Energy storage cell and preparation method thereof
By setting an insulating reinforcement layer at the end of the electrode and separating it from the active material layer, the problem of insufficient mechanical strength of lithium battery electrodes is solved, and the safety and electronic transmission capability of the cell are improved.
Patent Information
- Application Number
- CN202411216627.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-11-19
AI Technical Summary
The existing lithium battery tabs have insufficient mechanical strength and are prone to tearing, leading to safety risks and poor cell performance.
An insulating reinforcement layer is provided at the end of the tab to enhance its mechanical strength and to separate it from the active material layer to prevent cross-contamination. The position and thickness of the insulating reinforcement layer are precisely controlled by a dispensing process.
It improves the mechanical properties of the tabs, reduces the probability of cell tearing and differential pressure failure, and enhances the electron transport capability and safety of lithium-ion batteries.
Smart Images

Figure CN118983540A_ABST
Abstract
Description
Technical Field
[0001] The embodiments of the present application relate to the field of energy storage, and in particular to an energy storage battery cell and a method for preparing the same. Background Art
[0002] In recent years, lithium-ion batteries have attracted great attention due to their excellent characteristics such as high energy density, high output voltage, low self-discharge rate, long service life, no memory effect and environmental friendliness. They have developed by leaps and bounds, their market share has continued to expand, and they have occupied a dominant position.
[0003] At present, single lithium batteries are mainly cylindrical, square and soft-pack. The methods adopted in the battery production process are mainly stacking and winding. The stacking method is generally die-cut and then cut and stacked, which has low production efficiency, low consistency precision, and low rate and cycle performance. The winding method has higher production efficiency, but generally non-die-cutting process batteries use the post-process welding of the pole ears for drainage, which cannot well meet the high rate performance of energy storage batteries.
[0004] Among them, square batteries are mostly single-pole ear process and multi-pole ear process. The single-pole ear process is to connect the pole ear to the pole piece by ultrasonic welding before winding the pole piece, and then wind it into a battery through the welded pole ear drainage; the multi-pole ear process is to die-cut the pole piece. After die-cutting, it can be divided into two types: one is to stack the pieces after cutting, and the other is to directly wind. Both of them finally use the pole piece end as the pole ear for multi-pole ear super welding as the drainage terminal. Since the positive and negative poles of the single-pole ear are on the same side, the current-carrying area is small, resulting in poor overcurrent capacity and poor rate performance. In addition, since the single-pole ear process requires the pole ear to be welded on the pole piece separately, and in this process, the pole ear is very easy to tear, and there is no effective full inspection and interception measures. After flowing out, there are safety risks in the battery cell and poor pressure difference between the battery cells in the module. Summary of the invention
[0005] The embodiments of the present application provide an energy storage battery cell and a method for preparing the same, which are at least helpful in solving the problem of the mechanical strength of the tab.
[0006] According to some embodiments of the present application, on the one hand, an energy storage cell is provided in the embodiments of the present application, comprising: a diaphragm, and a positive electrode sheet and a negative electrode sheet located on both sides of the diaphragm; the positive electrode sheet comprises: a current collector, the current collector having a pole ear and an active material portion arranged along a first direction; an insulating reinforcement layer, the insulating reinforcement layer is at least located at the pole ear and the junction between the pole ear and the active material portion, and a first preset range is provided between the insulating reinforcement layer and the end of the pole ear along the first direction; an active material layer, the active material layer is located on the current collector corresponding to the active material portion, and a second preset range is provided between the active material layer and the insulating reinforcement layer along the first direction; the thickness of the insulating reinforcement layer is less than or equal to the thickness of the active material layer; wherein the insulating reinforcement layer satisfies the formula: 450≤W*H2 / (H1) 2 ≤1100, W is the width of the insulation reinforcement layer along the first direction, H1 is the thickness of the insulation reinforcement layer, and H2 is the thickness of the active material layer.
[0007] In some embodiments, the insulating reinforcement layer further extends to the current collector corresponding to the active material portion, wherein a width of the insulating reinforcement layer extending to the active material portion along the first direction is less than or equal to 5 mm.
[0008] In some embodiments, the first preset range is 6 mm to 20 mm; the second preset range is 0.5 mm to 1.5 mm.
[0009] In some embodiments, the positive electrode sheet further includes: a conductive carbon layer, wherein the conductive carbon layer is located between the current collector and the active material layer.
[0010] In some embodiments, the conductive carbon layer is located on the surface of the current collector, and the conductive carbon layer is also located between the current collector and the insulating reinforcement layer.
[0011] In some embodiments, the width of the insulation reinforcement layer along the first direction is 5 mm to 7 mm.
[0012] According to some embodiments of the present application, on the other hand, the embodiments of the present application further provide a method for preparing an energy storage battery cell, including: providing a current collector, the current collector having two pole ear portions and an active material portion located between the two pole ear portions; forming an insulation reinforcement layer, the insulation reinforcement layer being located at least at the pole ear portion and at the junction between the pole ear portion and the active material portion, and having a first preset range between the insulation reinforcement layer and the end of the pole ear portion along the first direction; forming an active material layer, the active material layer being located on the current collector corresponding to the active material portion, and having a second preset range between the active material layer and the insulation reinforcement layer along the first direction; the thickness of the insulation reinforcement layer is less than or equal to the thickness of the active material layer; wherein the insulation reinforcement layer satisfies the formula: 450≤W*H2 / (H1) 2 ≤1100, W is the width of the insulating reinforcement layer along the first direction, H1 is the thickness of the insulating reinforcement layer, H2 is the thickness of the active material layer, and the first direction is the arrangement direction of the pole ear portion and the active material portion; the current collector corresponding to the pole ear portion is die-cut according to preset parameters so that the pole ear portion of the current collector forms a pole ear; the current collector is cut to form two identical positive electrode sheets; a diaphragm and a negative electrode sheet are provided, the diaphragm is located between the positive electrode sheet and the negative electrode sheet, and the diaphragm, the positive electrode sheet and the negative electrode sheet are wound.
[0013] In some embodiments, the insulation reinforcement layer is formed by using a dispensing process.
[0014] In some embodiments, the process steps for forming the insulation enhancement layer include: mixing the polyimide material and ceramic particles evenly to form a mixed slurry; wherein the mass percentage of the ceramic particles is 80wt% to 95wt%, and the mass percentage of the polyimide material is 5wt% to 20wt%; coating the mixed slurry on the current collector and drying to form the insulation enhancement layer.
[0015] In some embodiments, the process steps for forming the insulating reinforcement layer include: mixing a polyimide material and a polyvinylidene fluoride material evenly to form a mixed slurry; wherein the mass percentage of the polyimide material is 80wt% to 95wt%, and the mass percentage of the polyvinylidene fluoride material is 5wt% to 20wt%; coating the mixed slurry on the current collector and drying to form the insulating reinforcement layer.
[0016] The technical solution provided by the embodiments of the present application has at least the following advantages:
[0017] The energy storage cell provided in the embodiment of the present application has an insulating reinforcement layer arranged on the current collector, and the insulating reinforcement layer is located on the pole ear and at the junction of the pole ear and the active material part, that is, at the end of the pole ear close to the active material part, so that the insulating reinforcement layer can completely wrap the end of the pole ear and the junction of the pole ear and the active material part, and the setting of the insulating reinforcement layer can enhance the mechanical strength of the current collector, that is, increase the mechanical properties of the pole ear, and show the effect of improving the tearing of the pole ear at the cell level, thereby improving the safety of the cell and reducing the pressure difference defect rate after the cell is assembled. Secondly, the distance range between the insulating reinforcement layer and the active material layer is the second preset range, that is, the two are arranged at intervals from each other and do not abut each other, so that the problem of mutual material between the slurry of the insulating reinforcement layer and the slurry of the active material layer can be effectively avoided, and the adsorption problem caused by the combination of the slurry of the active material layer and the slurry of the insulating reinforcement layer can be effectively avoided, thereby improving the electron transmission capacity of the lithium-ion battery.
[0018] In addition, the insulation reinforcement layer satisfies the formula: 450≤W*H2 / (H1) 2 ≤1100, and the thickness of the insulating reinforcement layer is less than that of the active material layer, thereby effectively avoiding the breakage problem caused by the step structure of the end ear and the extrusion stress generated by the step structure. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] One or more embodiments are exemplarily illustrated by the figures in the corresponding drawings. These exemplified descriptions do not constitute a limitation on the embodiments. Unless otherwise specified, the figures in the drawings do not constitute a scale limitation. In order to more clearly illustrate the embodiments of the present application or the technical solutions in the traditional technology, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0020] Figure 1 A cross-sectional view of an energy storage cell provided in one embodiment of the present application;
[0021] Figure 2 A top view of a positive electrode sheet in an energy storage cell provided in one embodiment of the present application;
[0022] Figure 3 for Figure 2 A cross-section along section A1-A2;
[0023] Figure 4 for Figure 2 Another cross-sectional view along the A1-A2 section;
[0024] Figure 5 for Figure 2Another cross-sectional view along the A1-A2 section. DETAILED DESCRIPTION
[0025] As can be seen from the background technology, the mechanical strength of the tabs of current energy storage cells is poor and they are easily torn.
[0026] An embodiment of the present application provides an energy storage battery cell, which increases the mechanical strength of the pole lug itself and avoids the problem of the pole lug being torn by providing an insulating reinforcement layer at the end of the pole lug.
[0027] In the description of the embodiments of the present application, the technical terms "first", "second", etc. are only used to distinguish different objects, and cannot be understood as indicating or implying relative importance or implicitly indicating the number, specific order or primary and secondary relationship of the indicated technical features. In the description of the embodiments of the present application, the meaning of "multiple" is more than two, unless otherwise clearly and specifically defined.
[0028] Reference to "embodiments" herein means that a particular feature, structure, or characteristic described in conjunction with the embodiments may be included in at least one embodiment of the present application. The appearance of the phrase in various locations in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described herein may be combined with other embodiments.
[0029] In the description of the embodiments of the present application, the term "and / or" is only a description of the association relationship of associated objects, indicating that three relationships may exist. For example, A and / or B can represent: A exists, A and B exist at the same time, and B exists. In addition, the character " / " in this article generally indicates that the associated objects before and after are in an "or" relationship.
[0030] In the description of the embodiments of the present application, the term "multiple" refers to more than two (including two). Similarly, "multiple groups" refers to more than two groups (including two groups), and "multiple pieces" refers to more than two pieces (including two pieces).
[0031] In the description of the embodiments of the present application, the technical terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise", "axial", "radial", "circumferential", etc. indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, which are only for the convenience of describing the embodiments of the present application and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the embodiments of the present application.
[0032] In the description of the embodiments of the present application, unless otherwise clearly specified and limited, technical terms such as "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense. For example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, and it can be the internal connection of two elements or the interaction relationship between two elements. For those of ordinary skill in the art, the specific meanings of the above terms in the embodiments of the present application can be understood according to the specific circumstances.
[0033] In the accompanying drawings corresponding to the embodiments of the present application, the thickness and area of the layer are magnified for better understanding and ease of description. When describing a component (such as a layer, film, region or substrate) on another component or on the surface of another component, the component can be "directly" located on the surface of another component, or there can be a third component between the two components. On the contrary, when describing a component on the surface of another component or when another component is formed or provided on the surface of a component, it means that there is no third component between the two components. In addition, when describing a component as "substantially" formed on another component, it means that the component is not formed on the entire surface (or front surface) of the other component, nor is it formed on a partial edge of the entire surface.
[0034] In the description of the embodiments of the present application, when a component "includes" another component, unless otherwise specified, other components are not excluded, and other components may be further included. In addition, when a component such as a layer, film, region, or plate is referred to as being "on / located on" another component, it may be "directly on" the other component (i.e., located on the surface of the other component with no other components between them), or another component may exist in between. In addition, when a component such as a layer, film, region, or plate is "directly located on" another component, or when a component such as a layer, film, region, or plate is located on the surface of another component, it means that no other components are located in between.
[0035] The terms used in the description of the various embodiments described herein are only used to describe specific embodiments and are not intended to be limiting. As used in the description of the various embodiments described and in the appended claims, "the part" is also intended to include plural forms unless the context clearly indicates otherwise. Among them, components include components such as layers, films, regions or plates. Thereby improving the yield of the battery cell.
[0036] The following will describe the various embodiments of the present application in detail with reference to the accompanying drawings. However, it will be appreciated by those skilled in the art that in the various embodiments of the present application, many technical details are provided in order to enable the reader to better understand the present application. However, even without these technical details and various changes and modifications based on the following embodiments, the technical solution claimed in the present application can be implemented.
[0037] Figure 1 A cross-sectional view of an energy storage cell provided in one embodiment of the present application; Figure 2 A top view of a positive electrode sheet in an energy storage cell provided in one embodiment of the present application; Figure 3 for Figure 2 A cross-section along section A1-A2; Figure 4 for Figure 2 Another cross-sectional view along the A1-A2 section; Figure 5 for Figure 2 Another cross-sectional view along the A1-A2 section.
[0038] It should be noted that in order to explain and distinguish the diaphragm, the positive electrode sheet and the negative electrode sheet, Figure 1 The dotted line indicates the separator, the thinner solid line indicates the negative electrode, and the thicker solid line indicates the positive electrode, but this does not represent the thickness relationship between the separator, the positive electrode, and the negative electrode. Figure 1 There are gaps between the middle diaphragm, the positive electrode sheet and the negative electrode sheet. This is to clearly indicate the winding correspondence between the diaphragm, the positive electrode sheet and the negative electrode sheet, but it does not mean that there must be a gap between the diaphragm and the positive electrode sheet or between the diaphragm and the negative electrode sheet. In other words, the diaphragm and the positive electrode sheet can contact each other, or the diaphragm and the negative electrode sheet can contact each other.
[0039] refer to Figure 1 and Figure 2 Some embodiments of the present application provide an energy storage cell. The energy storage cell includes a separator 3, and a positive electrode sheet 1 and a negative electrode sheet 2 located on both sides of the separator 3; the positive electrode sheet 1 includes: a current collector 10, the current collector 10 has a pole ear 110 arranged along a first direction Y and an active material portion 11.
[0040] The energy storage cell may further include an insulation reinforcement layer 120 , which is at least located at the electrode tab 110 and at the junction between the electrode tab 110 and the active material portion 11 . A first preset range L1 is defined along the first direction Y between the insulation reinforcement layer 120 and the end 101 of the electrode tab 110 .
[0041] The energy storage cell may further include an active material layer 130 . The active material layer 130 is located on the current collector 10 corresponding to the active material portion 11 . A second preset range L2 is defined along the first direction Y between the active material layer 130 and the insulation reinforcement layer 120 .
[0042] The thickness H1 of the insulating reinforcement layer 120 is less than or equal to the thickness H2 of the active material layer 130; wherein the insulating reinforcement layer 120 satisfies the formula: 450≤W*H2 / (H1) 2≤1100, W is the width of the insulating reinforcement layer 120 along the first direction Y, H1 is the thickness of the insulating reinforcement layer 120 , and H2 is the thickness of the active material layer 130 .
[0043] In the energy storage battery cell provided in the embodiment of the present application, an insulating reinforcement layer 120 is arranged on the current collector 10. The insulating reinforcement layer 120 is located on the pole ear 110 and at the junction of the pole ear 110 and the active material portion 11, that is, located at the end of the pole ear 110 close to the active material portion 11. In this way, the insulating reinforcement layer 120 can completely wrap the end of the pole ear 110 and the junction of the pole ear 110 and the active material portion 11. The setting of the insulating reinforcement layer 120 can enhance the mechanical strength of the current collector 10, that is, increase the mechanical properties of the pole ear 110, and show the effect of improving the tearing of the pole ear 110 at the battery cell level, thereby improving the safety of the battery cell and reducing the pressure difference defect rate after the battery cell is assembled. Secondly, the distance range between the insulating reinforcement layer 120 and the active material layer 130 is a second preset range L2, that is, the two are spaced apart from each other and do not abut each other. In this way, the problem of cross-contamination between the slurry of the insulating reinforcement layer 120 and the slurry of the active material layer 130 can be effectively avoided, and the adsorption problem caused by the combination of the slurry of the active material layer 130 and the slurry of the insulating reinforcement layer 120 can be effectively avoided, thereby improving the electron transmission capacity of the lithium-ion battery.
[0044] In addition, the insulating reinforcement layer 120 satisfies the formula: 450≤W*H2 / (H1) 2 ≤1100, and the thickness of the insulating reinforcement layer 120 is less than the thickness of the active material layer 130, thereby effectively avoiding the breakage problem caused by the step structure of the end ear 110 and the extrusion stress generated by the step structure. According to the appearance classification, the energy storage battery cell can be divided into a square battery cell, a round battery cell or a soft pack battery cell. According to the capacity classification, the energy storage battery cell can be divided into 50Ah, 100Ah, 150Ah, 200Ah, 280Ah, 306Ah, 314Ah, 500+Ah, 800+Ah and 1000+Ah and other models. According to the chemical composition and working principle of the battery cell, the energy storage battery cell can be a lithium-ion battery, a lead-acid battery, a sodium-ion battery or a nickel-hydrogen battery. The embodiment of the present application takes a lithium-ion battery as an example. Those skilled in the art can replace the lithium ions in the positive electrode sheet, the negative electrode sheet and the electrolyte with corresponding metal ions according to actual needs. For example, in sodium ion batteries, the lithium transition metal oxide of the positive electrode active material is replaced by any of the corresponding layered metal oxides (such as NaFeO2), polyanion compounds (NaFePO4) and Prussian blue compound systems (such as NaMnFe(CN)6-zH2O), and the electrolyte is replaced by any of the organic liquid electrolyte, solid composite electrolyte or solid electrolyte.
[0045] The separator 3 can be located between the positive electrode sheet 1 and the negative electrode sheet 2 to prevent the short circuit problem caused by the physical contact between the positive electrode sheet 1 and the negative electrode sheet 2, while allowing ions to be conducted through the electrolyte and hindering the transmission of electrons, so that ions and electrons form a circuit during the charge and discharge process of the battery.
[0046] The diaphragm 3 can be any one of a microporous membrane, a modified microporous membrane, a non-woven membrane and a composite membrane. A microporous membrane is a membrane with a pore size in the micrometer range, mainly including polyolefin microporous membranes and other polymer microporous membranes. A modified microporous membrane is a membrane obtained by modifying a microporous membrane. Common modification methods include surface treatment, chemical grafting, surface coating, etc. Non-woven membranes have a small fiber diameter and generally show a higher porosity than other types of membranes. Composite membranes are prepared by coating or filling inorganic materials in microporous membranes or non-woven membranes, and have higher thermal stability and electrolyte wettability than other types of membranes.
[0047] In some embodiments, the diaphragm 3 may be coated with a polyvinylidene fluoride (PVDF) material so that the diaphragm 3 has excellent adhesion and flexibility. Since the diaphragm 3 has excellent adhesion, the diaphragm 3 and the positive electrode sheet 1 or the diaphragm 3 and the negative electrode sheet 2 can have good contact performance, thereby reducing the assembly time of the energy storage battery cell, thereby effectively reducing the overall production cost of the energy storage battery cell. Since the diaphragm 3 has excellent flexibility, the strength of the diaphragm 3 is improved, which is conducive to effectively improving the impact resistance of the diaphragm 3.
[0048] The positive electrode sheet 1 and the negative electrode sheet 2 serve as the positive electrode and negative electrode of the energy storage cell respectively. The positive electrode is the electrode plate where oxidation reaction occurs in the energy storage cell, and the negative electrode is the electrode plate where reduction reaction occurs in the energy storage cell. The positive electrode and the negative electrode are isolated and connected together by an electrolyte. The positive electrode and the negative electrode serve as the electrochemical reaction area of the energy storage cell.
[0049] In some embodiments, the current collector 10 of the positive electrode sheet 1 can be aluminum foil, which is cheaper than copper foil. A dense oxide film is formed on the surface of the aluminum foil, and the oxide film is very thin, which can improve the corrosion resistance of the aluminum foil, and electrons can achieve conductivity through the tunnel effect.
[0050] In some embodiments, the current collector of the positive electrode sheet 1 may also be a composite current collector, which includes three stacked layers, the middle layer is organic, and the upper and lower layers are copper-plated and aluminum-plated. The organic material is PET (polyethylene terephthalate), PP (polypropylene), PI (polyimide), etc.
[0051] It is understandable that in other embodiments, for example, the current collector of the positive electrode sheet 1 in a sodium ion battery may also be aluminum foil.
[0052] In some embodiments, the tab 110 is a metal conductor that leads the positive electrode of the energy storage cell out of the cell. The tab 110 is the contact point between the positive electrode and the external contact component when the cell is charged and discharged. The external contact component can be a pole.
[0053] When the electrode tab is welded, that is, the electrode tab is welded to the adapter, the electrode tab 110 needs to be assisted in welding by making the welding surface perpendicular to the extension direction of the positive electrode sheet. During this process, the deformation degree of the electrode tab is large and welding stress exists, which makes the electrode tab prone to tearing. In the positive electrode sheet provided in the embodiment of the present application, the insulation reinforcement layer is arranged on the electrode tab and at the junction of the electrode tab and the active material part. The mechanical strength of the insulation reinforcement layer 120 is relatively high, which can enhance the mechanical strength of the electrode tab 110 and effectively avoid the problem of the electrode tab 110 tearing during the welding process.
[0054] In some embodiments, the insulation reinforcement layer 120 may be composed of polyimide (PI) particles and ceramic particles. Compared with the insulation reinforcement layer composed of ordinary ceramic particles, the polyimide particles serve as a polymer matrix, and the ceramic particles are dispersed in the polymer matrix. The polymer matrix plays a role of buffering and absorbing energy between the ceramic particles, which is conducive to improving the toughness and fracture resistance of the insulation reinforcement layer 120.
[0055] In addition, polyimide particles are used as insulating materials and adhesives. The high insulation of polyimide material as an insulating material allows the insulating reinforcement layer to act as an isolation layer, which can avoid the short circuit problem caused by the contact between the positive electrode sheet 1 and the negative electrode sheet 2, and further avoid the leakage current problem caused by the short circuit between the positive electrode sheet 1 and the negative electrode sheet 2. Polyimide particles as an adhesive have strong heat resistance, thermal oxidation resistance and high peel strength, so that the insulating reinforcement layer 200 has high adhesion.
[0056] In some embodiments, the polyimide particles may be any one or more of poly(pyromelliticimide) (PMMI) material, polyetherimide (PEI) material, or polyamide-imide (PAI) material.
[0057] In some embodiments, the ceramic particles are any one or more of oxides (such as aluminum oxide, zirconium oxide), carbides (such as silicon carbide, boron carbide), and nitrides (such as silicon nitride).
[0058] In other embodiments, the insulating reinforcement layer 120 may also be composed of a polyimide material and a polyvinylidene fluoride material. The polyimide material is used as an insulating material and an adhesive, and the polyvinylidene fluoride material is also used as an insulating material and an adhesive. Among them, the polyimide material has good flexibility, adhesion and insulation. The polyvinylidene fluoride material also has high adhesion and flexibility. The dual flexibility based on the polyimide material and the polyvinylidene fluoride material can improve the mechanical strength of the tab 110.
[0059] In some embodiments, the insulating reinforcement layer satisfies the formula: 240≤W*H2 / (H1) 2 ≤9000, wherein the width W of the insulating reinforcement layer 120 along the first direction Y is 5 mm to 20 mm, the thickness H1 of the insulating reinforcement layer 120 is 20 μm to 50 μm, and the thickness H2 of the active material layer 130 is 120 μm to 180 μm.
[0060] Furthermore, the insulation reinforcement layer satisfies the formula: 450≤W*H2 / (H1) 2 ≤1100, wherein the width W of the insulating reinforcement layer 120 along the first direction Y is 5 mm to 7 mm, and the thickness H1 of the insulating reinforcement layer 120 is 32 μm to 40 μm. The thickness H2 of the active material layer 130 is 145 μm to 150 μm. In some embodiments, reference Figure 3 , a width W of the insulating reinforcement layer 120 along the first direction Y is 5 mm to 7 mm.
[0061] The first direction is the arrangement direction between the electrode tab 110 and the active material portion 11 .
[0062] In some embodiments, reference Figure 3 The thickness H1 of the insulating reinforcement layer 120 is 32 μm to 40 μm. The thickness H2 of the active material layer 130 is 145 μm to 150 μm.
[0063] In one example, the width W of the insulating reinforcement layer 120 is 5 mm, the thickness H1 of the insulating reinforcement layer 120 is 32 μm, the thickness H2 of the active material layer 130 is 145 μm, and the relationship between the three satisfies 450≤W*H2 / (H1) 2 ≤1100. In another example, the width W of the insulating reinforcement layer 120 is 6 mm, the thickness H1 of the insulating reinforcement layer 120 is 38 μm, the thickness H2 of the active material layer 130 is 150 μm, and the relationship between the three satisfies 450≤W*H2 / (H1) 2 ≤1100.
[0064] In some embodiments, reference Figure 3The insulating reinforcement layer 120 may also extend to the current collector 10 corresponding to the active material portion 11, wherein the width L3 of the insulating reinforcement layer 120 extending to the active material portion 11 along the first direction Y is less than or equal to 5 mm. L3 may be 0 mm, 1 mm, 2 mm, 3 mm, 4 mm or 5 mm.
[0065] In some embodiments, the first preset range L1 is 6 mm to 20 mm. The first preset range L1 can be 6 mm, 8 mm, 10 mm, 13 mm, 15 mm or 20 mm.
[0066] In other embodiments, the insulating reinforcement layer 120 may also be located at the junction of the electrode tab and the active material portion, that is, the insulating reinforcement layer does not extend to the region corresponding to the active material portion 11 .
[0067] In some embodiments, the second preset range L2 may be 0.5 mm to 1.5 mm. The active material layer 130 and the materials in the insulating reinforcement layer 120 will not agglomerate, and the particles of the active material layer 130 are stably connected as transmission links, establishing a good ion transmission channel and conductive network, thereby improving the electrochemical performance of the electrode.
[0068] The active material layer 130 may be composed of a positive electrode active material, a conductive agent, and a binder.
[0069] The positive electrode active material may be lithium cobalt oxide, lithium iron phosphate or lithium manganese oxide.
[0070] The conductive agent collects microcurrent between active materials and between active materials and current collector 10 to reduce the contact resistance of the electrode. The conductive agent may include traditional conductive agents (such as carbon black, conductive graphite, and carbon fiber, etc.) and new conductive agents (such as carbon nanotubes, graphene, and mixed conductive slurries thereof, etc.).
[0071] The main function of the adhesive is to ensure that the active material particles and the active particles have a certain bonding strength with the current collector 10 during the use of the battery, and is conducive to the formation of the SEI (Solid Electrolyte Interphase) film. The adhesive can be an oily adhesive, such as PVDF; or an aqueous adhesive, such as natural cellulose.
[0072] In some embodiments, reference Figure 4 The positive electrode sheet 1 may further include a conductive carbon layer 103, which is located between the current collector 10 and the active material layer 130. The conductive carbon layer 103 is attached to the current collector 10 to prevent the electrolyte from corroding the metal current collector 10, and the conductive carbon layer 103 itself has a low resistivity, so that excessive electrical loss will not be generated.
[0073] The conductive carbon layer 103 may be made of flake graphite, spherical graphite, small-sized active particles, carbon nanotubes, graphene, etc. 2 / g) compared to flake graphite (specific surface area of 16m 2 / g) provides a larger surface area for contacting with the lithium ion particles in the active material layer 130, and the corresponding positive electrode exhibits a more excellent cyclic voltammetric characteristic and has better dispersibility in the slurry. Using active particles or carbon nanotubes, graphene, etc. with small particle sizes or even nanometer sizes as the conductive carbon layer can significantly improve the energy density, rate performance, etc. of the lithium ion battery.
[0074] In some embodiments, reference Figure 5 The conductive carbon layer 103 can be located on the surface of the current collector 10, and the conductive carbon layer 103 can also be located between the current collector 10 and the insulating reinforcement layer 120. The conductive carbon layer 103 can serve as a protective layer to effectively protect the current collector 10 to prevent corrosion of the metal current collector 10, thereby increasing the life of the current collector 10.
[0075] It should be noted that, in other embodiments, the conductive carbon layer can also be located on part of the current collector, such as in the area where the insulating reinforcement layer is located, the current collector area between the insulating reinforcement layer and the active material layer, and the area where the active material layer is located, for example, in the area where part of the active material layer is located.
[0076] The negative electrode sheet 2 includes a negative electrode current collector and a negative electrode active material layer, and the negative electrode active layer is located on the negative electrode current collector. A portion of the negative electrode current collector is cut into the shape of a tab and serves as a negative electrode tab.
[0077] The negative electrode current collector may be copper foil, which has low electrical conductivity and can have high electron transmission capacity, and copper foil has weak lithium insertion capacity and captures fewer lithium ions, thereby effectively reducing the loss of lithium ions. In other embodiments, the negative electrode current collector may also be a foam copper current collector, a copper mesh current collector, and a three-dimensional nano copper array current collector.
[0078] In some embodiments, the negative electrode active material layer may be composed of a negative electrode active material, a conductive agent, and a binder. The negative electrode active material may be carbon material and non-carbon material: carbon-based materials include graphite materials (natural graphite, artificial graphite, and mesophase carbon spheres) and other carbon-based materials (hard carbon, soft carbon, and graphene); non-carbon-based materials may be subdivided into titanium-based materials, silicon-based materials, tin-based materials, nitrides, and metallic lithium, etc.
[0079] The conductive agent is similar to that of the positive electrode active material layer, and the adhesive for the negative electrode is similar to that for the positive electrode, mainly including oil-based PVDF, water-based CMC, PAMAC, polyvinyl alcohol (PVA), sodium alginate, etc., which will not be repeated here.
[0080] The energy storage cell may further include a shell, and the whole formed by winding the positive electrode sheet 1, the negative electrode sheet 2 and the separator 3 is located in a chamber formed by the shell, and the chamber is also filled with electrolyte.
[0081] The electrolyte is a carrier that conducts electrons between the positive and negative electrodes in the battery. In some embodiments, the electrolyte can be an electrolyte, which consists of three parts: a solvent, a lithium salt, and an additive. The solvent is used to dissolve the lithium salt, and the solvent may include cyclic carbonates (PC, EC); chain carbonates (DEC, DMC, EMC); carboxylates (MF, MA, EA, MA, MP, etc.). The lithium salt may be LiPF6, LiClO4, LiBF4, LiAsF6, etc. The additive may be a film-forming additive, a conductive additive, a flame retardant additive, an overcharge protection additive, an additive for controlling the content of H2O and HF in the electrolyte, an additive for improving low temperature performance, and a multifunctional additive. One or more.
[0082] In some embodiments, the energy storage cell may further include a top cover, a transfer plate, and a pole. The top cover is engaged with the housing. The transfer plate is located in the chamber and is electrically connected to the pole lug 110. The pole passes through the top cover, and one end of the pole is electrically connected to the transfer plate.
[0083] Among them, the adapter plate includes at least a first adapter plate and a second adapter plate, the pole includes a positive pole pole and a negative pole pole, the first adapter plate is electrically connected to the pole ear 110 of the positive pole plate 1 and the positive pole pole respectively, and the second adapter plate is electrically connected to the negative pole ear and the negative pole pole of the negative pole plate 2 respectively.
[0084] The beneficial effects of the embodiments of the present application will be further illustrated below in combination with embodiments and comparative examples.
[0085] Embodiment 1: The energy storage cell includes: a diaphragm, and a positive electrode sheet and a negative electrode sheet located on both sides of the diaphragm. The positive electrode sheet includes: a current collector, an insulating reinforcement layer, and an active material layer. The insulating reinforcement layer is at least located at the junction between the pole ear and the pole ear and the active material part, and the insulation reinforcement layer and the end of the pole ear are spaced 6mm along the first direction; the active material layer is located on the current collector corresponding to the active material part, and the distance between the active material layer and the insulating reinforcement layer along the first direction is 0.6mm; the width W of the insulating reinforcement layer along the first direction is 5mm, the thickness H1 of the insulating reinforcement layer is 32μm, and the thickness H2 of the active material layer is 145μm.
[0086] Embodiment 2: The difference from Embodiment 1 is that the distance between the active material layer and the insulating reinforcement layer along the first direction is 1 mm.
[0087] Embodiment 3 is different from Embodiment 1 in that the distance between the active material layer and the insulating reinforcement layer along the first direction is 1.4 mm.
[0088] Example 4: The difference from Example 1 is that the width of the insulation reinforcement layer along the first direction is 6 mm, the thickness H1 of the insulation reinforcement layer is 38 μm, and the thickness H2 of the active material layer is 150 μm.
[0089] Comparative Example 1: The difference from Example 1 is that the distance between the active material layer and the insulating reinforcement layer along the first direction is 0.
[0090] Comparative Example 2: The difference from Comparative Example 1 is that the distance between the active material layer and the insulating reinforcement layer along the first direction is 3 mm.
[0091] Comparative Example 3 is different from Example 1 in that: the width of the insulating reinforcement layer along the first direction is 6 mm, the thickness H1 of the insulating reinforcement layer 120 is 138 μm, and the thickness H2 of the active material layer 130 is 150 μm.
[0092] Comparative Example 4 is different from Example 1 in that: the width of the insulating reinforcement layer along the first direction is 6 mm, the thickness H1 of the insulating reinforcement layer 120 is 200 μm, and the thickness H2 of the active material layer 130 is 150 μm.
[0093] Comparative Example 5: The difference from Example 1 is that no insulating reinforcement layer is provided.
[0094] The above-mentioned embodiments and comparative examples were subjected to cross-linking test, tearing test and electrochemical test in turn, and the test results were summarized and recorded in Table 1. The cross-linking test is used to characterize whether there is a cross-linking problem between the insulation reinforcement layer and the active material layer, and the tearing test is used to characterize whether the tab has a tearing problem; the electrochemical test is used to characterize the size relationship of the battery capacity of the formed energy storage cell under a fixed rate and a fixed volume.
[0095] The cross-link test includes: using a scanning electron microscope (SEM) to magnify the structure of the connection between the insulating reinforcement layer and the active material layer, and observe whether the two are in contact and whether the particles of the two are mixed. If the two are in contact with each other or the particles of the two are mixed, it is considered that there is cross-link. If not, it is considered that there is no cross-link.
[0096] The tear test includes: bending the positive electrode sheet including the tab along the arrangement direction of the tab and the active material part, with a bending angle of 60° to 120°. After bending 10 times, the surface condition of the end of the tab is observed under a microscope. If there are torn gaps or even damage on the surface of the tab, it is considered to have a tear probability, and the tear probability is judged based on the surface condition; if there is no trace, it is considered to have no tear probability.
[0097] The electrochemical test includes: the weight of the energy storage cell of each embodiment is a fixed value, i.e. 25g. The cell is fully charged at room temperature (25°C), and then discharged at a rate of 1C to a cut-off voltage (2.5V) after being fully left in the tested environment, and the released capacity (energy) is recorded. In actual experiments, the test can be repeated three times in a row and the average value can be taken to improve accuracy. The energy density is calculated, which is the battery energy given by the battery per unit mass.
[0098] Table 1
[0099]
[0100]
[0101] From the comparison of the above embodiments and comparative example 5, it can be seen that the provision of an insulating reinforcement layer can enhance the mechanical strength of the tab and avoid the tab tearing problem. From the comparison of embodiments 1-3 and comparative examples 1-2, it can be seen that separating the insulating reinforcement layer from the active material layer and controlling the spacing distance can avoid the problem of cross-linking and improve the energy density of the energy storage cell. From the comparison of embodiments 1 and 4 and comparative examples 3-4, it can be seen that the thickness of the active material layer and the insulating reinforcement layer is within the above range, which can improve the energy density of the energy storage cell.
[0102] In the energy storage battery cell provided in the embodiment of the present application, an insulating reinforcement layer 120 is arranged on the current collector 10. The insulating reinforcement layer 120 is located on the pole ear 110 and at the junction of the pole ear 110 and the active material portion 11, that is, located at the end of the pole ear 110 close to the active material portion 11. In this way, the insulating reinforcement layer 120 can completely wrap the end of the pole ear 110 and the junction of the pole ear 110 and the active material portion 11. The setting of the insulating reinforcement layer 120 can enhance the mechanical strength of the current collector 10, that is, increase the mechanical properties of the pole ear 110, and show the effect of improving the tearing of the pole ear 110 at the battery cell level, thereby improving the safety of the battery cell and reducing the pressure difference defect rate after the battery cell is assembled. Secondly, the distance range between the insulating reinforcement layer 120 and the active material layer 130 is a second preset range, that is, the two are spaced apart from each other and do not abut each other. In this way, the problem of cross-contamination between the slurry of the insulating reinforcement layer 120 and the slurry of the active material layer 130 can be effectively avoided, and the adsorption problem caused by the combination of the slurry of the active material layer 130 and the slurry of the insulating reinforcement layer 120 can be effectively avoided, thereby improving the electron transmission capacity of the lithium-ion battery.
[0103] Accordingly, according to some embodiments of the present application, the embodiments of the present application also provide a method for preparing an energy storage cell, which is used to prepare the energy storage cell provided by the above embodiments. The technical features that are the same as or corresponding to the above embodiments will not be described in detail here.
[0104] The preparation method comprises: preparing a positive electrode sheet 1.
[0105] In some embodiments, the process steps of preparing the positive electrode sheet 1 may include: providing a current collector 10 , wherein the current collector 10 has two electrode lugs 12 and an active material portion 11 located between the two electrode lugs 12 .
[0106] In some embodiments, the current collector 10 may be an aluminum current collector or a carbon-based current collector. The carbon-based current collector 10 refers to an aluminum current collector 10 with a conductive carbon layer 103 coated on its surface.
[0107] The carbon-based current collector 10 includes two types. The first type is that the current collector 10 corresponding to the active material part 11 is coated with a conductive carbon layer 103, and then formed as follows Figure 4 The second type is that the entire current collector 10 is coated with a conductive carbon layer 103, and then formed as shown. Figure 5 The positive electrode sheet 1 is shown.
[0108] In some embodiments, the step of forming the positive electrode sheet 1 includes: forming an insulating reinforcement layer 120, the insulating reinforcement layer 120 is at least located at the pole ear portion 12 and the junction between the pole ear portion 12 and the active material portion 11, and there is a first preset range L1 along the first direction Y between the insulating reinforcement layer 120 and the end of the pole ear portion 12.
[0109] In some embodiments, the process steps for forming the insulating reinforcement layer 120 include: mixing the polyimide material and ceramic particles evenly to form a mixed slurry; wherein the mass percentage of the ceramic particles is 80wt% to 95wt%, and the mass percentage of the polyimide material is 5wt% to 20wt%; coating the mixed slurry on the current collector 10, and drying to form the insulating reinforcement layer 120.
[0110] In some embodiments, the process steps for forming the insulating reinforcement layer 120 include: mixing the polyimide material and the polyvinylidene fluoride material evenly to form a mixed slurry; wherein the mass percentage of the polyimide material is 80wt% to 95wt%, and the mass percentage of the polyvinylidene fluoride material is 5wt% to 20wt%; coating the mixed slurry on the current collector 10 and drying to form the insulating reinforcement layer 120.
[0111] In some embodiments, the insulating reinforcement layer 120 is formed by a dispensing process. The dispensing process refers to applying, encapsulating or dripping the liquid or solid solution composed of the source material onto the product, so that the surface of the product can be adhered, encapsulated, insulated, fixed or smooth. In this way, the amount of dispensing and the dispensing position can be controlled, and then a uniform and smooth insulating reinforcement layer 120 can be achieved in a smaller area, thereby improving the problem of a narrow coating size window of the insulating reinforcement layer 120. Secondly, the dispensing process has a high precision, which can effectively control the first preset distance between the final insulating reinforcement layer 120 and the end of the tab 110 and the second preset range between the insulating reinforcement layer 120 and the active material layer 130, thereby improving the yield of the battery cell.
[0112] In some embodiments, the step of forming the positive electrode sheet 1 includes: forming an active material layer 130, the active material layer 130 is located on the current collector 10 corresponding to the active material part 11, and there is a second preset range between the active material layer 130 and the insulating reinforcement layer 120 along the first direction; the thickness of the insulating reinforcement layer 120 is less than or equal to the thickness of the active material layer 130; wherein the insulating reinforcement layer 120 satisfies the formula: 450≤W*H2 / (H1) 2 ≤1100, W is the width of the insulating reinforcement layer 120 along the first direction, H1 is the thickness of the insulating reinforcement layer 120, H2 is the thickness of the active material layer 130, and the first direction is the arrangement direction of the electrode ear portion 12 and the active material portion 11.
[0113] In some embodiments, the process steps for forming the active material layer 130 include: dissolving 85 wt% to 95 wt% of the positive electrode active material, 5 wt% to 10 wt% of the conductive agent and 2 wt% to 10 wt% of the binder in N-methylpyrrolidone solvent according to the mass ratio, stirring for 10 h to 15 h under the conditions of vacuum degree of -0.07 Mpa to -0.08 Mpa and stirring speed of 1000 rpm to 3500 rpm to obtain a mixture, sieving the mixture, controlling the mesh specification to 160 mesh, and filtering the mixture through the secondary stage to prepare the positive electrode slurry, coating the positive electrode slurry on the current collector 10, and drying to form the active material layer 130. During the mixing process, the temperature of the slurry is controlled not to be higher than 40°C, and the discharge temperature is controlled at 23 ± 5°C. Coating on the current collector 10 of 15 μm to 20 μm at a coating rate of 5 m / min to 8 m / min.
[0114] In some embodiments, the step of forming the positive electrode sheet 1 also includes: die-cutting the current collector 10 corresponding to the pole ear portion 12 according to preset parameters so that the pole ear portion 12 of the current collector 10 forms a pole ear 110; cutting the current collector 10 to form two identical positive electrode sheets 1.
[0115] In some embodiments, the method for preparing the energy storage cell further includes: providing a separator 3 and a negative electrode sheet 2, wherein the separator 3 is located between the positive electrode sheet 1 and the negative electrode sheet 2, and winding the separator 3, the positive electrode sheet 1 and the negative electrode sheet 2.
[0116] In some embodiments, the process steps for forming the negative electrode sheet 2 are: providing a negative electrode current collector; preparing a negative electrode slurry, and coating the negative electrode slurry on a negative electrode current collector of 15 μm to 20 μm at a speed of 5 m / min to 8 m / min, and die-cutting a portion of the negative electrode current collector according to preset parameters to form a negative electrode tab 110 at the end of the current collector 10; cutting the current collector 10 to form two identical negative electrode sheets 2.
[0117] In some embodiments, the preparation step of the negative electrode slurry includes: dissolving 85wt% to 95wt% of the negative electrode active material, 5wt% to 10wt% of the conductive agent and 2wt% to 10wt% of the binder in N-methylpyrrolidone solvent according to the mass ratio, stirring for 12h to 18h under the conditions of vacuum degree of -0.07Mpa to -0.08Mpa and stirring speed of 1000rpm to 3000rpm to obtain a mixture, sieving the mixture, controlling the mesh specification to 100 mesh, and filtering it through secondary filtering to prepare the negative electrode slurry.
[0118] In some embodiments, the winding process is to wind the separator 3, the positive electrode sheet 1, and the negative electrode sheet 2 into a single winding core by a winding machine. The order is to use the negative electrode sheet 2 to wrap the positive electrode sheet 1, and then separate the positive electrode sheet 1 and the negative electrode sheet 2 by the separator 3.
[0119] In some embodiments, a small winding tension will affect the internal resistance and shell penetration rate; excessive tension can easily cause short circuit or fragmentation risks. Therefore, the winding tension is generally between 0.08 and 0.15 MPa for positive tension, 0.08 and 0.15 MPa for negative tension, 0.08 and 0.15 MPa for upper diaphragm tension, and 0.08 and 0.15 MPa for lower diaphragm tension. The width of the negative electrode sheet 2, the width of the positive electrode sheet 1, and the width of the diaphragm 3 are not the same. For example, the width of the negative electrode sheet is 59.5 mm, the width of the positive electrode sheet is 58 mm, and the width of the diaphragm is 61 mm. The three are aligned in the center to improve the alignment of the electrode sheets and avoid the risk of short circuit. The electrode sheet alignment refers to the relative positions of the positive electrode sheet 1, the negative electrode sheet 2, and the diaphragm 3.
[0120] The beneficial effects of the embodiments of the present application will be further illustrated below in combination with embodiments and comparative examples.
[0121] Embodiment 5: An insulating reinforcement layer is formed by using a dispensing process, wherein the materials of the insulating reinforcement layer are a polyimide material and a polyvinylidene fluoride material, wherein the mass percentage of the polyimide material is 90wt%, and the mass percentage of the polyvinylidene fluoride material is 10wt%.
[0122] Embodiment 6: An insulating reinforcement layer is formed by using a dispensing process, wherein the materials of the insulating reinforcement layer are polyimide material and ceramic particles, wherein the mass percentage of the polyimide material is 90wt%, and the mass percentage of the ceramic particles is 10wt%.
[0123] Comparative Example 1: An insulating layer is formed by using a dispensing process, wherein the insulating layer is made of polyvinylidene fluoride material and ceramic particles, wherein the mass percentage of the polyvinylidene fluoride material is 10wt%, and the mass percentage of the ceramic particles is 90wt%.
[0124] Comparative Example 2: An insulating reinforcement layer is formed by a gravure coating process. The materials of the insulating reinforcement layer are a polyimide material and a polyvinylidene fluoride material. The mass percentage of the polyimide material is 90 wt %, and the mass percentage of the polyvinylidene fluoride material is 10 wt %.
[0125] Comparative Example 3: The insulating reinforcement layer is formed by a non-contact spray glue dripping process, and the materials of the insulating reinforcement layer are polyimide material and polyvinylidene fluoride material, wherein the mass percentage of the polyimide material is 90wt%, and the mass percentage of the polyvinylidene fluoride material is 10wt%.
[0126] The tearing test and accuracy test were performed on the above embodiments and comparative examples in turn, and the test results were summarized and recorded in Table 2. The accuracy of the insulation reinforcement layer is used to indicate whether the size of the insulation reinforcement layer deviates from the preset value and the preset position.
[0127] The accuracy test includes: setting the position and size of the insulation reinforcement layer, where the position is based on the end of the pole ear as a reference, and the size is based on the length of the pole ear and the arrangement direction of the active material part, and the preset size is set to 10mm. Based on the position and actual size of the insulation reinforcement layer observed under a microscope, verify whether the insulation reinforcement layer is deviated, and judge the accuracy of the insulation reinforcement layer according to the magnitude of the deviation.
[0128] Table 2
[0129] project Probability of tab tearing / % Accuracy of insulation reinforcement layer / % Example 5 0.03 92 Example 6 0.04 92 Comparative Example 6 15 92 Comparative Example 7 0.03 81 Comparative Example 8 0.03 85
[0130] From the comparison between the above-mentioned Examples 5-6 and Comparative Example 6, it can be seen that adding polyimide to the insulation reinforcement layer can improve the mechanical strength of the insulation reinforcement layer, thereby increasing the mechanical strength of the tab and avoiding the tab tearing problem. From the comparison between Examples 5-6 and Comparative Examples 7-8, it can be seen that the use of the dispensing process can improve the accuracy of the insulation reinforcement layer finally formed, thereby controlling the spacing distance and avoiding the problem of cross-linking.
[0131] The preparation method of the energy storage battery provided in the embodiment of the present application is to separate the insulation reinforcement layer and the active material layer from each other before designing the positions of the insulation reinforcement layer and the active material layer, so as to avoid the problem of material cross-contamination between the slurries of the two. Then, the preparation process of the insulation reinforcement layer adopts a dispensing process, which is easy to operate and precisely controlled based on the dispensing process, so as to avoid the problem of material cross-contamination caused by the slurry of the insulation reinforcement layer exceeding the gap between the insulation reinforcement layer and the active material layer.
[0132] Those skilled in the art will appreciate that the above-mentioned embodiments are specific examples for implementing the present application, and in practical applications, various changes may be made to the embodiments in form and detail without departing from the spirit and scope of the present application. Any person skilled in the art may make various changes and modifications without departing from the spirit and scope of the present application, and therefore the scope of protection of the present application shall be subject to the scope defined in the claims.
Claims
1. An energy storage battery cell, characterized in that: include: A diaphragm, and a positive electrode sheet and a negative electrode sheet located on both sides of the diaphragm; The positive electrode sheet comprises: A current collector, wherein the current collector has a tab and an active material portion arranged along a first direction; an insulating reinforcement layer, the insulating reinforcement layer being at least located at the electrode tab and at a junction between the electrode tab and the active material portion, and having a first preset range between the insulating reinforcement layer and an end of the electrode tab along the first direction; an active material layer, the active material layer being located on the current collector corresponding to the active material portion, and having a second preset range between the active material layer and the insulating reinforcement layer along the first direction; the thickness of the insulating reinforcement layer being less than or equal to the thickness of the active material layer; Wherein, the insulating reinforcement layer satisfies the formula: 450≤W*H2 / (H1) 2 ≤1100, W is the width of the insulation reinforcement layer along the first direction, H1 is the thickness of the insulation reinforcement layer, and H2 is the thickness of the active material layer.
2. The energy storage cell according to claim 1, characterized in that: The insulating reinforcement layer further extends to the current collector corresponding to the active material portion, wherein a width of the insulating reinforcement layer extending to the active material portion along the first direction is less than or equal to 5 mm.
3. The energy storage cell according to claim 1, characterized in that: The first preset range is 6 mm to 20 mm; the second preset range is 0.5 mm to 1.5 mm.
4. The energy storage cell according to claim 1, characterized in that: The positive electrode sheet further includes: a conductive carbon layer, wherein the conductive carbon layer is located between the current collector and the active material layer.
5. The energy storage cell according to claim 4, characterized in that: The conductive carbon layer is located on the surface of the current collector, and the conductive carbon layer is also located between the current collector and the insulating reinforcement layer.
6. The energy storage cell according to claim 1, characterized in that: The width of the insulation reinforcement layer along the first direction is 5 mm to 7 mm.
7. A method for preparing an energy storage battery cell, characterized in that: include: Providing a current collector, the current collector having two pole lug portions and an active material portion located between the two pole lug portions; forming an insulation reinforcement layer, wherein the insulation reinforcement layer is at least located at the pole ear portion and at the junction between the pole ear portion and the active material portion, and a first preset range is defined between the insulation reinforcement layer and the end of the pole ear portion along a first direction; An active material layer is formed, the active material layer is located on the current collector corresponding to the active material portion, and a second preset range is provided between the active material layer and the insulating reinforcement layer along the first direction; the thickness of the insulating reinforcement layer is less than or equal to the thickness of the active material layer; wherein the insulating reinforcement layer satisfies the formula: 450≤W*H2 / (H1) 2 ≤1100, W is the width of the insulation reinforcement layer along the first direction, H1 is the thickness of the insulation reinforcement layer, H2 is the thickness of the active material layer, and the first direction is the arrangement direction of the electrode ear portion and the active material portion; Die-cutting the current collector corresponding to the pole ear portion according to preset parameters so that the pole ear portion of the current collector forms a pole ear; Cutting the current collector to form two identical positive electrode sheets; A separator and a negative electrode sheet are provided, wherein the separator is located between the positive electrode sheet and the negative electrode sheet, and the separator, the positive electrode sheet and the negative electrode sheet are wound.
8. The method for preparing the energy storage battery cell according to claim 7, characterized in that: The insulating reinforcement layer is formed by using a dispensing process.
9. The method for preparing the energy storage battery cell according to claim 7 or 8, characterized in that: The process steps for forming the insulating reinforcement layer include: uniformly mixing the polyimide material and the ceramic particles to form a mixed slurry; wherein the mass percentage of the ceramic particles is 80wt% to 95wt%, and the mass percentage of the polyimide material is 5wt% to 20wt%; The mixed slurry is coated on the current collector and dried to form the insulation reinforcement layer.
10. The method for preparing the energy storage battery cell according to claim 7 or 8, characterized in that: The process steps for forming the insulating reinforcement layer include: mixing a polyimide material and a polyvinylidene fluoride material evenly to form a mixed slurry; wherein the mass percentage of the polyimide material is 80wt% to 95wt%, and the mass percentage of the polyvinylidene fluoride material is 5wt% to 20wt%; coating the mixed slurry on the current collector and drying to form the insulating reinforcement layer.
Citation Information
Cited By
Solid-state battery and manufacturing method of solid-state battery
CN119627183A