophosphate-based propane sulfone organic compound additive, it competes with the decomposition and film formation of high-concentration vinylene carbonate, reduces the decomposition amount of vinylene carbonate, and thus solves the problem of excessive DC internal resistance in the first cycle caused by high-concentration vinylene carbonate.
[0021] Furthermore, the fluorophosphate propane sultone organic compound has a chemical structure as shown in formula (I):
[0022]
[0023] Wherein, R1 and R2 are independently selected from hydrogen, halogen, substituted or unsubstituted alkane group, alkene group, alkyne group, aromatic group, phosphate group, sulfonate group, sulfate group, borate group, siloxy group, amino group, nitro group, oxalate group, dibasic acid anhydride group, difluorophosphate group, monofluorophosphate group, isocyanate group or carbonyl group.
[0024] Furthermore, the R1 and the R2 are independently selected from halogen, olefin, alkane or isocyanate.
[0025] Furthermore, the fluorophosphate propane sultone organic compound is one of the following structures:
[0026]
[0027] Further, the positive and negative electrode film-forming additives are selected from one or more of propane sultone, vinyl sulfate, methylene disulfonate, vinyl sulfite, propylene sultone, tris(trimethylsilane) phosphate, propylene sulfate, tris(trimethylsilane) borate, lithium bis(oxalatoborate), lithium tetrafluoroborate, lithium difluorooxalatoborate, lithium difluorophosphate, lithium difluorooxalatophosphate, vinylene carbonate, fluoroethylene carbonate, vinylethylene carbonate, methylene methanesulfonate, 1,3-propane sultone, vinyl sulfate, tris(trimethyl)silyl phosphate, lithium tetrafluorooxalatophosphate, lithium difluorooxalatoborate, lithium difluorophosphate, and 1,4-butane sultone.
[0028] Furthermore, the positive and negative electrode film-forming additives are selected from one or more of methylene methanesulfonate, 1,3-propane sultone, vinyl sulfate, tris(trimethyl)silyl phosphate, lithium tetrafluorooxalate phosphate, lithium difluorooxalate borate, and lithium difluorophosphate.
[0029] Furthermore, the addition amount of the positive and negative electrode film-forming additives is 1.0-2.6wt%, and is selected from at least two of fluoroethylene carbonate, vinyl sulfate, and tris(trimethylsilyl)phosphate.
[0030] The present invention also discloses a secondary liquid injection method, which adopts the electrolyte combination as described above; the method comprises the following steps performed in sequence:
[0031] (1) injecting a first electrolyte into the battery cell;
[0032] (2) Pre-charge;
[0033] (3) Formation;
[0034] (4) injecting a second electrolyte into the fully charged battery cell;
[0035] (5) Aging;
[0036] (6) Divide capacity.
[0037] Furthermore, in the step (2), the specific operation is to charge at 0.01C for 0.5-1.5h, charge at 0.02C for 8-12h, and charge at 0.1C constant current for 0.5-1.2h; then place at high temperature of 38°C for 30-60h, and place at room temperature of 25°C for 4-6h.
[0038] Furthermore, in the step (3), the specific operation is 0.1C constant current charge / discharge, then 0.1C constant current charge to 3.65V; high temperature 38°C for 18-30h; room temperature 25°C for 4-6h.
[0039] Furthermore, in the step (5), the specific operation is to place at a high temperature of 38°C for 24-72 hours; and place at a room temperature of 25°C for 5 hours.
[0040] Furthermore, in step (6), 0.1C constant current charging / discharging, and then 1C constant current charging / discharging;
[0041] The present invention also provides a lithium ion battery, which is prepared by the method described above, and has a 30-day storage capacity recovery rate greater than 98%, and a capacity retention rate greater than 91.5% after 3000 cycles at 25°C.
[0042] The positive electrode active material of the lithium ion battery used in the present invention is one or more of the commonly used positive electrode active materials, such as lithium cobalt oxide, lithium manganese oxide, lithium nickel oxide, lithium iron phosphate, lithium manganese iron phosphate, nickel cobalt manganese ternary material, nickel cobalt aluminum ternary material, lithium-rich manganese, etc.
[0043] The present invention does not strictly limit the type of negative electrode active material, and currently commonly used negative electrode active materials can meet the requirements of the present invention, such as natural graphite, artificial graphite, hard carbon, soft carbon, silicon carbon, silicon dioxide, lithium titanate, etc.
[0044] The present invention does not strictly limit the selection range of the diaphragm, and commonly used diaphragms meet the requirements of the present invention, for example: polypropylene diaphragm (PP), polyethylene diaphragm (PE), polyethylene / polypropylene double-layer composite film, polyimide electrospinning diaphragm (PI), polypropylene / polyethylene / polypropylene three-layer composite diaphragm (PP / PE / PP), ceramic diaphragm, PVDF coated diaphragm, etc.
[0045] The secondary injection method disclosed in the present invention reduces the decomposition amount of vinylene carbonate by preferentially forming a film of a novel fluorophosphate propane sultone organic compound additive during the first injection, thereby competing with the decomposition film formation of high-concentration vinylene carbonate, and solves the problem of excessively high first-cycle DC internal resistance caused by high-concentration vinylene carbonate.
[0046] In the present invention, the amount of vinylene carbonate added to the electrolyte of the first injection is 3.0-3.5wt%, the amount of fluorophosphate propane sultone organic compound additive added is 0.1-0.6wt%, and the amount of film-forming additive added is 0-5wt%. The problem of high internal resistance caused by excessive decomposition of high-concentration vinylene carbonate is suppressed by limited decomposition of fluorophosphate propane sultone organic compounds, thereby forming a SEI with low DC internal resistance, thermal stability and good mechanical properties. Then, the amount of vinylene carbonate additive added to the electrolyte is increased to 5-7wt% by the second injection, and a cycle life of 10,000 times of the lithium-ion battery is achieved without increasing the DC internal resistance of the battery cell. BRIEF DESCRIPTION OF THE DRAWINGS
[0047] Figure 1 It is the dQ / dV of Example 1, Example 5 and Comparative Example 1 in the pre-charge stage of the present invention. DETAILED DESCRIPTION
[0048] In order to make the technical solution of the present invention clearer, the present invention is further described in detail below with reference to the accompanying drawings and specific embodiments.
[0049] In addition to the concepts with meanings in the present invention, the concepts and technical terms involved in the following embodiments and comparative examples have the same meanings as those related to the field of lithium-ion batteries. The reagents involved in the following embodiments and comparative examples are all conventional chemical reagents unless otherwise specified; the experimental methods used in the present invention are all conventional methods. The present invention illustrates the influence of the secondary injection electrolyte solution of the present invention on the electrochemical performance of lithium-ion batteries by comparing the test data of the embodiments and comparative examples.
[0050] The electrolytes in the examples and comparative examples of this patent are prepared using the following steps: controlling the moisture content in the glove box to be less than 10 ppm, and controlling the moisture content of the solvent to be less than 10 ppm.
[0051] The positive electrode active material of the aluminum shell battery used in the embodiments and comparative examples of this patent is lithium iron phosphate, the negative electrode active material is artificial graphite, and the diaphragm adopts a three-layer composite ceramic diaphragm of polypropylene / polyethylene / polypropylene.
[0052] The main preparation method of the positive electrode sheet is to disperse lithium iron phosphate, conductive agent, and binder polyvinylidene fluoride (PVDF) in an appropriate amount of N-methylpyrrolidone according to a mass ratio of 95.5:2:2.5, and then stir them thoroughly according to the homogenization process. The evenly dispersed positive electrode slurry is evenly coated on aluminum foil, and the positive electrode sheet is obtained after baking, rolling, slitting, and punching.
[0053] The specific production process of the negative electrode sheet is as follows: artificial graphite, conductive agent, styrene-butadiene rubber (SBR), sodium carboxymethyl cellulose (CMC), all raw materials are put into a planetary mixing tank at a mass ratio of 96:1:2:1, and a uniformly dispersed negative electrode slurry is prepared according to the slurry making process. Then the negative electrode slurry is evenly coated on the copper foil, and after baking, rolling, slitting, and punching, the negative electrode sheet is obtained.
[0054] After the positive and negative electrodes are punched, the positive electrode is placed in an oven at 130°C and the negative electrode is placed in an oven at 95°C for 25 hours. When the moisture content of the electrode meets the requirements, the positive electrode, negative electrode and separator are placed in a stacking machine to stack into bare cells, and then the bare cells are packaged into stamped aluminum shells. The packaged dry cells are dried at 90°C for 12 hours.
[0055] The preparation methods of S1-S4 are as follows:
[0056] Synthesis method of S1:
[0057]
[0058] Synthesis method of S2:
[0059]
[0060] Synthesis method of S3:
[0061]
[0062]
[0063] Synthesis method of S4:
[0064]
[0065] Example 1
[0066] The composition of the first electrolyte is: 12.5wt% of lithium hexafluorophosphate, 3.5wt% of vinylene carbonate (VC), 1.5wt% of fluoroethylene carbonate, 0.8wt% of vinyl sulfate, 0.3wt% of tri(trimethylsilyl) phosphate, 0.25wt% of an organic compound additive with the structural formula S1 fluorophosphate propane sulfone and the remainder of a non-aqueous organic solvent.
[0067] The second electrolyte solution comprises 12.5 wt % of lithium hexafluorophosphate, 20.2 wt % of VC and the remainder of a non-aqueous organic solvent.
[0068] The total VC addition amount in the electrolyte is 6wt%.
[0069] The non-aqueous organic solvent in the first electrolyte is: ethylene carbonate, dimethyl carbonate, ethyl methyl carbonate, and the mass ratio thereof is: 1:1:2;
[0070] The non-aqueous organic solvent in the second electrolyte is ethylene carbonate and ethyl methyl carbonate, and the mass ratio thereof is 1:1.5.
[0071] The injection steps are as follows:
[0072] Step 1: Inject the first electrolyte into the aluminum shell battery cell with qualified moisture content and soak it at room temperature for 48 hours.
[0073] Step 2: Pre-charge, charge at 0.01C for 1h, charge at 0.02C for 10h, charge at 0.1C constant current for 1h; place at 38℃ for 50h; place at room temperature 25℃ for 5h.
[0074] Step 3: Formation, 0.1C constant current charge / discharge, then 0.1C constant current charge to 3.65V; place at 38℃ high temperature for 24h; place at room temperature 25℃ for 5h.
[0075] Step 4: Inject the second electrolyte into the fully charged battery cell.
[0076] Step 5: Aging: place at high temperature of 38℃ for 48h; place at room temperature of 25℃ for 5h.
[0077] Step 6: Capacity division, 0.1C constant current charge / discharge, then 1C constant current charge / discharge.
[0078] The amount of the first electrolyte injection accounts for 85wt% of the total injection amount, and the amount of the second electrolyte injection accounts for 15wt% of the total injection amount.
[0079] Example 2
[0080] The difference between this embodiment and embodiment 1 is that:
[0081] The composition of the first electrolyte is: 12.5wt% of lithium hexafluorophosphate, 3.5wt% of vinylene carbonate (VC), 1.5wt% of fluoroethylene carbonate, 0.8wt% of vinyl sulfate, 0.3wt% of tri(trimethylsilyl) phosphate, 0.25wt% of a fluorophosphate-based propane sultone organic compound additive with the structural formula S2, and the remainder of a non-aqueous organic solvent.
[0082] Example 3
[0083] The difference between this embodiment and embodiment 1 is that:
[0084] The composition of the first electrolyte is: 12.5wt% of lithium hexafluorophosphate, 3.5wt% of vinylene carbonate (VC), 1.5wt% of fluoroethylene carbonate, 0.8wt% of vinyl sulfate, 0.3wt% of tri(trimethylsilyl) phosphate, 0.25wt% of a fluorophosphate-based propane sultone organic compound additive with the structural formula S3, and the remainder of a non-aqueous organic solvent.
[0085] Example 4
[0086] The difference between this embodiment and embodiment 1 is that:
[0087] The composition of the first electrolyte is: 12.5wt% of lithium hexafluorophosphate, 3.5wt% of vinylene carbonate (VC), 1.5wt% of fluoroethylene carbonate, 0.8wt% of vinyl sulfate, 0.3wt% of tri(trimethylsilyl) phosphate, 0.25wt% of a fluorophosphate-based propane sultone organic compound additive with the structural formula S4, and the remainder of a non-aqueous organic solvent.
[0088] Example 5
[0089] The difference between this embodiment and embodiment 1 is that:
[0090] The composition of the first electrolyte is: 12.5wt% of lithium hexafluorophosphate, 3.5wt% of vinylene carbonate (VC), 0.8wt% of vinyl sulfate, 0.3wt% of tris(trimethylsilyl) phosphate, 0.55wt% of a fluorophosphate-based propane sultone organic compound additive with the structural formula S1, and the remainder of a non-aqueous organic solvent.
[0091] Example 6
[0092] The difference between this embodiment and embodiment 1 is that:
[0093] The first electrolyte is composed of 12.5 wt% lithium hexafluorophosphate, 3.5 wt% vinylene carbonate (VC), 0.8 wt% vinyl sulfate, 0.3 wt% tris(trimethylsilyl) phosphate, 0.55 wt% fluorophosphate propane sultone organic compound additive with the structural formula S2 and the balance non-aqueous organic solvent.
[0094] Example 7
[0095] The difference between this embodiment and embodiment 1 is that:
[0096] The composition of the first electrolyte is: 12.5wt% of lithium hexafluorophosphate, 3.5wt% of vinylene carbonate (VC), 0.8wt% of vinyl sulfate, 0.3wt% of tris(trimethylsilyl) phosphate, 0.55wt% of a fluorophosphate-based propane sultone organic compound additive with the structural formula S3, and the remainder of a non-aqueous organic solvent.
[0097] Example 8
[0098] The difference between this embodiment and embodiment 1 is that:
[0099] The composition of the first electrolyte is: 12.5wt.% lithium hexafluorophosphate, 3.5wt.% vinylene carbonate (VC), 0.8wt.% vinyl sulfate, 0.3wt.% tri(trimethylsilyl) phosphate, 0.55wt.% S4 fluorophosphate-based propane sulfone organic compound additive and the remainder of non-aqueous organic solvent.
[0100] Example 9
[0101] The difference between this embodiment and embodiment 1 is that the injection amount of the first electrolyte accounts for 75wt% of the total injection amount, and the injection amount of the second electrolyte accounts for 25wt% of the total injection amount.
[0102] Example 10
[0103] The difference between this embodiment and embodiment 1 is that the injection amount of the first electrolyte accounts for 90% of the total injection amount, and the injection amount of the second electrolyte accounts for 10wt% of the total injection amount.
[0104] Comparative Example 1
[0105] The difference between this embodiment and embodiment 1 is that the composition of the first electrolyte is: 12.5wt% of lithium hexafluorophosphate, 3.5wt% of vinylene carbonate (VC), 1.5wt% of fluoroethylene carbonate, 0.8wt% of vinyl sulfate, 0.3wt% of tris(trimethylsilyl) phosphate and the remainder of non-aqueous organic solvent.
[0106] Comparative Example 2
[0107] The difference between this embodiment and embodiment 1 is that the composition of the first electrolyte is: 12.5wt% of lithium hexafluorophosphate, 3.5wt% of vinylene carbonate (VC), 1.8wt% of fluoroethylene carbonate, 0.8wt% of vinyl sulfate, 0.3wt% of tris(trimethylsilyl)phosphate and the remainder of non-aqueous organic solvent.
[0108] Performance Test:
[0109] The electrolytes and cells of the embodiments and comparative examples were tested and their performance differences were compared using the following methods:
[0110] The state of the electrode after formation, the DC internal resistance of the formation line, and the dQ / dV in the pre-charge stage
[0111] After formation, the battery was fully charged and disassembled to confirm the battery electrode condition. The relevant test results are shown in Table 1. The dQ / dV of Example 1, Example 5 and Comparative Example 1 in the pre-charge stage are as follows: Figure 1 .
[0112] Lithium-ion battery 60°C storage test
[0113] The steps of the high temperature storage performance test of the battery cell in the embodiments and comparative examples of this patent are as follows: discharge the fixed capacity battery cell to 2.5V at 1C constant current, leave it for 5 minutes, and then charge it to 3.65V at 1C constant current and constant voltage, with a cut-off current of 0.05C. The battery was placed in a constant temperature box at 60°C and stored for 30 days respectively. After the battery reaches the specified storage date, take out the battery cell, connect the battery test cabinet, discharge it to 2.5V at 1C constant current, and then charge it at 1C constant current and constant voltage. The 1C constant current discharge process is repeated 3 times. Finally, the discharge capacity recovery rate of the battery cell is obtained. The same battery is charged at 1C constant current and constant voltage, and then the discharge time at 50% SOC is calculated according to the discharge capacity, and the capacity of the battery is adjusted to 50% SOC. After standing for one hour, the battery cell is charged and discharged for 20 seconds with a 3C pulse current. According to the change in voltage, the DC internal resistance of the battery is calculated. The relevant test results are shown in Table 1.
[0114] Lithium-ion battery 45°C cycle test
[0115] The embodiments and comparative examples in the patent carry out a 45°C cycle test on lithium-ion batteries according to the following steps. The detailed steps are as follows: Take a lithium-ion battery that has been fixed in capacity and place it in a constant temperature box at 45°C. In order to fully reduce the temperature of the battery, control the shelf time of the battery to ensure that it is more than 1 hour. Then charge it at a constant current and constant voltage of 1C, with a cut-off voltage of 3.6V and a cut-off current of 0.05C. Then discharge it to 2.5V at a constant current of 1C. Perform charge and discharge cycles on the battery according to the above steps, and record the discharge capacity retention rate after 2000 cycles. The discharge capacity retention rate of the battery after 1000 cycles is calculated as the discharge capacity of the battery after 1000 cycles divided by the discharge capacity of the battery in the first cycle. See Table 1 for specific test data.
[0116] Lithium-ion battery 25°C cycle test
[0117] The embodiments and comparative examples in the patent are subjected to 25°C cycle test on lithium-ion batteries according to the following steps. The detailed steps are as follows: At room temperature, take a lithium-ion battery that has been fixed in volume, charge it at 1C constant current and constant voltage, the cut-off voltage is 3.6V, and the cut-off current is 0.05C. Then discharge it to 2.5V at 1C constant current. Perform charge and discharge cycles on the battery according to the above steps, and record the discharge capacity retention rate after 3000 cycles. See Table 1 for specific test data.
[0118] Table 1 High temperature and room temperature performance test results of lithium-ion batteries
[0119]
[0120]
[0121] Result analysis:
[0122] By comparing Examples 1-4 with Comparative Examples 1-2, it can be seen that the addition of fluorophosphate propane sultone organic compound additives S1-S4 in the first electrolyte can significantly reduce the DC internal resistance of the battery cell, and also effectively inhibit the growth of the DC internal resistance of the storage battery cell, and improve the capacity retention rate of high-temperature storage, high-temperature 45°C cycling, and room temperature 25°C cycling;
[0123] like Figure 1 As shown in the figure, the peak near 2.5V is the decomposition peak of VC. After adding S1, the decomposition peak of VC becomes weaker, which indicates that the addition of S1 partially inhibits the decomposition of VC, which is consistent with the result that the DC internal resistance of the battery cell filled with the electrolyte containing the S1 additive is lower after formation. The effects of S2-S4 are consistent with those of S1, and they can partially inhibit the decomposition of VC.
[0124] As shown in Table 1, obvious black spots appeared in the battery cell of Example 9 after formation. This is because the electrolyte added in the first injection is insufficient and the battery cell is not fully wetted. By comparing Example 1 and Examples 9-10, the performance is best when the mass ratio of the first injection electrolyte is 85%. It is recommended that the addition ratio of the first injection electrolyte should not be too low, and should be 80% or above;
[0125] By comparing Examples 1-4 with Examples 5-8, it can be seen that reducing fluoroethylene carbonate and increasing the amount of fluorophosphate propane sultone organic compound additives S1-S4 have a positive effect on reducing the DC internal resistance of the battery cell and optimizing the storage and cycle performance. This is because fluoroethylene carbonate and fluorophosphate propane sultone organic compound additives compete for film formation and both have the effect of partially inhibiting VC film formation, and the stability of the film-forming decomposition product of fluoroethylene carbonate is inferior to that of fluorophosphate propane sultone organic compound additives, so Examples 5-8 have better storage and cycle performance.
[0126] The above-mentioned embodiments only express several implementation methods of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the patent of the present invention. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. An electrolyte combination suitable for secondary injection, characterized in that: comprising a first electrolyte for a first injection and a second electrolyte for a second injection; The first electrolyte contains 5-19wt% lithium salt, 3-3.5wt% vinylene carbonate, 0.1-0.6wt% fluorophosphate propane sultone organic compound additive, 0-5wt% positive and negative electrode film-forming additives and the balance non-aqueous organic solvent; The second electrolyte contains 5-19wt% lithium salt, 13-25wt% vinylene carbonate and the balance non-aqueous organic solvent; The weight ratio of the first electrolyte to the second electrolyte is 75-92:8-25.
2. The electrolyte combination suitable for secondary injection according to claim 1, characterized in that: The fluorophosphate propane sultone organic compound has a chemical structure as shown in formula (I): Wherein, R1 and R2 are independently selected from hydrogen, halogen, substituted or unsubstituted alkane group, alkene group, alkyne group, aromatic group, phosphate group, sulfonate group, sulfate group, borate group, siloxy group, amino group, nitro group, oxalate group, dibasic acid anhydride group, difluorophosphate group, monofluorophosphate group, isocyanate group or carbonyl group.
3. The electrolyte combination suitable for secondary injection according to claim 2, characterized in that: The R1 and R2 are independently selected from halogen, olefin group, alkane group or isocyanate group.
4. The electrolyte combination suitable for secondary injection according to claim 3, characterized in that: The fluorophosphate propane sultone organic compound is one of the following structures:
5. The electrolyte combination suitable for secondary injection according to claim 1, characterized in that: The positive and negative electrode film-forming additives are selected from one or more of propane sultone, vinyl sulfate, methylene methane disulfonate, vinyl sulfite, propylene sultone, tris(trimethylsilane) phosphate, propylene sulfate, tris(trimethylsilane) borate, lithium bis(oxalatoborate), lithium tetrafluoroborate, lithium difluorooxalatoborate, lithium difluorophosphate, lithium difluorooxalatophosphate, vinylene carbonate, fluoroethylene carbonate, vinylethylene carbonate, methylene methanesulfonate, 1,3-propane sultone, vinyl sulfate, tris(trimethyl)silyl phosphate, lithium tetrafluorooxalatophosphate, lithium difluorooxalatoborate, lithium difluorophosphate, and 1,4-butane sultone.
6. The electrolyte combination suitable for secondary injection according to claim 5, characterized in that: The positive and negative electrode film-forming additives are selected from one or more of methylene methanesulfonate, 1,3-propane sultone, vinyl sulfate, tris(trimethyl)silyl phosphate, lithium tetrafluorooxalate phosphate, lithium difluorooxalate borate, and lithium difluorophosphate.
7. A secondary liquid injection method, characterized in that: The method adopts the electrolyte combination as described in any one of claims 1 to 6; the method comprises the following steps performed in sequence: (1) injecting a first electrolyte into the battery cell; (2) Pre-charge; (3) Formation; (4) injecting a second electrolyte into the fully charged battery cell; (5) Aging; (6) Capacity division.
8. A secondary liquid injection method according to claim 7, characterized in that: In the step (2), the specific operation is to charge at 0.01C for 0.5-1.5h, charge at 0.02C for 8-12h, and charge at 0.1C constant current for 0.5-1.2h; then place at high temperature of 38°C for 30-60h, and place at room temperature of 25°C for 4-6h.
9. A secondary liquid injection method according to claim 7, characterized in that: In the step (3), the specific operation is 0.1C constant current charge / discharge, then 0.1C constant current charge to 3.65V; high temperature 38°C for 18-30h; room temperature 25°C for 4-6h.
10. A lithium ion battery, characterized in that: The nanostructured carbon nanotube is prepared by the method as described in any one of claims 7 to 9, and has a 30-day storage capacity recovery rate greater than 98%, and a capacity retention rate greater than 91.5% after 3000 cycles at 25°C.