Cemented carbide powder for binder jet additive manufacturing

Through the dual sintering cycle process and binder jet technology, the high density of cemented carbide powder in additive layer manufacturing is solved, and efficient manufacturing of poreless 3D printed objects is achieved.

CN118984747APending Publication Date: 2024-11-19HYPERION MATERIALS TECH CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380033839.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-13
Filing Date
2023-03-01
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

In the field of additive layer manufacturing, it is difficult to obtain poreless 3D printed objects, especially high density problems of cemented carbide powder, which makes it difficult to achieve efficient sintering of adhesive spray technology.

Method used

By preparing a slurry composition of ceramic hard phase powder, metal bonded phase powder and organic binder, grinding and spray drying, followed by a double sintering cycle process to obtain a densified printable powder and using a binder Jet technology performs 3D printing.

Benefits of technology

The densification of high-density cemented carbide powder is achieved, ensuring the non-porous and high density of 3D printed objects, and improving the efficiency and effect of adhesive spraying technology.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

A method of manufacturing a three-dimensional (3D) object by forming a printable cemented carbide powder having a full density from a dual sintering cycle process is provided. The formed fully densified printable cemented carbide powder is then used in binder jet additive manufacturing to 3D print the object.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to a method of manufacturing three-dimensional (3D) objects by binder jetting additive manufacturing. Background Art

[0002] Additive layer manufacturing (ALM) generally encompasses a process in which digital 3-dimensional (3D) design data is used to 3D print physical articles or parts in a manner that forms successive layers through sequential deposition of materials and liquid binders, followed by processing. There is growing evidence that the ALM market is maturing rapidly, with a growing interest, in particular, from manufacturers to build physical objects and parts in a just-in-time manner. In fact, a variety of technology options have been developed that traditionally fall under the general category of ALM. In this regard as well, conventional 3D technologies can include, but are not limited to, technologies such as stereolithography that introduces UV lasers to cure photopolymers, inkjet printers that utilize UV ​​radiation to polymerize photomonomers and photooligomers, metal sintering (e.g., selective laser sintering and direct metal laser sintering), fused deposition modeling (FDM, an extrusion-based technology), and deposition of liquid binders on powders.

[0003] In the context of ALM, this 3D printing technology has become an attractive tool for manufacturing physical articles and parts in a variety of different fields such as: architecture, construction (AEC), industrial design, automotive, aerospace, military, engineering, dental and medical industries, biotechnology (e.g. human tissue replacement), fashion, footwear, jewelry, eyewear, education, geographic information systems, food and many other fields. A compelling motivation for adopting ALM is that it provides an effective and economical alternative to the traditional and more commonly used object making technology based solely on molding processes. With ALM, it is possible to avoid the considerable time and expense of mold and / or die construction and other tools. In fact, ALM technology provides advantageous material usage by allowing recycling in the process and avoiding the necessity of using mold lubricants and coolants. In short, ALM advantageously provides manufacturers with a full range of choices and freedom in the design of articles. Importantly, the effect is that objects with highly complex shapes can be manufactured by avoiding a lot of expenses, while being cumbersome.

[0004] In the platform of ALM technologies for 3D printing objects, binder jetting additive manufacturing, or simply binder jetting, is a next-generation technology that covers a well-defined ALM process. An industrial print head selectively deposits a liquid binder on a thin layer of powdered particles, which can be metal, sand, ceramic or composite materials. The process is repeated in sequence, so that successive layers are added by using a specially created map from a digital design file until the object is finally 3D printed and cured.

[0005] Thus, the liquid binder acts as an adhesive, much like a glue between multiple incremental, accumulated powdered layers. The binder is typically in liquid form, while the build material is in powder form. The print head moves horizontally along the x- and y-axes of the machine and deposits alternating layers of build material and liquid binder material in a sequential manner. After each successive layer, the object being 3D printed is lowered onto its build platform.

[0006] One inherently significant obstacle that is often faced is the inability to obtain a non-porous component after furnace sintering. Thus, for cemented carbide powders, there is a compromise between good and adequate flowability (i.e., the particles should ideally not sinter to each other) and producing a sufficiently high density that is typically required for binder jetting. Thus, this compromise must be considered when manufacturing cemented carbide powders for binder jetting purposes.

[0007] In view of the above, there is a need in the field of ALM for a method of manufacturing high-density cemented carbide for binder jetting to 3D print objects, which aims to solve the above problems. Summary of the invention

[0008] According to a first aspect, a method for manufacturing a three-dimensional (3D) object is provided, the method comprising: preparing a slurry composition comprising a ceramic hard phase powder, a metal binder phase powder and an organic binder in a grinding liquid. Next, the slurry composition is ground to obtain a slurry blend, and thereafter the slurry blend is spray dried to obtain an RTP powder. After screening the RTP powder, the RTP powder is then pre-sintered in a first cycle to obtain densification of the RTP powder. The pre-sintered RTP powder is then sintered in a second cycle to form a printable powder with enhanced densification. After screening the formed printable powder, the formed printable powder is subjected to a binder jet to 3D print a green body. Thereafter, the 3D printed green body is cured and sintered to ultimately form the 3D object.

[0009] Optionally, the RTP powder is free flowing.

[0010] Optionally, the pre-sintering in the first cycle is performed at a temperature starting at about 550°C and ending at about 1250°C.

[0011] Optionally, the pre-sintering in the first cycle is performed in an atmosphere of hydrogen pressure up to about 35 mbar, with an applied hydrogen flow of up to about 6000 liters / hour.

[0012] Optionally, the pre-sintering in the first cycle is performed for about 15 minutes to about 30 minutes.

[0013] Optionally, the pre-sintering in the first cycle is performed for about 30 minutes to about 45 minutes.

[0014] Optionally, the sintering in the second cycle is performed at a temperature starting at about 550°C and ending at about 1250°C.

[0015] Optionally, the sintering in the second cycle is performed in an atmosphere with an argon pressure of up to about 50 mbar, with an applied argon flow of up to about 300 1 / h.

[0016] Optionally, the sintering in the second cycle is performed for about 15 minutes to about 30 minutes.

[0017] Optionally, the sintering in the second cycle is performed for about 30 minutes to about 45 minutes.

[0018] Optionally, the yield of the printable powder formed is from about 60% to about 90%.

[0019] Optionally, the yield of the printable powder formed is from about 70% to about 90%.

[0020] Optionally, the yield of the printable powder formed is from about 80% to about 90%.

[0021] Optionally, the yield of the printable powder formed is from about 85% to about 90%.

[0022] Optionally, the yield of the printable powder formed is at least 90%.

[0023] Optionally, the RTP powder and the printable powder have an apparent density ranging from at least about 5 g / cm 3 About 15g / cm 3 within the range.

[0024] Optionally, the ceramic hard phase comprises one or more of the following substances: tungsten carbide (WC), titanium carbide (TiC), tantalum carbide (TaC), niobium carbide (NbC), vanadium carbide (VC), zirconium carbide (ZrC), molybdenum carbide (Mo2C) or hafnium carbide (HfC), or any combination thereof.

[0025] Optionally, the ceramic hard phase comprises WC.

[0026] Optionally, the metallic binder phase powder comprises cobalt.

[0027] Optionally, the RTP powder is sieved through a 4 mesh sieve, a 6 mesh sieve, an 8 mesh sieve, a 12 mesh sieve, a 16 mesh sieve, a 20 mesh sieve, a 30 mesh sieve, a 40 mesh sieve, a 50 mesh sieve, a 60 mesh sieve, a 70 mesh sieve, an 80 mesh sieve, a 100 mesh sieve, a 140 mesh sieve, or a 200 mesh sieve.

[0028] Optionally, the printable powder is sieved through a 4 mesh sieve, a 6 mesh sieve, an 8 mesh sieve, a 12 mesh sieve, a 16 mesh sieve, a 20 mesh sieve, a 30 mesh sieve, a 40 mesh sieve, a 50 mesh sieve, a 60 mesh sieve, a 70 mesh sieve, an 80 mesh sieve, a 100 mesh sieve, a 140 mesh sieve, a 200 mesh sieve, a 230 mesh sieve, a 270 mesh sieve, a 325 mesh sieve or a 400 mesh sieve.

[0029] Optionally, curing of the 3D printed green body is performed at a temperature starting at about 150°C and ending at about 180°C.

[0030] Optionally, curing of the 3D printed green body is performed at a temperature starting at about 180°C and ending at about 200°C.

[0031] Optionally, curing of the 3D printed green body is performed for up to about 6 hours.

[0032] Optionally, sintering of the solidified 3D printed green body is performed at a temperature starting from 1500°C and ending at about 1560°C.

[0033] Optionally, sintering of the solidified 3D printed green body is performed at a temperature starting from 1560°C and ending at about 1600°C.

[0034] Optionally, the printable powder is fully densified.

[0035] Other systems, methods, features and advantages will be or will become apparent to those skilled in the art upon reading the following drawings and detailed description. All such additional systems, methods, features and advantages are intended to be included in this specification, within the scope of the present disclosure, and protected by the appended claims. Nothing in this section should be construed as limiting these claims. Further aspects and advantages are discussed below in conjunction with the embodiments of the present disclosure. It should be understood that the foregoing general description and the following detailed description of the present disclosure are exemplary and illustrative, and are intended to provide further explanation of the disclosure claimed. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] The accompanying drawings, which are included to provide a further understanding of the subject matter and are incorporated in and constitute a part of this specification, illustrate embodiments of the subject matter and together with the description serve to explain the principles of the disclosure.

[0037] Figure 1 is a flow chart illustrating various process steps for making high density cemented carbide powder for binder jetting to 3D print objects according to an exemplary embodiment of the present subject matter. DETAILED DESCRIPTION

[0038] Unless defined otherwise, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which the presently described subject matter belongs.

[0039] Where a numerical range (e.g., a concentration range, a percentage range, or a ratio range) is provided, it is understood that each intervening value (to the nearest tenth of the unit of the lower limit unless the context clearly dictates otherwise) between the upper and lower limits of that range and any other stated value or intervening value in that stated range is encompassed within the subject matter. The upper and lower limits of these smaller ranges may independently be included in the smaller ranges, and such embodiments are also encompassed within the subject matter, subject to any specifically excluded limits in the stated range. Where the stated range includes one or both of the limits, ranges excluding one or both of those included limits are also encompassed within the described subject matter.

[0040] The following definitions set forth the parameters of the described subject matter.

[0041] As used in this disclosure, the term "Additive Layer Manufacturing (ALM)" refers to a process in which digital 3-dimensional (3D) design data is used to fabricate a physical article or part in the form of various successive layers through alternating and sequential powder material and liquid binder deposition and processing methods. With the recent convergence of breakthrough technologies for 3D printing objects, such as Fused Deposition Modeling (FDM) and Binder Jetting are examples of such next generation ALM processes. An industrial print head selectively deposits a liquid binder onto a thin layer of powdered particles, which can be metal, sand, ceramic, or a composite material. The process is repeated sequentially, such that successive layers are added using a specially created map from the digital design file until the object is finally 3D printed and solidified.

[0042] As used in the present disclosure, the term "RTP powder" refers herein to a ground and spray-dried compressible cemented carbide powder comprising: a mixture of a ceramic hard phase and a metallic binder phase comprising cobalt, with a particle size typically spanning from about 10 microns to about 250 microns. The RTP powder is densified after screening, and the densification is promoted by a first pre-sintering consolidation step. Then, a second sintering cycle process is subsequently performed to finally enhance and further densify the particle density of the cemented carbide powder to obtain a fully dense "printable powder". Therefore, the RTP powder is further densified by the second sintering cycle to form a fully densified printable powder. After screening, the fully densified printable powder formed is then used in binder jetting additive manufacturing to 3D print a green body.

[0043] As used in this disclosure, the term "curing" refers to a chemical or physical process that produces toughening or hardening through chain crosslinking. Curing may involve a chemical reaction such as polymerization, or a physical reaction such as evaporation, resulting in more stable chain crosslinks.

[0044] As used in this disclosure, the term "sintering" refers to a process in which heating under controlled pressure is performed to minimize the surface of a particle system, which is associated with the formation of bonds between adjacent particles or particles and the shrinkage of aggregated particles or particles. The compaction and formation of a dense mass is performed by heating the particles without melting them to the liquefaction point. The atoms in the particles diffuse across the boundaries of the particles, thereby fusing the particles together and producing a solid mass.

[0045] As used in this disclosure, the term "spherical" refers to a solid circular figure, every point on its surface is located equidistant from its center.

[0046] As used in the present disclosure, unless specifically stated otherwise, the term “wt %” refers to a given weight percentage based on the total weight of a high-density cemented carbide used for binder jetting additive manufacturing to 3D print an object.

[0047] As used in the present disclosure, the term "D50" refers to the particle size corresponding to 50% of the volume of the sampled particles being less than the D50 value and 50% of the volume of the sampled particles being greater than the D50 value. Similarly, the term "D90" refers to the particle size corresponding to 90% of the volume of the sampled particles being less than the D90 value and 10% of the volume of the sampled particles being greater than the D90 value. The term "D10" refers to the particle size corresponding to 10% of the volume of the sampled particles being less than the D10 value and 90% of the volume of the sampled particles being greater than the D10 value. The width of the particle size distribution can be calculated by measuring the span defined by the formula (D90-D10) / D50. The span gives an indication of how far the 10% and 90% points are apart relative to the midpoint.

[0048] To determine the average grain size from a given grain size distribution of a sintered microstructure, a person skilled in the art will readily be familiar with the ISO 4499-2:2008 standard. The ISO 4499-2:2008 standard provides guidance for measuring the grain size of hard metals by metallographic techniques using optical or electron microscopy. It is intended for sintered WC / Co hard metals containing primarily WC as the ceramic hard phase. It is also intended to measure grain size and distribution by the linear intercept technique.

[0049] To further supplement the ISO 4499-2:2008 standard, those skilled in the art will also be aware of the ASTM B390-92 (2006) standard, which is used to empirically visually compare and classify the apparent grain size and distribution of sintered tungsten carbides, which typically contain cobalt as a metal binder in the binder phase.

[0050] Cemented carbide grades can be classified based on grain size. Different types of grades have been defined for different materials as nano, ultrafine, submicron, fine, medium, medium coarse, coarse and ultra coarse. As used in the present disclosure, the term (I) "nanoscale" is defined as a material having a grain size of less than about 0.2 μm; (II) "ultrafine" is defined as a material having a grain size from about 0.2 μm to about 0.5 μm; (III) "submicron" is defined as a material having a grain size from about 0.5 μm to about 0.9 μm; (IV) "fine" is defined as a material having a grain size from about 1.0 μm to about 1.3 μm; (V) "intermediate" is defined as a material having a grain size from about 1.4 μm to about 2.0 μm; (VI) "intermediate-coarse" is defined as a material having a grain size from about 2.1 μm to about 3.4 μm; (VII) "coarse" is defined as a material having a grain size from about 3.5 μm to about 5.0 μm; and (VIII) "ultra-coarse" is defined as a material having a grain size greater than about 5.0 μm.

[0051] As used in the present disclosure, the term "hard alloy" generally refers to a metal matrix composite material consisting of the following substances: a ceramic hard phase is usually embedded and anchored in a matrix by a ductile metal binder element such as cobalt (i.e., a metal binder, thereby producing a metal binder phase). The ceramic hard phase and the metal binder phase powder can be processed into various microstructures that achieve different mechanical and physical properties. In addition, additional ingredients can be added to the composition to help control and improve the performance achieved by the hard alloy composition. By controlling various parameters, including grain size, cobalt content, doping (dotation) (e.g., alloy carbides) and carbon content, hard alloy manufacturers can advantageously adjust their performance for specific applications. Hard alloys are ideally designed to provide the physical best properties of ceramics such as high temperature resistance, hardness and fracture toughness and the physical best properties of metals such as the ability to withstand plastic deformation. The naturally ductile metal binder is used to offset the characteristic brittle behavior of the ceramic hard phase, thereby improving its hardness, fracture toughness and durability. The combination of good hardness and fracture toughness makes cemented carbide become the ideal candidate for application such as material processing, tool blade such as blade blank, structural component etc. that relates to a large amount of wear. The ceramic hard phase of cemented carbide is usually made of refractory carbide, boride, nitride or carbonitride or any desired combination of metal (such as but not limited to tungsten, titanium, niobium, tantalum, chromium, vanadium, molybdenum, zirconium, hafnium) from the 4th family, the 5th family and the 6th family of the periodic table. The ceramic hard phase can be present in the powder in the mode of any possible combination with the metal mentioned, and exists with inconsistent and incompatible weight with the target of this theme. In order to meet the qualification of the cemented carbide in the present disclosure, cemented carbide usually has the ceramic hard phase that is made of at least 60 weight % by gross weight based on the cemented carbide.

[0052] As used in the present disclosure, the term "about" refers to plus or minus 5% of the numerical value of the numbers used in the claims and the present disclosure. Therefore, "about" can be used to provide flexibility to numerical range endpoints, wherein a given value can be "above" or "below" the given value. Thus, for example, a value of 50% may be intended to encompass a range that may be defined by, for example, the following ranges: 47.5%-52.25%, 47.5%-52.5%, 47.75%-50%, 50%-52.5%, 48%-48.5%, 48%-48.75%, 48%-49%, 48%-49.5%, 48%-49.75%, 48%-50%, 48%-50.25%, 48%-50.5%, 48%-50.75%, 48%-51%, 48%-51.5%, 48%-51.75%, 48%-52%, 48%-52.25%, 48%-52. ... 52.5%, 48.25%-48.5%, 48.25%-48.75%, 48.25%-49%, 48.25%-49.5%, 48.25%-49.75%, 48.25%-50%, 48.25%-50.25%, 48.25%-50.5%, 48.25%-50.75%, 48.25%-51%, 48.25%-51.25%, 48.25%-51.5%, 48.25%-51.75%, 48.25%-52%, 48.25%-52.25%, 48.25%-52.5%, 48.5%-48.75%, 48.5%-49%, 48.5%-49.5%, 48.5%-49.75%, 48.5%-50%, 48.5%-50.25%, 48.5%-50.5%, 48.5%-50.75%, 48.5%-51%, 48.5%-51.25%, 48.5%-51.5%, 48.5%-51.75%, 48.5%-52%, 48.5%-52.25%, 48.5%-52.5%, 49%-49.25%, 49%-49.5%, 49%-49.75%, 49%-50%, 49%-50.25%, 49%-50.5% , 49%-50.75%, 49%-51%, 49%-51.25%, 49%-51.5%, 49%-51.75%, 49%-52%, 49%-52.25%, 49%-52.5%, 49.5%-49.75%, 49.5%-50%, 49.5%-50.25%, 49.5%-50.5%, 49.5%-50.75%, 49.5%-51%, 49.5%-51.5%, 49.5%-51.75%, 49.5%-52%, 49.5%-52.25%, 49.5%-52.5%, 49.75%-50%, 49.75%-50.25%, 49.75%-50.5%, 49.75%-50.75%, 49.75%-51%, 49.75%-51.25%, 49.75%-51.5%, 49.75%-51.75%, 49.75%-52%, 49.75%-52.25%, 49.75%-52.5%, 50%-50.25%, 50%-50.5%, 50%-50.75%, 50%-51%, 50%-51.25%, 50%-51.5%, 50%-52%, 50%-52.25%, 50%-52.5%, etc. .

[0053] As used in this disclosure, the term "green body" refers to a material in the form of a coherent powder or sheet before the material is physically sintered.

[0054] As used herein, "spherical" refers to grains having a substantially round shape.

[0055] Wherever used throughout this disclosure, the term "generally" has the meaning of "typically" or "closely" or "around or in the vicinity of."

[0056] As used herein, the term "substantially" refers to the complete or nearly complete extent or degree of an action, characteristic, performance, state, structure, item, or result.

[0057] As used herein, the term "apparent density" refers to the mass of a powder or cemented carbide particle per unit volume in bulk conditions, expressed in g / cm 3 Thus, the term "apparent density" refers to the bulk density of free-flowing powders and loosely packed powders of cemented carbide that exhibit pore spaces between free-flowing particles of cemented carbide. It is provided that any given value of "apparent density" requires that the particles of the cemented carbide powder are loosely packed and also in a free-flowing state. The apparent density of sintered hard particles can be determined using a Hall flowmeter funnel in accordance with the ASTM B212 standard test method for apparent density of free-flowing metal powders.

[0058] As used in this disclosure, the term "free-flowing" refers to a loosely packed cemented carbide powder that exhibits pore spaces between individual free-flowing particles of the cemented carbide powder without any physical restrictions or obstructions that inhibit the free-flowing ability of the particles of the cemented carbide powder.

[0059] As used in this disclosure, "high-density cemented carbide" is intended to encompass materials with an apparent density ranging from at least about 5 g / cm 3 to about 15 g / cm 3 range of cemented carbide powders.

[0060] Method for producing high density cemented carbide for binder jetting additive manufacturing

[0061] The present disclosure is based on the intention of manufacturing a high-density cemented carbide powder, which is mainly composed of a ceramic hard phase powder and a metal binder phase powder, for binder jetting to 3D print objects through a roughly double sintering cycle process. A first pre-sintering process step is first performed to impart densification to the RTP powder (i.e., composed of a mixture of ceramic hard phase powder and metal binder phase powder). Next, a second sintering process step is subsequently performed to impart enhanced densification, thereby ultimately obtaining a printable powder with full density, and wherein the particles of the cemented carbide powder are no longer sintered to each other. Thereafter, the fully densified printable powder obtained can be advantageously used for binder jetting to 3D print objects.

[0062] It is obvious to those skilled in the art that the desired particle size of the cemented carbide powder mixture consisting of a ceramic hard phase powder, a metal binder phase powder and an organic binder can be achieved by a first grinding operation of typically several hours (e.g., 8, 16, 32, 64 hours) under ambient conditions to obtain a slurry blend (i.e., in a ball mill, attritor or planetary mill, 25°C, 298.15 K and a pressure of 101.325 kPa). In some embodiments, instead of using a ball mill, attritor or planetary mill as a physical machine, ultrasonic mixing can be suitably selected as a blending method. Therefore, in this case, ultrasonic mixing uses acoustic energy to effectively process, for example, powders, pastes, liquids and combinations thereof at a breakthrough speed, quality and repeatability. Powders of almost any size, material properties or morphology can be mixed quickly and thoroughly using, for example, an acoustic mixer. Acoustic processing is typically several orders of magnitude faster than conventional techniques. Here, the acoustic mixer can, for example, use a 60 Hz motion, which then causes each particle to collide randomly with adjacent particles, change their paths, collide, and then collide again with other particles that behave in the same chaotic manner. The main purpose of the blending operation is to promote good metal binder distribution and good wettability between the components of the slurry blend. Subjecting the cemented carbide mixture consisting of ceramic hard phase powder, metal binder phase powder and organic binder to a grinding operation is the key to strengthening the physical integrity of the ground cemented carbide powder mixture, and in some cases is to deagglomerate tungsten carbide (WC) crystals. Acceptable metal binder distribution and good quality wettability are basic and necessary parameters for obtaining cemented carbide blends of outstanding physical quality. On the other hand, if the quality of the metal binder phase distribution and wettability is too poor, holes and cracks may be formed undesirably in the final sintered body, which is unfavorable to the manufactured cemented carbide.

[0063] It is obvious to those skilled in the art that grinding is carried out by first adding a grinding liquid into a powder material batch comprising ceramic hard phase powder, metal binding phase powder and an organic binder mixture to form a slurry composition. The grinding liquid can be water, alcohol (such as but not limited to ethanol, methanol, isopropanol, butanol, cyclohexanol), an organic solvent (similar to, for example, heptane, hexane, acetone or toluene), an alcohol mixture, a mixture of alcohol and a solvent or any combination thereof. The property of the slurry composition depends in particular on the amount of the grinding liquid added. Because the drying of the slurry composition requires energy, the amount of the grinding liquid used to obtain the slurry composition should ideally be minimized to keep low cost. However, it is necessary to add enough grinding liquids to realize a pumpable slurry composition, and to avoid system clogging. In addition, other compounds commonly known to those skilled in the art can be added to the slurry composition, such as dispersants, pH adjusting agents, etc. Non-limiting examples of organic binders can be polyethylene glycol (PEG), paraffin, polyvinyl alcohol (PVA), long chain fatty acids, waxes or any combination thereof, which are added to the slurry composition prior to grinding, typically in an amount of, for example, from 15% to 25% by volume of the total volume of the formed slurry composition (i.e., the total volume % constituted by the individual mentioned ingredients).

[0064] The slurry blend obtained from the milled slurry composition can then be spray dried, freeze dried or vacuum dried and granulated to advantageously provide free-flowing powder aggregates in, for example, spherical shapes. Alternatively, the slurry blend can be vacuum dried to form an RTP powder.

[0065] In the case of spray drying, a slurry blend containing powder materials (i.e., having a ceramic hard phase powder and a metal binder phase powder) is mixed with an organic liquid, and the organic binder can be atomized by an appropriate nozzle in a drying tower, where the small droplets are instantaneously dried by a hot gas stream (e.g., in a stream of nitrogen, argon, or air) flowing horizontally into the drying tower to form spherical RTP powder aggregates with free-flowing properties. As used in the present disclosure, "atomization" refers to a process in which a large amount of liquid feed is converted into discrete droplets, greatly increasing the surface area of ​​the feed liquid, thereby significantly increasing the achievable evaporation rate of the solvent (i.e., grinding liquid). The atomization stage is designed to produce optimal conditions for evaporating the solvent from the slurry composition and causing an optimized dry RTP powder with desired free-flowing properties. Nozzles and rotary atomizers are used to form a spray. The drying tower can be equipped with only one nozzle or multiple nozzles to form spherical RTP powder aggregates with free-flowing properties.

[0066] Next, the RTP powder, which typically has a particle size below about 63 microns, is screened. For screening, a 200 mesh screen may be suitably used, which passes powders having particle size characteristics measuring less than about 74 microns. One of ordinary skill in the art of making high density carbide powders for 3D printing will know that the mesh number is inversely proportional to the particle size of the powder passing through the screen. In other words, the higher the mesh number of the screen or sieve used, the smaller the particle size passing through the screen or sieve used. Therefore, alternatively, in other examples, for screening, a 4-mesh sieve, a 6-mesh sieve, an 8-mesh sieve, a 12-mesh sieve, a 16-mesh sieve, a 20-mesh sieve, a 30-mesh sieve, a 40-mesh sieve, a 50-mesh sieve, a 60-mesh sieve, a 70-mesh sieve, an 80-mesh sieve, a 100-mesh sieve, or a 140-mesh sieve can be used, which respectively pass powders having particle size characteristics with the following measurement results: less than about 4760 microns, less than about 3360 microns, less than about 2380 microns, less than about 1680 microns, less than about 1190 microns, less than about 840 microns, less than about 590 microns, less than about 420 microns, less than about 297 microns, less than about 250 microns, less than about 210 microns, less than about 177 microns, less than about 149 microns, or less than about 105 microns. A person skilled in the art will readily be aware of different screening methods, and non-limiting examples of such screening techniques may include, but are not limited to, for example, the following screening techniques: vibratory screening, wet screening, horizontal screening, percussion screening, and air jet screening.

[0067] The screened RTP powder is then subjected to a pre-sintering temperature ramp in a first cycle. Typical temperatures for the pre-sintering in the first cycle may be temperatures starting at about 500°C and ending at about 1250°C, starting at about 500°C and ending at about 1275°C, starting at about 500°C and ending at about 1300°C, starting at about 500°C and ending at about 1325°C, starting at about 520°C and ending at about 1250°C, starting at about 520°C and ending at about 1275°C, starting at about 520°C and ending at about 1300°C, starting at about 520°C and ending at about 1325°C, starting at about 550°C and ending at about 1250°C, starting at about 550°C and ending at about 1275°C, starting at about 550°C and ending at about 1300°C, or starting at about 550°C and ending at about 1325°C. This is typically performed in a reactive hydrogen (H2) atmosphere, typically with a hydrogen (H2) flow rate of about 1000 liters / hour to about 6000 liters / hour, about 2000 liters / hour to about 6000 liters / hour, about 3000 liters / hour to about 6000 liters / hour, about 4000 liters / hour to about 6000 liters / hour, or about 5000 liters / hour to about 6000 liters / hour. The temperature can typically be continuously increased at a rate of, for example, about 0.70°C / minute. In some instances, the temperature can be sequentially increased in series in the following manner: a rate of about 2°C / minute is changed to about 10°C / minute, or, for example, a rate of about 2°C / minute is changed to about 5°C / minute. The heating can be performed in a sintering furnace at the highest temperature in a given temperature range for about 15 minutes to about 30 minutes, or about 30 minutes to about 45 minutes. The particular type of heating pattern selected is performed for a particular amount of time in a manner that imparts the desired phase change during the first pre-sintering cycle.

[0068] Typically, the pre-sintering temperature rise program in the first cycle can be carried out in a reactive hydrogen (H2) atmosphere, and the hydrogen (H2) pressure applied is usually up to about 35 mbars. In some examples, the hydrogen (H2) pressure applied is in the range of from about 5 mbars to about 35 mbars. In other examples, the hydrogen (H2) pressure applied is in the range of from about 10 mbars to about 35 mbars. In some other examples, the hydrogen (H2) pressure applied is in the range of from about 15 mbars to about 35 mbars. In some other examples, the hydrogen (H2) pressure applied is in the range of from about 20 mbars to about 35 mbars. In further other examples, the hydrogen (H2) pressure applied is in the range of from about 25 mbars to about 35 mbars. In even other examples, the hydrogen (H2) pressure applied is in the range of from about 30 mbars to about 35 mbars.

[0069] The applied hydrogen (H2) pressure can also be in the range of from about 5 mbar to about 10 mbar, from about 10 mbar to about 15 mbar, from about 15 mbar to about 20 mbar, from about 5 mbar to about 20 mbar, from about 5 mbar to about 25 mbar, from about 5 mbar to about 27 mbar, from about 5 mbar to about 30 mbar, from about 5 mbar to about 32 mbar, from about 15 mbar to about 25 mbar, from about 20 mbar to about 25 mbar, from about 20 mbar to about 27 mbar, from about 20 mbar to about 30 mbar, from about 20 mbar to about 32 mbar, from about 22 mbar to about 30 mbar, from about 25 mbar to about 30 mbar, from about 27 mbar to about 30 mbar, from about 27 mbar to about 32 mbar, or from about 27 mbar to about 35 mbar.

[0070] Next, the pre-sintered RTP powder in the first cycle is then subjected to a sintering consolidation process in a second cycle to finally form a sintered printable powder, which is finally used for binder jetting to 3D print objects after undergoing a screening operation. Typically, the sintering consolidation process in the second cycle can be appropriately carried out in an inert argon (Ar) atmosphere, typically applying an argon (Ar) pressure of up to about 50 mbar, suitably applied at a flow rate of about 30 liters / hour to about 300 liters / hour, about 100 liters / hour to about 300 liters / hour, about 150 liters / hour to about 300 liters / hour, about 200 liters / hour to about 300 liters / hour, or about 250 liters / hour to about 300 liters / hour. In some examples, the applied argon (Ar) pressure is in the range of argon (Ar) from about 10 mbar to about 50 mbar. In other examples, the applied argon (Ar) pressure is in the range of from about 15 mbar to about 50 mbar. In some other examples, the applied argon (Ar) pressure is in the range of from about 20 mbar to about 50 mbar. In some other examples, the applied argon (Ar) pressure is in the range of from about 25 mbar to about 50 mbar. In even other examples, the applied argon (Ar) pressure is in the range of from about 30 mbar to about 50 mbar. In further other examples, the applied argon (Ar) pressure is in the range of from about 35 mbar to about 50 mbar. In some other embodiments, the applied argon (Ar) pressure is in the range of from about 40 mbar to about 50 mbar. In even other embodiments, the applied argon (Ar) pressure is in the range of from about 45 mbar to about 50 mbar.

[0071] The applied argon (Ar) pressure can also be in the range of from about 10 mbar to about 15 mbar, from about 10 mbar to about 20 mbar, from about 15 mbar to about 20 mbar, from about 15 mbar to about 22 mbar, from about 15 mbar to about 25 mbar, from about 15 mbar to about 27 mbar, from about 20 mbar to about 25 mbar, from about 10 mbar to about 25 mbar, from about 25 mbar to about 30 mbar, from about 25 mbar to about 35 mbar, from about 30 mbar to about 35 mbar, from about 30 mbar to about 37 mbar, from about 30 mbar to about 40 mbar, from about 30 mbar to about 45 mbar, from about 35 mbar to about 40 mbar, from about 25 mbar to about 40 mbar, from about 25 mbar to about 45 mbar, or from about 40 mbar to about 45 mbar. Typical temperatures for the sintering in the second cycle may be applied at temperatures starting from about 500° C. and ending at about 1250° C., starting from about 500° C. and ending at about 1275° C., starting from about 500° C. and ending at about 1300° C., starting from about 500° C. and ending at about 1325° C., starting from about 520° C. and ending at about 1250° C., starting from about 520° C. and ending at about 1275° C., starting from about 520° C. and ending at about 1300° C., starting from about 520° C. and ending at about 1325° C., starting from about 550° C. and ending at about 1250° C., starting from about 550° C. and ending at about 1275° C., starting from about 550° C. and ending at about 1300° C., or starting from about 550° C. and ending at about 1325° C. The specific sintering temperature range is selected in such a way that the metal binder phase is sufficiently melted. In this process, the metal binder phase will eventually enter the liquid phase, while the carbide grains (i.e., having a much higher melting point) will remain in the solid phase. At the sintering temperature, the metal binder and the carbide grains form a eutectic liquid phase, in which the carbide grains are positioned and subsequently coated by the metal binder. As a result of this process, the metal binder embeds and bonds the carbide grains, thereby producing a metal matrix composite material with its unique material properties. The temperature can generally be continuously increased at a rate of, for example, about 0.70°C / minute. In some examples, the temperature can be sequentially increased in series in the following manner: a rate of about 2°C / minute is switched to about 10°C / minute, or, for example, a rate of about 2°C / minute is changed to about 5°C / minute. The heating can be maintained in the sintering furnace at the highest temperature of a given temperature range for about 15 minutes to about 30 minutes, or about 30 minutes to about 45 minutes, until the desired phase change occurs during the second sintering cycle. A cooling procedure can then be performed, typically by dropping the temperature to about 25°C over a time span of about 2 hours.

[0072] The sintered printable powder is thereafter sieved, typically having a particle size of about 25 microns. For sieving, a 400 mesh sieve may suitably be used, which passes powder having a particle size characteristic measuring less than about 37 microns. One of ordinary skill in the art of manufacturing high density carbide powders for 3D printing will appreciate that the mesh number is inversely proportional to the particle size of the powder passing through the sieve. In other words, the higher the mesh number of the sieve or screen used, the smaller the particle size passing through the sieve or screen used. Therefore, alternatively, in other examples, for sieving, a 4-mesh sieve, a 6-mesh sieve, an 8-mesh sieve, a 12-mesh sieve, a 16-mesh sieve, a 20-mesh sieve, a 30-mesh sieve, a 40-mesh sieve, a 50-mesh sieve, a 60-mesh sieve, a 70-mesh sieve, an 80-mesh sieve, a 100-mesh sieve, a 140-mesh sieve, a 200-mesh sieve, a 230-mesh sieve, a 270-mesh sieve, or a 325-mesh sieve may be used, which are respectively measured by having a particle size of Characteristic powder: less than about 4760 microns, less than about 3360 microns, less than about 2380 microns, less than about 1680 microns, less than about 1190 microns, less than about 840 microns, less than about 590 microns, less than about 420 microns, less than about 297 microns, less than about 250 microns, less than about 210 microns, less than about 177 microns, less than about 149 microns, less than about 105 microns, less than about 74 microns, less than about 62 microns, less than about 53 microns, or less than about 44 microns. Those skilled in the art will easily know different screening methods, and the non-limiting examples of such screening techniques can include, but are not limited to, for example, the following screening techniques: vibration screening, wet screening, horizontal screening, knocking screening and air jet screening.

[0073] To determine the specific particle size of the RTP powder and the printable powder, a person skilled in the art will be readily familiar with the following techniques: techniques using dynamic digital image analysis (DIA), static laser scattering (SLS) (also known as laser diffraction), or visual measurement by electron microscopy (techniques known as image analysis and light shielding). Each method covers a range of characteristic sizes that can be measured. These ranges overlap in part. However, the results of measuring the same sample may be different, which depends entirely on the specific method used. A technician who wants to determine the particle size or particle size distribution will readily know how each of the mentioned methods is generally performed and practiced. Thus, the reader is referred to, for example, (i) "Comparison of Methods. Dynamic Digital Image Analysis, Laser Diffraction, Sieve Analysis", Retsch Technology, Inc. and (ii) the scientific publication by Kelly et al., "Graphical comparison of image analysis and laser diffraction particle size analysis data obtained from the measurements of nonspherical particle systems", AAPS PharmSciTech. 2006 Aug 18; Vol. 7(3):69, for further insight into the various procedures and methods, all of which are incorporated herein by reference in their entirety.

[0074] The manufacturing techniques for 3D printing contemplated herein may include, for example, but are not limited to, the following techniques: binder jetting, fused deposition modeling (FDM), material jetting, electron beam powder bed, or directed energy deposition, as described in ASTM (American Society for Testing and Materials) Additive Manufacturing Technology Committee F-42.

[0075] Binder jetting can be used to 3D print a green body formed of sintered printable carbide powder. As described herein, sintered printable carbide particles can be 3D printed as a green body by using one or more ALM techniques. In theory, any feasible ALM technique that converts sintered printable carbide powder into a green body during 3D printing can be actually used. In the binder jetting process, an electronic file detailing the design parameters of the green body is provided. The binder jetting device spreads a first layer of sintered printable carbide powder in a build box. Next, the print head moves over the powder layer and deposits a liquid binder according to the specific design parameters of the unique layer. Thereafter, the formed layer is dried and cured, and the build box is lowered. A new specific layer of sintered printable carbide powder is spread according to the design parameters on the previously formed and cured layer, and the process is repeated in sequence until the entire green body is finally 3D printed. In some embodiments, other 3D printing equipment besides binder jetting may also be used to print a green body or green article from the sintered printable cemented carbide powder.

[0076] The 3D printed green body is then typically thermally cured in an oven at a temperature starting at about 150° C. and ending at about 180° C., or starting at about 180° C. and ending at about 200° C. for about 6 hours. Here, the sole purpose of the thermal curing is essentially to thermally cure the organic binder, thereby strengthening and physically holding the 3D printed green body together much like a glue. Finally, after thermal curing, the 3D printed green body is then sintered at a temperature starting at about 1500° C. and ending at about 1560° C., or starting at about 1560° C. and ending at about 1600° C., thereby completing the entire process of 3D printing an object by binder jetting.

[0077] Now go to Figure 1 , which depicts a flow chart showing all of the aforementioned process steps for making high density cemented carbide powder for binder jetting to 3D print objects according to an exemplary embodiment of the present subject matter.

[0078] like Figure 1As shown in, in step 90, a slurry composition comprising a ceramic hard phase powder, a metal binder phase powder and an organic binder in a grinding liquid is first prepared as described in paragraph

[0062] of (paragraph of the international publication text). Next, in step 95, the slurry composition is ground as described in paragraph

[0061] to obtain a slurry blend, which is then spray dried in step 100 as disclosed in paragraphs

[0063] -

[0064] to form an RTP powder. In step 105, after sieving the RTP powder as disclosed in paragraph

[0065] , the RTP powder is then pre-sintered in a first cycle as disclosed in paragraphs

[0066] -

[0068] in step 107 to obtain densification of the RTP powder. The pre-sintered RTP powder is then sintered in a second cycle as described in paragraphs

[0069] -

[0070] to form a printable powder with enhanced densification in step 110. After screening the formed printable powder in step 115 as disclosed in paragraph

[0071] , the formed printable powder is subjected to binder jetting to 3D print a green body as disclosed in paragraphs

[0073] -

[0074] . The 3D printed green body is then thermally cured in step 125 as disclosed in paragraph

[0075] , and finally the method is terminated in step 130 by sintering the thermally cured 3D printed green body to finally form the 3D object as disclosed in paragraph

[0075] .

[0079] A ceramic hard phase may be present in the RTP powder, which is suitably composed of a hard metal, typically a carbide, boride, nitride and / or carbonitride, but most typically tungsten carbide. In some instances, the ceramic hard phase of the cemented carbide composition is composed of, for example, a carbide, boride, nitride or carbonitride of at least one metal selected from Groups IVB, VB and VIB of the periodic table, or any desired combination thereof. In certain specific embodiments, the ceramic hard phase is composed of at least one of the following substances or any desired combination thereof: a carbide, boride, nitride or carbonitride of tungsten, titanium, tantalum, niobium, vanadium, zirconium, molybdenum, chromium or hafnium. In certain other specific embodiments, the ceramic hard phase is composed of tungsten carbide, tantalum carbide, niobium carbide, vanadium carbide, molybdenum carbide, chromium carbide, zirconium carbide, hafnium carbide, titanium carbide, niobium carbide, or any desired combination thereof. The ceramic hard phase encompassing the mentioned metal carbides, borides, nitrides or carbonitrides may contain them in any combination not inconsistent and incompatible with the objectives of the present subject matter.

[0080] The ceramic hard phase can generally be present in the RTP powder from about 60% to about 95% by weight based on the total weight of the cemented carbide. In some examples, the ceramic hard phase is present from about 65% to about 95% by weight based on the total weight of the cemented carbide. In other examples, the ceramic hard phase is present from about 70% to about 95% by weight based on the total weight of the cemented carbide. In some other examples, the ceramic hard phase is present from about 75% to about 95% by weight based on the total weight of the cemented carbide. In some other examples, the ceramic hard phase is present from about 80% to about 95% by weight based on the total weight of the cemented carbide. In further examples, the ceramic hard phase is present from about 85% to about 95% by weight based on the total weight of the cemented carbide. In even other examples, the ceramic hard phase is present from about 90% to about 95% by weight based on the total weight of the cemented carbide.

[0081] The ceramic hard phase may also be present in the RTP powder in an amount from about 60 wt % to about 65 wt %, from about 60 wt % to about 70 wt %, from about 65 wt % to about 70 wt %, from about 65 wt % to about 75 wt %, from about 70 wt % to about 75 wt %, from about 60 wt % to about 75 wt %, from about 60 wt % to about 80 wt %, from about 62 wt % to about 80 wt %, from about 65 wt % to about 80 wt %, from about 67 wt % to about 80 wt %, from about 70 wt % to about 80 wt %, from about 75 wt % to about 80 wt %, from about 60 wt % to about 85 wt %, from about 65 wt % to about 85 wt %, from about 67 wt % to about 85 wt %, from about 70 wt % to about 85 % to 90 weight %, from about 65 wt % to about 90 wt %, from about 67 wt % to about 90 wt %, from about 70 wt % to about 90 wt %, from about 75 wt % to about 90 wt %, from about 77 wt % to about 90 wt %, from about 80 wt % to about 90 wt %, from about 85 wt % to about 90 wt %, from about 60 wt % to about 92 wt %, from about 65 wt % to about 92 wt %, from about 67 wt % to about 92 ...2 wt %, from about 75 wt % to about 92 wt %, from about 77 wt % to about 92 wt %, from about 80 wt % to about 92 wt %, or from about 85 wt % to about 92 wt %.

[0082] The RTP powder may further suitably contain at least one or more metal binders.

[0083] The metal binder can generally be cobalt. In certain embodiments, the metal binder can desirably include one or more transition metals of Group VIIIB of the periodic table. In certain specific embodiments, the metal binder can also be a cobalt-based alloy. In certain other specific embodiments, the cobalt-based metal alloy binder can include an alloy of cobalt-transition metals. For example, the transition metal of the cobalt-based metal alloy binder can be appropriately selected from one or more of the following substances: platinum, ruthenium, rhenium, rhodium, platinum, palladium, manganese, copper, iron, nickel, or any desired combination thereof. In other embodiments, a transition metal comprising at least one of platinum, ruthenium, rhenium, rhodium, platinum, palladium, manganese, copper, iron, nickel, or any desired combination thereof can be used without cobalt. In yet other examples, the metal binder can further include a metalloid such as silicon and / or can include aluminum.

[0084] The metal binder may be present in the RTP powder in any amount that is not inconsistent and incompatible with the purposes and principles of the present disclosure. The metal binder may generally be present in the RTP powder in an amount of about 1% to about 30% by weight based on the total weight of the cemented carbide. In some examples, the metal binder is present in the RTP powder in an amount of about 1% to about 3% by weight based on the total weight of the cemented carbide. In other examples, the metal binder is present in the RTP powder in an amount of about 1% to about 5% by weight based on the total weight of the cemented carbide. In still other examples, the metal binder is present in the RTP powder in an amount of about 1% to about 7% by weight based on the total weight of the cemented carbide. In still other examples, the metal binder is present in the RTP powder in an amount of about 1% to about 10% by weight based on the total weight of the cemented carbide. In further other examples, the metal binder is present in the RTP powder in an amount of about 1% to about 15% by weight based on the total weight of the cemented carbide. In even other examples, the metal binder is present in the RTP powder in an amount of about 1 wt % to about 20 wt % based on the total weight of the cemented carbide. In still other embodiments, the metal binder is present in the RTP powder in an amount of about 1 wt % to about 25 wt % based on the total weight of the cemented carbide. In even other embodiments, the metal binder is present in the RTP powder in an amount of about 1 wt % to about 27 wt % based on the total weight of the cemented carbide.

[0085] The metallic binder may also be present in the RTP powder in an amount based on the total weight of the cemented carbide of about 1 wt % to about 2 wt %, from about 2 wt % to about 5 wt %, from about 5 wt % to about 7 wt %, from about 3 wt % to about 7 wt %, from about 7 wt % to about 10 wt %, about 10.1 wt %, about 10.2 wt %, about 10.3 wt %, about 10.4 wt %, about 10.5 wt %, about 10.6 wt %, about 10.7 wt %, about 10.8 wt %, about 10.9 wt %, from about 7 wt % to about 13 wt %, from about 7 wt % to about 15 wt %, from about 7 wt % to about 17 wt %, from about 7 wt % to about 20 wt %, from about 7 wt % to about 22 wt %, from about 7 wt % to about 25 wt %, from about 7 wt % to about % to about 27% by weight, from about 7% to about 30% by weight, from about 10% to about 13% by weight, from about 10% to about 15% by weight, from about 10% to about 17% by weight, from about 10% to about 20% by weight, from about 10% to about 22% by weight, from about 10% to about 25% by weight, from about 15% to about 20% by weight, from about 15% to about 22% by weight, from about 15% to about 25% by weight, from about 15% to about 27% by weight, from about 10% to about 30% by weight, from about 15% to about 30% by weight, from about 17% to about 30% by weight, from about 20% to about 30% by weight, from about 22% to about 30% by weight, from about 25% to about 30% by weight, or from about 27% to about 30% by weight.

[0086] The processed RTP powders and printable powders disclosed in this application may each have a range from at least about 5 g / cm 3 to about 15 g / cm 3 In some examples, the processed RTP powder and the printable powder have an apparent density ranging from at least about 7 g / cm 3 to about 15 g / cm 3 In other examples, the processed RTP powder and the printable powder have an apparent density ranging from at least about 10 g / cm 3 to about 15 g / cm 3 In yet other examples, the processed RTP powder and the printable powder have an apparent density ranging from at least about 12 g / cm 3 to about 15 g / cm 3 In yet other examples, the processed RTP powder and the printable powder have an apparent density ranging from at least about 14 g / cm 3 to about 15 g / cm 3within the range.

[0087] The processed RTP powder and the printable powder may also have an apparent density in the range of from at least about 5 g / cm 3 to about 6 g / cm 3 , from at least about 5 g / cm 3 to about 7 g / cm 3 , from at least about 5 g / cm 3 to about 8 g / cm 3 , from at least about 5 g / cm 3 to about 9 g / cm 3 , from at least about 5 g / cm 3 to about 10 g / cm 3 , from at least about 5 g / cm 3 to about 11 g / cm 3 , from at least about 5 g / cm 3 to about 12 g / cm 3 , from at least about 5 g / cm 3 to about 13 g / cm 3 , from at least about 5 g / cm 3 to about 14 g / cm 3 , 6 g / cm 3 to about 7 g / cm 3 , from at least about 6 g / cm 3 to about 8 g / cm 3 , from at least about 6 g / cm 3 to about 9 g / cm 3 , from at least about 6 g / cm 3 to about 10 g / cm 3 , from at least about 6 g / cm 3 to about 11 g / cm 3 , from at least about 6 g / cm 3 to about 12 g / cm 3 , from at least about 6 g / cm 3 to about 13 g / cm 3 , from at least about 6 g / cm 3 to about 14 g / cm 3 , from at least about 6 g / cm 3 to about 15 g / cm 3 , from at least about 7 g / cm 3 to about 8 g / cm 3 , from at least about 7 g / cm 3 to about 9 g / cm 3 , from at least about 7g / cm 3to about 10 g / cm 3 , from at least about 7 g / cm 3 to about 11 g / cm 3 , from at least about 7 g / cm 3 to about 12 g / cm 3 , from at least about 7 g / cm 3 to about 13 g / cm 3 , from at least about 7 g / cm 3 to about 14 g / cm 3 , from at least about 8 g / cm 3 to about 9 g / cm 3 , from at least about 8 g / cm 3 to about 10 g / cm 3 , from at least about 8 g / cm 3 to about 11 g / cm 3 , from at least about 8 g / cm 3 About 12g / cm 3 , from at least about 8 g / cm 3 to about 13 g / cm 3 , from at least about 8 g / cm 3 to about 14 g / cm 3 , from at least about 8 g / cm 3 to about 15 g / cm 3 , from at least about 9 g / cm 3 to about 10 g / cm 3 , from at least about 9 g / cm 3 to about 11 g / cm 3 , from at least about 9 g / cm 3 to about 12 g / cm 3 , from at least about 9 g / cm 3 to about 13 g / cm 3 , from at least about 9 g / cm 3 to about 14 g / cm 3 , from at least about 9 g / cm 3 to about 15 g / cm 3 , from at least about 10 g / cm 3 to about 11 g / cm 3 , from at least about 10 g / cm 3 to about 12 g / cm 3 , from at least about 10 g / cm 3 to about 13 g / cm 3 , from at least about 10 g / cm 3 to about 14 g / cm 3, from at least about 11 g / cm 3 to about 12 g / cm 3 , from at least about 11 g / cm 3 to about 13 g / cm 3 , from at least about 11 g / cm 3 to about 14 g / cm 3 , or from at least about 11 g / cm 3 to about 15 g / cm 3 , from at least about 12 g / cm 3 to about 13 g / cm 3 , from at least about 12 g / cm 3 to about 14 g / cm 3 , from at least about 13 g / cm 3 to about 14 g / cm 3 , or from at least about 13 g / cm 3 to about 15 g / cm 3 .

[0088] The yield of the formed printable powder can generally be from about 60% to about 90%, or can be at least 90%. In some instances, the yield of the formed printable powder is from about 70% to about 90%. In other instances, the yield of the formed printable powder is from about 80% to about 90%. In yet other instances, the yield of the formed printable powder is from about 85% to about 90%. In even other instances, the yield of the formed printable powder is at least 90%.

[0089] The yield of the printable powder formed can also be from about 60% to about 65%, from about 60% to about 70%, from about 60% to about 75%, from about 60% to about 80%, from about 60% to about 85%, from about 65% to about 70%, from about 65% to about 75%, from about 65% to about 80%, from about 65% to about 85%, from about 65% to about 90%, from about 70% to about 75%, from about 70% to about 80%, from about 70% to about 85%, from about 75% to about 80%, from about 75% to about 85%, from about 75% to about 90%, or from about 80% to about 85%.

[0090] Example

[0091] The following examples are put forward to provide those of ordinary skill in the art with a complete disclosure and description of how to make and use the subject matter, and are not intended to limit the scope of what the inventors regard as their disclosure, nor are they intended to represent that the experiments below are all or the only experiments performed. Efforts have been made to ensure accuracy of the numbers used, but some experimental errors and deviations should be accounted for.

[0092] Example 1

[0093] Printable powders show higher apparent density than pre-sintered RTP powders

[0094]

[0095] The apparent density of a high-density cemented carbide powder for binder jetting to 3D print objects according to an exemplary embodiment of the present subject matter is determined after different processing stages. First, the apparent density of the RTP powder formed after spray drying the slurry blend is determined. Next, the apparent density of the pre-sintered RTP powder in the first cycle is obtained. Finally, the apparent density of the sintered RTP powder in the second cycle is obtained. In order to achieve the above objectives, the RTP powder having a particle size of less than about 63 microns is sieved using a 200-mesh sieve. Obtain the apparent density of the RTP powder. Next, the RTP powder is pre-sintered in the first cycle at about 1250° C. in a furnace using a zirconia crucible for about 30 minutes to increase the density and further maintain the spherical morphology of the RTP powder particles. The RTP powder is crushed in a grinding mill by grinding the RTP powder for about 30 minutes to break up any remaining lumps. Next, the ground RTP powder is sieved through a 200-mesh sieve to remove any remaining aggregates and measure the apparent density. The RTP powder is then sintered in a second cycle at about 1250°C for about 30 minutes to increase the apparent density and form a printable powder. The formed printable powder is then crushed in a grinder by grinding the printable powder for about 30 minutes to break up any remaining lumps. Next, the ground printable powder having a particle size of about 25 microns is sieved through a 400-mesh sieve to remove any aggregates present and maintain the desired particle size, and the apparent density is measured. Finally, the fully densified printable powder obtained can then be used for binder jetting to 3D print objects. The results obtained are shown in Table 1. Obviously, Table 1 shows that the apparent density increases with each increase in the number of sintering cycles. The unsintered RTP powder shows an apparent density of 3.27 g / cm 3 When the RTP powder was pre-sintered in the first cycle, the pre-sintering procedure of the RTP powder caused the apparent density to increase from 3.27 g / cm 3 Increased to 5.25 g / cm 3 , an increase of nearly 60.5%. When the RTP powder is sintered in the second cycle to finally form a fully densified printable powder, the apparent density further increases from 5.25 g / cm 3 Increased to 5.45 g / cm 3 , so the apparent density increases by about 3.8%.

[0096] While the present disclosure has been described in conjunction with embodiments thereof, those skilled in the art will appreciate that additions, deletions, modifications and substitutions not specifically described may be made without departing from the spirit and scope of the present disclosure as defined in the appended claims.

[0097] With respect to the use of substantially any plural and / or singular terms herein, those skilled in the art may convert from the plural to the singular and / or from the singular to the plural as appropriate, depending on the context and / or application. For clarity, various singular / plural permutations are not explicitly set forth herein.

[0098] The subject matter described herein sometimes shows the different parts that are contained in different other parts or are connected with different other parts.It should be understood that the structure described in this way is only exemplary, and in fact many other structures that realize the same function can be implemented.In a conceptual sense, any arrangement of the parts realizing the same function is effectively "associated" so that the desired function is realized.Therefore, any two parts that are combined to realize a specific function herein can be regarded as "associated" with each other so that the desired function is realized, regardless of the structure or the intermediate parts.Similarly, any two parts that are so associated can also be regarded as "operably connected" or "operably combined" with each other to realize the desired function, and any two parts that can be so associated can also be regarded as "operably combined" with each other to realize the desired function.The specific example that can be operably combined includes but is not limited to physically matchable and / or physically interactive parts, and / or wirelessly interactive and / or wirelessly interactive parts, and / or logically interactive and / or logically interactive parts.

[0099] In some cases, one or more components may be referred to herein as being "configured to," "configured by," "configurable to," "operable / operable to," "adapted / adaptable," "capable of," "conformable / conformable to," etc. Those skilled in the art will recognize that such terms (e.g., "configured to") may generally encompass active state components and / or inactive state components and / or standby state components unless the context requires otherwise.

[0100] Although particular aspects of the subject matter described herein have been shown and described, it will be apparent to those skilled in the art that, based on the teachings herein, changes and modifications may be made without departing from the subject matter described herein and its broader aspects, and therefore, the appended claims will cover within their scope all such changes and modifications that are within the true spirit and scope of the subject matter described herein. Those skilled in the art will understand that, in general, the terms used herein, especially in the appended claims (e.g., the bodies of the appended claims), are generally intended to be "open" terms (e.g., the term "including" should be interpreted as "including but not limited to", the term "having" should be interpreted as "having at least", the term "comprising" should be interpreted as "including but not limited to", etc.).

[0101] Those skilled in the art will further understand that if a specific number of claim statements are intended to be introduced, such intent will be explicitly stated in the claim, and in the absence of such a statement, no such intent exists. For example, to aid understanding, the appended claims may contain the use of the introductory phrases "at least one" and "one or more" to introduce claim statements. However, the use of such phrases should not be interpreted as implying that a claim statement introduced by the indefinite article "a" or "an" will limit any particular claim containing such introduced claim statement to a claim containing only one such feature, even when the same claim includes the introductory phrases "one or more" or "at least one" and an indefinite article such as "a" or "an" (e.g., "a" and / or "an" should generally be interpreted as meaning "at least one" or "one or more"); the same is true for the use of definite articles used to introduce claim statements.

[0102] Furthermore, even if a specific number of an introduced claim statement is explicitly recited, those skilled in the art will recognize that such a statement should generally be interpreted to mean at least the stated number (e.g., a bare statement of "two statements" without other modifiers generally means at least two statements, or more than two statements).

[0103] Furthermore, in those cases where a convention similar to “at least one of A, B, and C, etc.” is used, generally such construction is intended to mean that one skilled in the art will understand the convention (e.g., “a system having at least one of A, B, and C” will include but is not limited to systems having A alone, B alone, C alone, A and B together, A and C together, B and C together, and / or A, B, and C together, etc.). In those cases where a convention similar to “at least one of A, B, or C, etc.” is used, generally such construction is intended to mean that one skilled in the art will understand the convention (e.g., “a system having at least one of A, B, or C” will include but is not limited to systems having A alone, B alone, C alone, A and B together, A and C together, B and C together, and / or A, B, and C together, etc.). One skilled in the art will further understand that generally disjunctive words and / or phrases (whether in the specification, claims, or drawings) that present two or more alternative terms should be understood to contemplate the possibility of including one, either, or both terms, unless the context dictates otherwise. For example, the phrase "A or B" will generally be understood to include the possibilities of "A" or "B" or "A and B."

[0104] With respect to the appended claims, those skilled in the art will appreciate that the operations stated therein may generally be performed in any order. Moreover, although various operational flows are presented in order, it should be understood that the various operations may be performed in an order different from the order shown, or may be performed simultaneously. Unless the context otherwise dictates, examples of such alternative orderings may include overlapping, interleaved, interrupted, reordered, incremental, preparatory, supplementary, simultaneous, reverse, or other variant orderings. In addition, terms such as "responsive to," "about," or other past tense adjectives are generally not intended to exclude such variants, unless the context otherwise dictates.

[0105] Those skilled in the art will appreciate that the foregoing specific exemplary processes and / or apparatus and / or techniques represent more general processes and / or apparatus and / or techniques taught elsewhere herein, such as in the claims filed herein and / or elsewhere in this application.

[0106] While various aspects and embodiments have been disclosed herein, other aspects and embodiments will be apparent to those skilled in the art. The various aspects and embodiments disclosed herein are for purposes of illustration and are not intended to be limiting, with the true scope and spirit being indicated by the following claims.

[0107] The exemplary embodiments described in the detailed description, drawings, and claims are not meant to be limiting. Other embodiments may be utilized, and other changes may be made, without departing from the spirit or scope of the subject matter presented here.

[0108] Where a range of values ​​is provided, it is understood that each intervening value (to the tenth of the unit of the lower limit unless the context clearly dictates otherwise) between the upper and lower limits of that range and any other stated value or intervening value in that stated range is encompassed within the disclosed range. The upper and lower limits of these smaller ranges, which may independently be included in smaller ranges, are also encompassed within the disclosed content, subject to any specifically excluded limits in the stated range. Where the stated range includes one or both of the limits, ranges excluding one or both of those included limits are also encompassed within the disclosed content.

[0109] Those skilled in the art will recognize that for conceptual clarity, the components (e.g., operations), devices, objects, and discussions accompanying them described herein are used as examples, and various configuration modifications are contemplated. Therefore, as used herein, the specific examples set forth and the accompanying discussions are intended to represent their more general categories. In general, the use of any specific example is intended to represent its category, and the exclusion of specific components (e.g., operations), devices, and objects should not be considered limiting.

[0110] Additionally, for example, any sequence and / or chronological order of the systems and methods described herein is exemplary and should not be construed as being limiting in nature. Thus, it should be understood that process steps may be shown and described as being in sequence or chronological order, but they are not necessarily limited to being performed in any particular order or sequence. For example, the steps in such a process or method may generally be performed in a variety of different sequences and orders while still falling within the scope of the present disclosure.

[0111] Finally, the applications, publications and / or patents discussed herein are provided solely for their disclosure prior to the filing date of the disclosure. Nothing herein should be construed as an admission that the disclosed disclosure is not entitled to antedate such publication by virtue of prior publication.

Claims

1. A method for manufacturing a three-dimensional (3D) object, comprising: preparing a slurry composition comprising a ceramic hard phase powder, a metal binder phase powder and an organic binder in a grinding liquid; grinding the slurry composition to form a slurry blend; spray drying the slurry blend to obtain an RTP powder; sieving the RTP powder; pre-sintering the RTP powder in a first cycle to obtain densification of the RTP powder; sintering the pre-sintered RTP powder in a second cycle to form a printable powder with enhanced densification; sieving the printable powder; subjecting the printable powder to binder jetting to 3D print a green body; Solidifying the 3D printed green body; and The solidified 3D printed green body is sintered to form the 3D object.

2. The method of manufacturing a three-dimensional (3D) object according to claim 1, wherein the RTP powder is free-flowing.

3. The method of manufacturing a three-dimensional (3D) object according to claim 1, wherein the pre-sintering in the first cycle is performed at a temperature starting from about 550°C and ending at about 1250°C.

4. A method for manufacturing a three-dimensional (3D) object according to claim 3, wherein the pre-sintering in the first cycle is carried out in an atmosphere with a hydrogen pressure of up to about 35 mbar and the applied hydrogen flow is up to about 6000 liters / hour. 5 . The method for manufacturing a three-dimensional (3D) object according to claim 3 , wherein the pre-sintering in the first cycle is performed for about 15 minutes to about 30 minutes. 6 . The method for manufacturing a three-dimensional (3D) object according to claim 3 , wherein the pre-sintering in the first cycle is performed for about 30 minutes to about 45 minutes.

7. The method of manufacturing a three-dimensional (3D) object according to claim 1, wherein the sintering in the second cycle is performed at a temperature starting from about 550°C and ending at about 1250°C.

8. The method for manufacturing a three-dimensional (3D) object according to claim 7, wherein the sintering in the second cycle is carried out in an atmosphere with an argon pressure of up to about 50 mbar and the applied argon flow is up to about 300 liters / hour. 9 . The method for manufacturing a three-dimensional (3D) object according to claim 7 , wherein the sintering in the second cycle is performed for about 15 minutes to about 30 minutes.

10. The method of manufacturing a three-dimensional (3D) object according to claim 7, wherein the sintering in the second cycle is performed for about 30 minutes to about 45 minutes.

11. The method of manufacturing a three-dimensional (3D) object according to claim 1, wherein the yield of the printable powder formed is from about 60% to about 90%.

12. The method of manufacturing a three-dimensional (3D) object according to claim 11, wherein the yield of the printable powder formed is from about 70% to about 90%.

13. The method of manufacturing a three-dimensional (3D) object according to claim 12, wherein the yield of the printable powder formed is from about 80% to about 90%.

14. The method of manufacturing a three-dimensional (3D) object according to claim 13, wherein the yield of the printable powder formed is from about 85% to about 90%.

15. A method for manufacturing a three-dimensional (3D) object according to claim 14, wherein the yield of the printable powder formed is at least 90%.

16. The method of manufacturing a three-dimensional (3D) object according to claim 1, wherein the apparent density of the RTP powder and the printable powder is from at least about 5 g / cm 3 to about 15 g / cm 3 within the range.

17. The method for manufacturing a three-dimensional (3D) object according to claim 1, wherein the ceramic hard phase comprises one or more of the following substances: tungsten carbide (WC), titanium carbide (TiC), tantalum carbide (TaC), niobium carbide (NbC), vanadium carbide (VC), zirconium carbide (ZrC), molybdenum carbide (Mo2C) or hafnium carbide (HfC), or any combination thereof.

18. The method of manufacturing a three-dimensional (3D) object according to claim 17, wherein the ceramic hard phase comprises WC.

19. The method of manufacturing a three-dimensional (3D) object according to claim 1, wherein the metallic binder phase powder comprises cobalt.

20. The method for manufacturing a three-dimensional (3D) object according to claim 1, wherein the RTP powder is sieved through a 4-mesh sieve, a 6-mesh sieve, an 8-mesh sieve, a 12-mesh sieve, a 16-mesh sieve, a 20-mesh sieve, a 30-mesh sieve, a 40-mesh sieve, a 50-mesh sieve, a 60-mesh sieve, a 70-mesh sieve, an 80-mesh sieve, a 100-mesh sieve, a 140-mesh sieve, or a 200-mesh sieve.

21. The method for manufacturing a three-dimensional (3D) object according to claim 1, wherein the printable powder is sieved through a 4-mesh sieve, a 6-mesh sieve, an 8-mesh sieve, a 12-mesh sieve, a 16-mesh sieve, a 20-mesh sieve, a 30-mesh sieve, a 40-mesh sieve, a 50-mesh sieve, a 60-mesh sieve, a 70-mesh sieve, an 80-mesh sieve, a 100-mesh sieve, a 140-mesh sieve, a 200-mesh sieve, a 230-mesh sieve, a 270-mesh sieve, a 325-mesh sieve, or a 400-mesh sieve.

22. The method of manufacturing a three-dimensional (3D) object according to claim 1, wherein curing the 3D printed green body is performed at a temperature starting from about 150°C and ending at about 180°C.

23. The method of manufacturing a three-dimensional (3D) object according to claim 1, wherein the curing of the 3D printed green body is performed at a temperature starting at about 180°C and ending at about 200°C.

24. The method of manufacturing a three-dimensional (3D) object according to claim 22, wherein curing the 3D printed green body is performed for up to about 6 hours.

25. The method of manufacturing a three-dimensional (3D) object according to claim 1, wherein the sintering of the solidified 3D printed green body is performed at a temperature starting from 1500°C and ending at about 1560°C.

26. The method of manufacturing a three-dimensional (3D) object according to claim 1, wherein the sintering of the solidified 3D printed green body is performed at a temperature starting from 1560°C and ending at about 1600°C.

27. A method for manufacturing a three-dimensional (3D) object according to claim 1, wherein the printable powder is fully densified.