Novel welding duplex stainless steel material suitable for welding duplex stainless steel, and welding joint and welding method thereof

By balancing the contents of chromium, nickel, nitrogen, Mo and W, a new type of welded duplex stainless steel material was developed, which solved the problems of insufficient strength and toughness and nitrogen loss when welding high-alloy duplex stainless steel, and achieved high mechanical properties of the welded joints and Corrosion resistance ensures the stability of the welding process and the superiority of multi-pass welding.

CN118984757APending Publication Date: 2024-11-19HORIMAI PIPE CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202380033665.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-12
Filing Date
2023-04-11
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

When welding high alloy duplex stainless steel, it is difficult to find welding materials that can provide sufficient strength and maintain toughness. At the same time, there is a problem of nitrogen loss, which affects the mechanical properties and corrosion resistance of the welded joints.

Method used

By balancing the contents of chromium, nickel, nitrogen, Mo and W, a new welded duplex stainless steel material is developed to ensure high strength and toughness of the welded joints, and to reduce nitrogen loss, avoiding intermetallic phases and undesired nitride formation. Ensure the stability of the welding process to ferrite austenite balance.

Benefits of technology

The high mechanical properties and corrosion resistance of welded joints are achieved, ensuring that the effect of the welding process does not negatively affect the ferrite austenite balance, maintains ductility, and provides an excellent range of alloy elements in multi-pass welding to ensure that High strength and toughness of welded joints.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_2
    Figure FT_2
  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The present disclosure relates to a welded duplex stainless steel material comprising the following alloying elements (in wt%): C at maximum 0.030, Si at maximum 0.50, Mn from 0.50 to 2.50, P at maximum 0.030, S at maximum 0.030, Cr from 29.0 to 32.0, Ni from 7.0 to 11.0, Mo from 0.50 to 1.50, W from 3.00 to 4.50, Cu at maximum 0.50, N from 0.25 to 0.45, Fe and unavoidable impurities balance and ferrite: austenite content from 35: 65 to 65: 35 by volume. The duplex stainless steel material may be in the form of a wire or a strip. The welding material will be used to join duplex stainless steel, and the welding material will have and also produce a welded joint with high strength. The invention further relates to a welding method for carrying out single-pass or multi-pass welding by using the welding material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to a novel welded duplex stainless steel material, which may be in the form of a wire or a strip. The welded material is intended for use in joining duplex stainless steels. The present disclosure also relates to a welding method using the welded material. Background Art

[0002] In order to be able to launch components such as tubes or strips made of new alloys on the market, it is often necessary to be able to weld these components. The welding material used should essentially have the material properties of the components in question in order to avoid the produced welds being weak points in terms of mechanical properties (such as strength and toughness) and / or corrosion resistance.

[0003] The oil and gas industry has an increasing demand for high-strength components made of high-alloy duplex stainless steels, as these materials are attractive for their corrosion resistance and their good mechanical properties. However, it is difficult to find welding materials that provide sufficient strength to the weld joint while maintaining its strength and toughness when used for single and multi-pass welding.

[0004] Additionally, these high alloy duplex stainless steels are also known to suffer from nitrogen losses during welding when used as filler materials, and there is a need for a welding material that mitigates the negative effects of these losses on the strength and toughness of the weld joint.

[0005] Therefore, the present disclosure will solve or at least alleviate the above problems. BRIEF DESCRIPTION OF THE DRAWINGS

[0006] The present disclosure is also illustrated by the following non-limiting drawings:

[0007] Figure 1 shows the intermetallic phase of material 1 of Example measured using LOM (image analysis, 500 times magnification);

[0008] Figure 2 The intermetallic phase of Material 2 of Example measured using LOM (image analysis, 500 times magnification) is shown. Summary of the invention

[0009] The present disclosure relates to a novel welded duplex stainless steel material, which may be in the form of a wire or strip. The welding material is intended to be used to join duplex stainless steels, and the welding material itself will have and also produce welded joints with high strength. The present disclosure also relates to a welding method using the welding material for single-pass or multi-pass welding. DETAILED DESCRIPTION

[0010] The inventors of the present invention have found that by balancing the ranges of chromium, nickel and nitrogen as well as Mo and W, a welded duplex stainless steel material suitable for welding duplex stainless steels will be obtained.

[0011] The present welded duplex stainless steel material will have both high strength and toughness, and also provide welded joints with high strength and toughness, even providing welded joints formed in multiple passes. In addition, when used for welding, the welded duplex stainless steel material forms little or no intermetallic phases, such as sigma phase and undesirable nitrides, in both the joint and the heat affected zone, and the present welded duplex stainless steel material can also reduce the effects of nitrogen loss in the filler material during welding.

[0012] Furthermore, the alloying range of the welded duplex stainless steel material of the present invention will ensure that the effects of the welding process will not negatively affect the ferrite:austenite balance, thereby ensuring that the welded joint has good mechanical properties and corrosion resistance. Furthermore, the alloying range of the welded duplex stainless steel material of the present invention will make the material resistant to intermetallic phase precipitation, which means that despite the heating associated with welding, which is often repeated, the material will maintain its ductility.

[0013] Therefore, the present disclosure relates to a welded duplex stainless steel material comprising the following alloying elements (in weight %):

[0014] C Max 0.030

[0015] Si max 0.50

[0016] Mn 0.50 to 2.50

[0017] P max 0.030

[0018] S Max 0.030

[0019] Cr 29.0 to 32.0

[0020] Ni 7.0 to 11.0

[0021] Mo 0.50 to 1.50

[0022] W 3.00 to 4.50

[0023] Cu Max 0.50

[0024] N 0.25 to 0.45

[0025] Fe and unavoidable impurities balance

[0026] And the ferrite:austenite content is 35:65 to 65:35 by volume.

[0027] In this disclosure, the terms "weight %" and "wt %" are used interchangeably.

[0028] According to an embodiment, in order to provide sufficient corrosion resistance, the welded duplex stainless steel material has a PRE ([Cr]+3.3×([Mo]+0.5×[W])+16×[N])≥43. The values ​​of the alloying elements are in weight %.

[0029] Furthermore, the present disclosure relates to a welded duplex stainless steel material as defined above or below for obtaining a welded joint. Thus, the welded joint will contain the same range of alloying elements as the welded duplex stainless steel material as defined above or below.

[0030] The present disclosure also relates to a method of producing a welded joint comprising a material as defined above or below, wherein the method is a single-pass or multi-pass welding method.

[0031] According to the present disclosure, the yield strength of the obtained welded joint at room temperature may be at least 700 MPa (ISO 6892-1).

[0032] According to the present disclosure, the impact toughness of the obtained welded joint at room temperature may be at least 50 J (ISO 148-1).

[0033] The principles and advantages of the present welded duplex stainless steel material and the selection of the range of alloying elements that give duplex stainless steel unexpected superiority can be described as follows. However, the present disclosure is not limited to the exemplary embodiments discussed, but can be varied within the scope of the appended claims. Unless otherwise explicitly disclosed, the upper and lower limits of individual constituent elements can be freely combined within the widest limits described in the claims. In addition, when a range is disclosed in the present disclosure, unless otherwise explicitly disclosed, the range includes the corresponding endpoint values ​​of the range. Similarly, when an open range is disclosed, unless otherwise explicitly disclosed, the open range also includes the single endpoint values ​​of the open range.

[0034] Chromium (Cr)

[0035] Chromium is an essential element, the range of which has been selected to support the strength and corrosion resistance of the present duplex stainless steel. In order to have good strength properties, good impact properties and corrosion resistance, the chromium content should be equal to or at least 29.0 wt%.

[0036] However, even though chromium is a beneficial element, its content should not be greater than or equal to 32.0 wt % because a high content of Cr will increase the risk of forming sigma phase during welding.

[0037] Furthermore, the inventors have found that it is important to ensure a balance of chromium, nickel and nitrogen content in order to avoid the formation of sigma phase and obtain maximum strength. Furthermore, as can be seen in the examples of the present disclosure, it has been shown that the chromium content of the present invention is sufficient to compensate for the nitrogen loss that occurs during welding, thereby avoiding a decrease in strength.

[0038] Therefore, the chromium content of the present welded duplex stainless steel material is 29.0 wt % to 32.0 wt %. To further ensure that the above properties can be obtained, the chromium content is 29.5 wt % to 32.0 wt %, such as 30.0 wt % to 32.0 wt %, such as 30.5 wt % to 31.5 wt %.

[0039] Nickel (Ni)

[0040] Ni is used as an austenite stabilizing element and is added to the present welded duplex stainless steel material at a suitable level to obtain the desired austenite and ferrite content. In order to obtain a volume ratio of ferrite: austenite of 35-65:65-35, the nickel content should be equal to or at least 7.0 wt%. In addition, the inventors have found that the recommended nickel content in the present welded duplex stainless steel material will hardly form intermetallic phases such as σ phase and undesirable nitrides, and thus have high impact toughness, because the σ phase will have a negative impact on the impact toughness.

[0041] According to the present disclosure, the maximum content of nickel is 11.0 wt %.

[0042] According to the present disclosure, the Ni content may be 7.5 wt % to 11.0 wt %, such as 8.0 wt % to 11.0 wt %, such as 8.5 wt % to 10.5 wt %.

[0043] Molybdenum (Mo)

[0044] Mo is an active element that improves strength and corrosion resistance in chloride environments and reducing acids.

[0045] However, excessive Mo content combined with high Cr content will increase the risk of σ phase formation. Therefore, it is important to select the Mo content to avoid the formation of σ phase in the weld joint and to obtain the maximum strength of the weld joint. In addition, if the present welded duplex stainless steel material does not contain any Mo, too many nitrides will be formed during cooling.

[0046] Therefore, the content of Mo should be in a range of equal to or at least 0.50 wt %, and the content of Mo should be equal to or not greater than 1.50 wt %. The content of Mo may also be equal to or not greater than 1.20 wt %. In addition, the content of Mo may be at least 0.50 wt % to 1.00 wt %.

[0047] Tungsten (W)

[0048] W will improve the corrosion resistance in chloride environments as well as the pitting and crevice corrosion resistance. However, too high a W content combined with a high Cr content will increase the risk of σ phase precipitation in the weld joint. Therefore, it is very important to optimize the combined amounts of chromium, molybdenum and tungsten to avoid the formation of σ phase and undesirable nitrides.

[0049] Therefore, the content of W is 3.00 wt % to 4.50 wt %. According to an embodiment, the content of W may be 3.00 wt % to 4.00 wt %.

[0050] Nitrogen (N)

[0051] Nitrogen is a very active element that increases corrosion resistance as well as strength. To achieve good results, at least 0.25 wt. % N should be added.

[0052] However, since the added N must be dissolved in the welded duplex stainless steel material and in the weld joint, the N content must be carefully selected, as too high a N content increases the risk of chromium nitride precipitation, especially when the chromium content is also high. Excessive nitrogen also carries the risk of pore formation in the weld. Therefore, the N content should be limited to equal to or less than 0.45 wt.%.

[0053] Nitrogen is also an element that is very important to the microstructure of the weld and weld material. During welding, the weld material will lose a large amount of nitrogen due to evaporation due to the heat of the welding process. The loss of nitrogen will result in the weld joint having a more ferritic microstructure with larger grains and nitride precipitates. These microstructural changes will have a negative impact on the mechanical properties and corrosion resistance of the weld. However, the inventors have discovered a nitrogen range for the present welded duplex stainless steel material where the effects of these losses will be reduced, such that the welded duplex stainless steel material may lose nitrogen but still provide a weld joint with excellent mechanical properties and corrosion resistance.

[0054] Therefore, the content of nitrogen is 0.25 wt % to 0.45 wt %. In addition, the content of N may be 0.25 wt % to 0.40 wt %, such as 0.25 wt % to 0.35 wt %.

[0055] Manganese (Mn)

[0056] In order to increase the solubility of nitrogen, Mn is added. However, Mn may also form manganese sulfide, which becomes the starting point of pitting corrosion. Therefore, the content of Mn is 0.50 wt % or more and less than or equal to 2.50 wt %, and the content of Mn can be 0.50 wt % to 2.00 wt %, such as 0.50 wt % to 1.50 wt %.

[0057] Silicon (Si)

[0058] Si is used as a deoxidizer during steel manufacturing and can also improve the fluidity of the molten weld metal. It is known that high silicon content can stabilize the σ phase. Therefore, the content of silicon should be limited to a maximum of 0.50 wt%. Since Si should be present, in order to provide the desired effect, the content of Si can be at least or equal to 0.05 wt%. In addition, according to the present disclosure, the content of silicon can be 0.10 wt% to 0.30 wt%.

[0059] Carbon (C)

[0060] C strengthens stainless steel, but also promotes the formation of chromium carbides which are harmful to corrosion. Carbon also has limited solubility in both ferrite and austenite. Therefore, the carbon content should be limited to a maximum of 0.030% by weight, such as a maximum of 0.025% by weight.

[0061] Carbon is not an intentionally added element and there is no critical lower limit to the carbon content. However, pursuing extremely low carbon content will excessively increase processing costs. Therefore, in practice, the amount of carbon present can be at least 0.01% or even at least 0.02%.

[0062] According to an embodiment, the carbon content is 0.005 wt % to 0.025 wt %.

[0063] Copper (Cu)

[0064] In order to improve the resistance to certain corrosive environments such as acidic environments and reduce the sensitivity to stress corrosion cracking, Cu can be added. In addition, Cu will increase the strength and delay the formation of σ phase in the welded joint.

[0065] Copper is therefore an alloying element that is beneficial for increasing strength, but due to its negative effect on nitrogen solubility, this element may increase the risk of chromium nitride formation. Therefore, it is very important to carefully adjust the amount of copper if added.

[0066] Therefore, the content of Cu is limited to be equal to or less than 0.50 wt%. According to one embodiment, Cu is intentionally added, and the content of Cu is between 0.15 wt% and 0.50 wt%. According to an embodiment, the Cu content may be between 0.20 wt% and 0.40 wt%.

[0067] Sulfur (S)

[0068] Sulfur is an impurity element and must be removed in order to improve hot workability. The sulfur content should not be greater than 0.030 wt % so that the adverse effects of sulfur can be avoided.

[0069] Phosphorus (P)

[0070] Phosphorus is also an impurity element, and when the total phosphorus content is not more than 0.030 wt %, its adverse effect on hot workability is reduced.

[0071] The ferrite content of the present welding material, that is, the volume ratio of ferrite: austenite is 35-65:65-35. According to an embodiment, the ferrite content is at least or equal to 45% by volume, and should not be greater than 60% by volume, and the rest is essentially austenite. According to an embodiment, the ferrite content is in the range of 48% by volume to 55% by volume, and the rest is essentially austenite. Phase balance is important in welding duplex stainless steel materials because it helps to obtain optimal mechanical properties and corrosion resistance. In addition, too low a ferrite content will increase the risk of forming intermetallic phases such as σ phases and undesirable nitrides because ferrite is rich in chromium and molybdenum. In addition, too high a ferrite content will increase the risk of secondary austenite forming within the ferrite grains. The amount of ferrite can be measured metallographically by studying the weld metal microstructure at 200 to 500 times magnification, and corrosion is performed to distinguish ferrite and austenite by color. The volume percentage is the area fraction of the two.

[0072] Throughout this disclosure, the amount of phase in a microstructure is given in volume % (vol%). It should be appreciated that in the art, a certain volume percentage is usually determined by considering the area percentage of the relevant constituent components (phases) in the sample, which is considered to correspond to the volume percentage.

[0073] The balance of the present welded duplex stainless steel material is iron (Fe) and unavoidable impurities. The unavoidable impurities are elements that are not intentionally added but may be in the steel of the present invention due to scrap and / or manufacturing processes used to obtain the duplex stainless steel. Examples of these elements include, but are not limited to, Co, V, Ti, Al, Nb, Pb, and Sn. The total content of these elements is less than 0.5 wt%. Cerium (Ce) may also be present as an impurity, but Ce cannot be greater than 0.07 wt% as this can cause problems during welding because the cathode bright spot movement caused by Ce / O formation can interfere with the welding arc.

[0074] In addition, the present welding material may optionally contain alloying elements added to improve the manufacturing process. Examples of alloying elements for improving the manufacturing process include, but are not limited to, magnesium (Mg), calcium (Ca) and boron (B). These elements may be added alone or in combination, and the content of these elements is less than 0.50% by weight in total.

[0075] Other impurity elements not discussed above may be present in amounts less than 0.1 wt %, and in a total amount less than 0.5%.

[0076] Furthermore, the present welded duplex stainless steel material may comprise or consist of the alloying elements mentioned herein within any ranges of the specific elements mentioned herein and meeting the requirements mentioned herein.

[0077] According to an embodiment, the welded duplex stainless steel material is in the form of welding wire or welding powder.

[0078] The present welded duplex stainless steel material as defined above or below may be manufactured in a method comprising the steps of:

[0079] - melting the raw materials, which can be performed by a high-frequency induction furnace or an electric arc furnace;

[0080] - Casting;

[0081] - optionally solution annealing in a temperature range of 1000°C to 1150°C followed by quenching in water;

[0082] - hot working, which can be carried out by forging and / or rolling and / or extrusion;

[0083] - optionally solution annealing in the temperature range of 1000°C to 1150°C followed by quenching in water; and

[0084] - Cold working, which may be performed by drawing or rolling.

[0085] If a powder is to be produced, conventional powder production procedures are used after melting.

[0086] The present disclosure also relates to a welded joint. The welded joint is obtained by the following method comprising the following steps:

[0087] - providing a welded duplex stainless steel material as defined above or below, said material being provided in the form of, for example, wire or strip;

[0088] - providing at least one substrate to be welded, for example, but not limited to, a duplex stainless steel in the form of a tube, such as the one sold under the trade name SAF TM 2507 and SAF TM 2906 Materials sold;

[0089] - applying the welded duplex stainless steel material to and / or onto the substrate;

[0090] - Applying shielding gas or flux powder to the area where a solder joint is to be obtained;

[0091] - Welding the base material and the duplex stainless steel material together by using tungsten inert gas or metal inert gas / metal active gas or submerged arc welding or electroslag welding.

[0092] If the weld joint is a multi-pass joint, applying the weld duplex stainless steel material will occur multiple times. The weld material is allowed to cool before a new layer of weld material is applied.

[0093] The present disclosure is further described by the following non-limiting examples.

[0094] Example

[0095] Two materials (heat) were formed, and their chemical compositions are shown in Table 2.

[0096] The material is formed by melting raw materials and scrap using an induction furnace.

[0097] The melt is poured, the casting is solution annealed at a temperature in the range of 1000°C to 1100°C for about 0.5 hour to 2 hours, and then quenched in water. The resulting billet is hot rolled and then drawn into wire. The resulting wire is then welded to a substrate of a duplex stainless steel material of similar composition using TIG and a shielding gas consisting essentially of argon and nitrogen.

[0098] Samples were obtained from the welded joints by cutting and milling and the obtained samples were tested as follows:

[0099] - Rp0.2 measured at room temperature using standard ISO 6892-1,

[0100] - Impact toughness was measured by measuring Charpy V at room temperature and at -46°C,

[0101] - Ferrite content measurement using LOM (image analysis, 500x magnification),

[0102] - Image analysis to measure the area fractions of different phases,

[0103] - Measurement of intermetallic phases using LOM (image analysis, 500x magnification), see Figure 1 and Figure 2 .

[0104] During visual analysis, no intermetallic (undesired nitride) particles were seen in the LOM images.

[0105] The test results are shown in Table 1. From the results, it can be seen that the welded duplex stainless steel provides a welded joint with high mechanical strength, no intermetallic phase and good impact toughness. PRE indicates high corrosion resistance.

[0106]

[0107]

Claims

1. A welded duplex stainless steel material, comprising the following alloying elements in weight %: C Max 0.030 Si Max 0.50 Mn 0.50 to 2.50 P max 0.030 S Max 0.030 Cr 29.0 to 32.0 Ni 7.0 to 11.0 Mo 0.50 to 1.50 W 3.00 to 4.50 Cu Max 0.50 N 0.25 to 0.45 Fe and unavoidable impurities balance And the ferrite:austenite content is 35:65 to 65:35 by volume.

2. The welded duplex stainless steel material according to claim 1, wherein PRE≥43, wherein PRE is calculated by the following formula: [Cr]+3.3×([Mo]+0.5×[W])+16×[N], wherein the value of the alloying element is in weight %.

3. The welded duplex stainless steel material according to any one of the preceding claims, wherein the Cr content is in the range of 29.5 wt. % to 32.0 wt. %.

4. The welded duplex stainless steel material according to any one of the preceding claims, wherein the content of Mn is in the range of 0.50 wt. % to 1.00 wt. %.

5. Welded duplex stainless steel material according to any one of the preceding claims, wherein the Si content is in the range of 0.10 wt. % to 0.30 wt. %.

6. The welded duplex stainless steel material according to any one of the preceding claims, wherein the content of W is in the range of 3.00 wt. % to 4.00 wt. %.

7. Welded duplex stainless steel material according to any one of the preceding claims, wherein the N content is in the range of 0.25 wt. % to 0.40 wt. %.

8. Welded duplex stainless steel material according to any one of the preceding claims, wherein the N content is in the range of 0.25 wt. % to 0.35 wt. %.

9. Welded duplex stainless steel material according to any one of the preceding claims, wherein the ferrite:austenite content is in the range of 48 to 55:52 to 45 by volume.

10. Welded duplex stainless steel material according to any one of the preceding claims, wherein the weld material has an Rp0.2 of at least 700 MPa, measured according to ISO 6892-1 at room temperature.

11. Use of a welded duplex stainless steel material according to any one of claims 1 to 10 for obtaining a welded joint.

12. A method of manufacturing a welded joint comprising a welded duplex stainless steel material as defined in any one of claims 1 to 10, wherein the method is a multi-pass welding method or a single-pass welding method.

13. The method according to claim 12, wherein the Rp0.2 of the obtained weld joint is at least 700 MPa, measured according to ISO 6892-1 at room temperature.

14. The method according to any one of claims 12 or 13, wherein the impact toughness of the obtained weld joint is at least 40 J or 50 J, measured according to ISO 148-1 at -46°C.

15. The method according to any one of claims 12 to 14, wherein the method comprises the following steps: - Providing a welded duplex stainless steel material according to any one of claims 1 to 10; - Provide at least one base material to be welded; - applying the welded duplex stainless steel material to and / or onto the substrate; - Applying shielding gas or flux powder to the area where a solder joint is to be obtained; - Welding the base material and the duplex stainless steel material together by using tungsten inert gas or metal inert gas / metal active gas or submerged arc welding or electroslag welding.

Citation Information

Cited By

  • Duplex stainless steel metal type flux-cored wire and method for 3D printing flange structural component

    CN119635067A