Processing of mining feedstock with kinetic comminution and separation

Through the combination of kinetic crushing and chemical additives, the problem of low extraction efficiency of valuable components in mining material processing is solved, efficient size reduction and component separation is achieved, and processing efficiency and output is improved.

CN118984881APending Publication Date: 2024-11-19TORKES POWER CRUSHER CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202380032492.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-02-25
Filing Date
2023-02-24
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The prior art is difficult to efficiently extract valuable components in mining material processing, and there are challenges in size reduction and separation processes.

Method used

The mining raw materials are fed into the kinetic crusher using the kinetic crushing stage, crushed by the self-collision generated by the vortex, and mixed with chemical additives to selectively release valuable components, and then separate the valuable components rich in the extraction stage. and flows that consume valuable components.

Benefits of technology

It realizes efficient dimensional reduction of mining materials and extraction of valuable components, improves processing efficiency and output, and enhances the recycling capacity of valuable components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118984881A_ABST
    Figure CN118984881A_ABST
Patent Text Reader

Abstract

This document relates to the processing of mining materials, such as ores, rocks, minerals and aggregates, to separate valuable components. A method and system for extracting valuable components from a mining feedstock comprising geologic material is provided. The method may include subjecting a mining feedstock to a dynamic comminution stage, wherein the mining feedstock undergoes self-collisions generated by vortices within a dynamic comminutor to produce comminuted material; mixing the mining feedstock or comminuted material with a chemical additive configured to selectively release valuable components from the geological material; and subjecting the comminuted material to an extraction stage to produce a stream rich in the valuable components and a stream depleting the valuable components. Also provided are methods for producing a homogeneous mixture of geological material derived from mining feedstock and additives, as well as methods for mechanochemically processing feedstock.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The technical field generally relates to the processing of mined materials such as ores, rocks, minerals and aggregates to separate valuable components. Background Art

[0002] Various materials can be mined and processed to extract valuable components. Processing such mined raw materials can include size reduction and separation methods. Processing mined materials involves various challenges, and there is a need for technologies that overcome at least some of these challenges. Summary of the invention

[0003] Therefore, an object of the present invention is to solve the above-mentioned problems.

[0004] According to a general aspect, a method for extracting a valuable component from a mining material containing a geological material embedded with the valuable component is provided, the method comprising: subjecting the mining material to a kinetic comminution stage, wherein the mining material is fed into a kinetic pulverizer and subjected to self-collision generated by a vortex within the kinetic pulverizer to produce a comminuted material; mixing the mining material or the comminuted material with a chemical additive, wherein the chemical additive is configured to selectively release the valuable component from the geological material; and subjecting the comminuted material to an extraction stage to produce a stream enriched in the valuable component and a stream depleted in the valuable component.

[0005] In some embodiments, the chemical additive includes a cation source configured to perform an ion exchange with the valuable component.

[0006] In some embodiments, the chemical additive includes a salt compound.

[0007] In some embodiments, the chemical additive is selected from the group consisting of NaCl, PCl3, KCl, Na2SO4, K2SO4, MgSO4, CaSO4, NaNO3, KNO3, CaCl2, MgCl2, Ca(NO3)2 and Mg(NO3)2.

[0008] In some embodiments, the chemical additive is NaCl.

[0009] In some embodiments, the chemical additive is mixed with the mined feedstock simultaneously with or before the mined feedstock undergoes a kinetic comminution stage.

[0010] In some embodiments, the chemical additive is introduced directly into the kinetic pulverizer simultaneously with the mined feedstock and as a separate stream from the mined feedstock.

[0011] In some embodiments, the chemical additive is intimately mixed with the mined material to form part of the comminuted material.

[0012] In some embodiments, the chemical additive is mixed with the pulverized material after the mined feedstock has passed through a kinetic pulverization stage.

[0013] In some embodiments, the leachate is introduced into at least one of: a mined feedstock, a kinetic pulverizer, a pulverized material, and a chemical additive.

[0014] In some embodiments, the leachate is introduced into at least one of the chemical additive, the kinetic pulverizer, and the mined material at least one of simultaneously with and before the mined material undergoes a kinetic pulverization stage.

[0015] In some embodiments, the leachate is introduced directly into the kinetic pulverizer simultaneously with the mined material and as a separate leach stream from the mined material.

[0016] In some embodiments, the leachate is introduced after the mined feedstock has undergone a kinetic comminution stage to at least one of: a chemical additive and a comminution material.

[0017] In some embodiments, the extraction stage includes subjecting the comminuted stream to a passing stage.

[0018] In some embodiments, the leaching stage includes separating a stream enriched in the valuable component from a stream depleted in the valuable component.

[0019] In some embodiments, a mechanical screen is used to separate a stream enriched in valuable components from a stream depleted in valuable components.

[0020] In some embodiments, the mechanical screen is a rotary screen.

[0021] In some embodiments, the mechanical screen is a trommel screen.

[0022] In some embodiments, the mechanical screen is a vibrating screen.

[0023] In some embodiments, the mechanical screen is a rotary screen.

[0024] In some embodiments, the mechanical screen is a high frequency screen.

[0025] In some embodiments, the mechanical screen is a sorting device.

[0026] In some embodiments, the classification device is an air classifier.

[0027] In some embodiments, the classification device is a hydrocyclone.

[0028] In some embodiments, a filter is utilized to separate a stream enriched in the valuable component from a stream depleted in the valuable component.

[0029] In some embodiments, the method further comprises agitating the mixture of the comminuted material and the chemical additive with a leachate to produce a stream enriched with the valuable component.

[0030] In some embodiments, the stirring comprises stirring at a temperature between 60°C and 100°C.

[0031] In some embodiments, the stirring comprises stirring between 800 rpm and 1200 rpm.

[0032] In some embodiments, the stirring comprises stirring for at least 10 minutes.

[0033] In some embodiments, the extraction stage further comprises subjecting the valuable component-rich stream to a recovery stage to recover the valuable component.

[0034] In some embodiments, the kinetic pulverization stage is performed in an inert environment.

[0035] In some embodiments, the chemical additives are mixed with the mined or crushed material in an inert environment.

[0036] In some embodiments, the inert environment substantially comprises an oxygen-deficient environment.

[0037] In some embodiments, the inert environment includes nitrogen.

[0038] In some embodiments, the mining feedstock includes at least one of ore, rock, mineral, slag, clinker, petroleum coke, clay mineral, and soil mineral.

[0039] In some embodiments, the valuable component includes at least one of lithium, sodium, potassium, aluminum, silicon, magnesium, calcium, iron, nickel, and oxygen.

[0040] In some embodiments, the valuable component includes graphene.

[0041] In some embodiments, the valuable components include rare earth minerals.

[0042] In some embodiments, the rare earth mineral includes at least one of neodymium, yttrium, cerium, scandium, lanthanum, praseodymium, promethium, samarium, europium, gadolinium, terbium, dysprosium, holmium, erbium, thulium, ytterbium, and lutetium.

[0043] In some embodiments, the mined feedstock includes lithium-rich clay minerals.

[0044] In some embodiments, the valuable component is lithium.

[0045] In some embodiments, the mined feedstock includes material having a size less than 12 inches.

[0046] In some embodiments, the mined feedstock includes material having a size less than 6 inches.

[0047] In some embodiments, the mined feedstock includes material having a size between about 1 inch and about 4 inches.

[0048] In some embodiments, the kinetic pulverizer is operated at a speed between 500 RPM and 1500 RPM.

[0049] In some embodiments, the kinetic pulverizer is operated at a speed between 700 RPM and 1000 RPM.

[0050] In some embodiments, the kinetic pulverizer is operated such that the pulverized material is substantially sand or silt sized particles.

[0051] In some embodiments, the kinetic pulverizer is operated such that the pulverized material is substantially micron-sized particles.

[0052] In some embodiments, the kinetic pulverizer is operated such that the pulverized material is substantially sub-micron sized particles.

[0053] In some embodiments, the mined feedstock has a moisture content of between 10% and 50% upon entering the kinetic pulverizer.

[0054] In some embodiments, the mined feedstock has a moisture content of between 15% and 40% upon entering the kinetic pulverizer.

[0055] In some embodiments, the pulverized material is a homogeneous mixture in the pulverized output stream.

[0056] In some embodiments, the method further comprises introducing a friable additive into the mined material, whereby the friable additive is reduced in size and uniformly mixed with the mined material to form a portion of the comminuted material.

[0057] In some embodiments, the friable additive and the chemical additive are pulverized and uniformly mixed with the mined material simultaneously in a kinetic pulverizer.

[0058] In some embodiments, a friable additive is introduced into the mined feedstock upstream of the kinetic comminution stage.

[0059] In some embodiments, the friable additive is introduced directly into the kinetic pulverizer as a friable stream separate from the mined feedstock.

[0060] In some embodiments, the method further comprises subjecting the mined feedstock to a pre-treatment stage prior to the kinetic comminution stage.

[0061] In some embodiments, the pre-processing stage is a magnetic separation stage that separates ferrous material from the mined material before it passes through the kinetic comminution stage.

[0062] In some embodiments, the magnetic separation stage is performed by one or more magnetic separators configured relative to the feed of mined material.

[0063] In some embodiments, the pre-treatment stage comprises at least one of: a coarse screening stage, a chemical addition stage, a drying stage, and a fragment separation stage.

[0064] In some embodiments, the method further comprises subjecting the shredded material to a post-processing stage.

[0065] In some embodiments, the post-processing stage includes at least one of: a chemical addition stage, a heating stage, a fragment separation stage, an electrostatic separation stage, a dust collection stage, and a secondary size reduction stage.

[0066] In some embodiments, the dust collection stage includes recovering a dust portion therefrom and producing a dust-reduced pulverized stream.

[0067] In some embodiments, the dust-reduced pulverized stream passes through an extraction stage, and optionally, a dust fraction is also recovered and sent to the extraction stage.

[0068] In some embodiments, the electrostatic separation stage comprises electrostatically separating the particulate material from the comminuted material.

[0069] In some embodiments, the secondary size reduction stage includes passing the shredded material into a size reducer.

[0070] In some embodiments, the size reduction machine comprises at least one of a ball mill, an oscillating motion mill, a hammer mill, a high shear energy mill, a vibrating mill, an attritor, a crusher, and a grinder.

[0071] In some embodiments, the fragment separation stage comprises flotation separation of the comminuted material.

[0072] In some embodiments, the method further comprises: monitoring at least one of: at least one feed parameter of the mined material; and at least one output parameter of the comminuted material; and adjusting the kinetic comminution stage based on at least one of: the at least one feed parameter and the at least one output parameter.

[0073] In some embodiments, the at least one feed parameter includes at least one of a feed rate of the mined feedstock, a moisture content of the mined feedstock, and a composition of the mined feedstock.

[0074] In some embodiments, the at least one output parameter includes at least one of: size characteristics of the pulverized material, composition of the pulverized material, moisture content of the pulverized material, flow rate of the pulverized material, and composition of the pulverized material.

[0075] In some embodiments, adjustment of the kinetic pulverization stage comprises adjusting the rotational speed of the kinetic pulverizer.

[0076] In some embodiments, regulation of the kinetic pulverizing stage includes regulating a feed rate of the mined material into the kinetic pulverizer.

[0077] According to another aspect, a method for producing a pulverized material comprising a homogeneous mixture of geological material and additives from a mining raw material is provided, comprising: providing a mining raw material comprising the geological material; mixing the additive with the mining raw material; subjecting the mining raw material to a kinetic comminution stage, wherein the mining raw material is fed into a kinetic pulverizer and undergoes self-collision generated by a vortex within the kinetic pulverizer to produce a homogeneous mixture of the geological material and the additive; and removing the homogeneous mixture from the kinetic pulverizer; wherein the additive is mixed with the mining raw material simultaneously with or before the kinetic comminution stage.

[0078] In some embodiments, additives are introduced into the mined feedstock upstream of the kinetic comminution stage.

[0079] In some embodiments, the additive is introduced directly into the kinetic pulverizer as an additive stream separate from the mined feedstock.

[0080] In some embodiments, the method further comprises mixing a friable additive with the mined feedstock simultaneously with or prior to the kinetic comminution stage to reduce size and homogenize with the geological material.

[0081] In some embodiments, the friable additive is introduced into the mined feedstock upstream of the kinetic comminution stage.

[0082] In some embodiments, the friable additive is introduced directly into the kinetic pulverizer as a friable stream separate from the mined feedstock.

[0083] In some embodiments, the method further comprises subjecting the mined material to a magnetic separation stage prior to the kinetic comminution stage to remove ferrous metals therefrom and produce a metal-depleted feed stream that is fed to the kinetic comminution stage.

[0084] In some embodiments, magnetic separation is performed by one or more magnetic separators configured relative to the feed of the mined material.

[0085] In some embodiments, the method further comprises passing the pulverized material through a dust collection stage to recover a dust portion therefrom and produce a dust-reduced pulverized stream.

[0086] In some embodiments, at least a portion of the dust fraction is combined with at least a portion of the dust-reduced pulverized stream.

[0087] In some embodiments, all dust fractions are combined with a dust-reduced comminution stream.

[0088] In some embodiments, the dust-reduced pulverized stream, the dust portion, or both are subjected to an extraction stage to extract at least one valuable component therefrom.

[0089] In some embodiments, the dust collection stage includes: a dust collector, which is connected to the outlet of the kinetic comminution stage, or to a solid conveying device, which is configured to convey the comminuted material out of the kinetic comminution stage; and a dust recovery unit, which is connected to the dust collector and configured to separate the dust portion and convey the dust portion from the dust collector to a storage container.

[0090] In some embodiments, the dust collector includes a settling chamber.

[0091] In some embodiments, the dust recovery unit includes a bag filter in fluid communication with the settling chamber via a conduit.

[0092] In some embodiments, the dust recovery unit includes a cyclone separator in fluid communication with the settling chamber via a conduit.

[0093] In some embodiments, the solid transport device comprises a conveyor.

[0094] In some embodiments, the dust collector surrounds the solids conveying device along a majority of the length of the solids conveying device.

[0095] In some embodiments, the geological material is clinker.

[0096] In some embodiments, the additive is gypsum.

[0097] According to another aspect, a system is provided, comprising: a kinetic pulverizer configured to receive and process mining raw materials including geological materials to produce pulverized material; a processing unit for processing the mining raw materials, the pulverized material and / or material within the kinetic pulverizer, the processing unit being configured to: add chemical additives, leachate and / or friable additives; pre-treat the mining raw materials; and / or post-treat the pulverized material; a pulverizer conveyor system configured to transport the pulverized material downstream; and an extraction unit configured to receive the pulverized material from the pulverizer conveyor system and extract valuable components therefrom.

[0098] In some embodiments, the processing unit is a chemical addition unit configured to add a chemical additive to at least one of the mined material and the comminuted material.

[0099] In some embodiments, the extraction unit comprises: a leaching unit configured to receive a pulverized material, add a leachate to the pulverized material and produce a leachate comprising valuable components and a solids-rich depleted (valuable components) material; and a recovery unit configured to receive the leachate from the leaching unit and produce a valuable component product and a leachate depleted (valuable components), which can be optionally recycled back to the leaching unit.

[0100] In some embodiments, the recovery unit is configured to cause crystallization of valuable components in the leachate.

[0101] In some embodiments, the depleted leachate is treated and recycled back to the leaching unit.

[0102] In some embodiments, the recovery unit further comprises a screen to remove valuable components in solid form from the leachate.

[0103] In some embodiments, the kinetic pulverizer is configured to operate at a speed between 500 RPM and 1500 RPM.

[0104] In some embodiments, the kinetic pulverizer is configured to operate at a speed between 700 RPM and 1000 RPM.

[0105] In some embodiments, the system further comprises: a monitoring unit configured to monitor at least one of: at least one feed parameter of the mined material; and at least one output parameter of the crushed material; and a control unit coupled to the monitoring unit and configured to adjust the kinetic crusher based on at least one of: the feed parameter and the output parameter.

[0106] In some embodiments, the monitoring unit and the control unit are configured such that the at least one feed parameter comprises at least one of: a feed rate of the mining material, a moisture content of the mining material, a composition of the mining material, and a feed rate of at least one unit.

[0107] In some embodiments, the control unit is configured to adjust the rotation speed of the kinetic pulverizer.

[0108] In some embodiments, the control unit is configured to regulate a feed rate of the mined material into the kinetic pulverizer.

[0109] In some embodiments, the processing unit includes a magnetic separator for pre-processing to remove ferrous metals from the mined material and produce a metal-depleted feed stream that is fed to a kinetic pulverizer.

[0110] In some embodiments, the processing unit comprises a dust collection unit for post-processing to recover dust fractions from the pulverized material and to produce a dust-reduced pulverized stream.

[0111] In some embodiments, the dust collection unit includes: a dust collector coupled relative to an outlet of the kinetic pulverizer or relative to a pulverizer conveyor; and a dust recovery unit coupled to the dust collector and configured to separate dust and transport the dust portion from the dust collector to a storage container.

[0112] In some embodiments, the dust collector includes a settling chamber.

[0113] In some embodiments, the dust recovery unit includes a bag filter in fluid communication with the settling chamber via a conduit.

[0114] In some embodiments, the dust recovery unit includes a cyclone separator in fluid communication with the settling chamber via a conduit.

[0115] In some embodiments, a dust collector surrounds the shredder conveyor system along a majority of its length.

[0116] In some embodiments, the system further comprises an inerting system operatively coupled to at least one of: the kinetic pulverizer, the pulverizer conveyor system, the processing unit, and the extraction unit.

[0117] In some embodiments, the inerting system is configured to provide anoxic conditions.

[0118] In some embodiments, the inerting system is configured to provide nitrogen for inerting.

[0119] According to another aspect, a method for mechanochemically processing raw materials is provided, comprising: providing a mined raw material comprising the raw material; and subjecting the mined raw material to a kinetic comminution stage, wherein the mined raw material is fed into a kinetic pulverizer and undergoes self-collision generated by a vortex within the kinetic pulverizer to produce a pulverized material, and the kinetic pulverizer is operated to convert the raw material into a mechanochemically modified material; removing the pulverized material from the kinetic pulverizer, wherein the pulverized material comprises the mechanochemically modified material and a size-reduced matrix portion; and separating the mechanochemically modified material from the size-reduced matrix portion.

[0120] In some embodiments, the mechanochemically modified material includes metal nanoparticles, catalysts, magnets, γ-graphene, metal iodates, nickel-vanadium carbide, and molybdenum-vanadium carbide nanocomposite powders.

[0121] In some embodiments, the mined feedstock includes clay minerals which, upon comminution, form part of the size-reduced matrix portion.

[0122] According to another aspect, a method for extracting valuable components from a mining material is provided, the method comprising: subjecting the mining material to a kinetic pulverizing stage, wherein the mining material is fed into a kinetic pulverizer and subjected to self-collision generated by a vortex within the kinetic pulverizer to produce a pulverized material; and extracting the released valuable components from the pulverized material with a leachate.

[0123] According to another aspect, a method for extracting valuable components from a mined material is provided, the method comprising: subjecting the mined material to a kinetic pulverizing stage, wherein the mined material is fed into a kinetic pulverizer and undergoes self-collision generated by a vortex within the kinetic pulverizer to produce a pulverized material; contacting at least one of the mined material and the pulverized material with a chemical additive to selectively release the valuable components from a size-reduced matrix material; and separating the released valuable components from the size-reduced matrix material of the pulverized material.

[0124] In some embodiments, the kinetic comminution stage is a single kinetic comminution stage.

[0125] In some embodiments, the kinetic comminution stage is a multi-pass kinetic comminution stage, wherein the comminuted material undergoes a second comminution stage in the kinetic pulverizer or in a second kinetic pulverizer.

[0126] In some embodiments, the method further comprises subjecting the shredded material to a secondary size reduction stage to produce an oversized material.

[0127] In some embodiments, the secondary size reduction stage includes placing the shredded material in a secondary size reducer.

[0128] In some embodiments, the size reduction machine comprises at least one of a ball mill, an oscillating motion mill, a hammer mill, a high shear energy mill, a vibrating mill, an attritor, a crusher, and a grinder.

[0129] In some embodiments, the chemical additive is contacted with the mined feedstock simultaneously with or before the mined feedstock undergoes a kinetic comminution stage.

[0130] In some embodiments, contacting at least one of the mining feedstock and the crushed material with the chemical additive comprises at least one of: introducing the chemical additive directly into a kinetic pulverizer simultaneously with the mining feedstock and as a separate stream from the mining feedstock; uniformly mixing the chemical additive with the mining feedstock to form a portion of the crushed material; and mixing the chemical additive with the crushed material after the mining feedstock has undergone a kinetic pulverization stage.

[0131] In some embodiments, the method further comprises agitating the mixture of the comminuted material and the chemical additive with a leachate to produce a stream enriched with the valuable component.

[0132] In some embodiments, separating the released valuable components from the size-reduced matrix material comprises subjecting the size-reduced matrix material to a recovery stage to recover the valuable components.

[0133] In some embodiments, the method further comprises subjecting the mined feedstock to a pre-treatment stage prior to the kinetic comminution stage.

[0134] In some embodiments, the pre-treatment stage comprises at least one of: a coarse screening stage, a chemical addition stage, a drying stage, a fragment separation stage, and a magnetic separation stage.

[0135] In some embodiments, the method further comprises subjecting the shredded material to a post-processing stage.

[0136] In some embodiments, the post-processing stage includes at least one of: a chemical addition stage, a heating stage, a debris separation stage, an electrostatic separation stage, and a dust collection stage.

[0137] In some embodiments, the fragment separation stage comprises flotation separation of the comminuted material. BRIEF DESCRIPTION OF THE DRAWINGS

[0138] Figure 1 is a flow chart of a method for extracting valuable components from mined raw materials, including a kinetic comminution stage.

[0139] Figure 2 It is a flow chart of a method for extracting valuable components from mined raw materials, including a pretreatment stage, a kinetic comminution stage, a post-treatment stage and an extraction stage.

[0140] Figure 3A is a flow chart of a method for extracting valuable components from mined raw materials, including a kinetic comminution stage.

[0141] Figure 3B is a flow chart of a method of reducing the size of mined raw materials and uniformly mixing them with additives to manufacture the final product.

[0142] Figure 3C is a flow diagram of a process for reducing the size of mined raw material and producing a raw material stream comprising the raw material, including a kinetic comminution stage.

[0143] Figure 4 is a left side perspective view of a pulverizing apparatus according to an embodiment, showing a motor and a housing of the pulverizing apparatus.

[0144] Figure 5 yes Figure 2 A right side perspective view of the comminution apparatus is shown, illustrating the outlet port near the bottom end of the housing.

[0145] Figure 6 yes Figure 2A bottom perspective view of a comminution apparatus is shown illustrating a belt connection connecting the motor and the rotatable shaft.

[0146] Figure 7 yes Figure 5 A cross-sectional view of the housing is shown, illustrating the rotatable shaft and rotor within the housing.

[0147] Figure 8 yes Figure 4 A partially exploded view of the housing of the comminution device is shown.

[0148] Fig. 9 yes Figure 4 A top cross-sectional view of a housing of a comminution apparatus is shown illustrating a plurality of deflectors spaced about a rotatable shaft along a side wall of the housing.

[0149] Fig.10 yes Figure 7 A cross-sectional view of the housing is shown with the rotatable shaft and rotor removed, illustrating shelves arranged at different heights along the side walls within the housing.

[0150] Fig.11 Is installed in Figure 4 A partial cross-sectional view of a pulverizing rotor within a housing of a pulverizing apparatus is shown, illustrating the vortex generated within the housing.

[0151] Fig.12 is a schematic top view of a housing showing overlapping vortices within an interior chamber of the housing according to one embodiment.

[0152] Fig.13 is a schematic diagram of a kinetic pulverizer system including a plurality of units for processing mined material.

[0153] Fig.14 is a flow diagram of a method for processing mining raw materials including geological materials, which uses kinetic crushing followed by screening and also includes a magnetic separation stage and a dust collection stage.

[0154] Fig.15 is a flow diagram of a method for processing mining raw materials including geological materials using kinetic crushing followed by screening and also including a dust collection stage.

[0155] Fig.16 is a side view schematic of an example magnetic separation stage.

[0156] Fig.17 is a schematic side view of another example of a magnetic separation stage. DETAILED DESCRIPTION

[0157] Processing and extraction of valuable components from mined raw materials can be enhanced by using a kinetic pulverizing stage to promote size reduction of the mined raw materials. The kinetic pulverizing stage can be a single shot, where the feed material is passed through a kinetic pulverizer to produce a pulverized output stream, which is then processed downstream to extract valuable components. In some embodiments, the pulverized output stream can be sorted by size, with larger particle sizes optionally reintroduced into the kinetic pulverizing stage, and smaller sized materials subjected to extraction processing to recover valuable components. The material can also be passed through one or more kinetic pulverizers multiple times. The high-energy self-collision mechanism of kinetic pulverization can cause raw material chunks and particles to collide, thereby promoting efficient size reduction and energy input, which is significantly greater than conventional mills, and the pulverized material produced has characteristics including a particle size distribution suitable for subsequent extraction of valuable components.

[0158] In one example, the mining feedstock is a lithium-bearing clay ore which is subjected to a kinetic comminution stage followed by extraction of lithium from the reduced size comminuted material. The extraction may include a leaching stage using acid or water to produce a lithium-rich leachate which is then subjected to lithium recovery to produce a lithium product. Lithium may be extracted from the comminuted material using a variety of extraction methods.

[0159] However, it is noted that a variety of mined raw materials can be kinetically pulverized and then a customized extraction method can be adopted depending on the valuable components of interest, the properties of the raw material matrix and processing design considerations. The kinetic pulverization stage can be operated to facilitate efficient energy input, rapid and efficient size reduction, mechanochemical processing of the mined raw materials, and enhanced extraction of the resulting pulverized material. It is noted that the technology described herein can be used in conjunction with the methods and systems described in the patent application disclosed as WO2021138345, which is incorporated herein by reference. For example, the kinetic pulverizer described herein can be used to process clay minerals in place of the size reduction and / or grinding unit described in WO2021138345, or in addition to the size reduction and / or grinding unit described in WO2021138345.

[0160] Reference now Figure 1, the mined raw material 10 from the mining operation 12 is provided to a kinetic pulverizer 16 to undergo a kinetic pulverization stage 13, thereby producing a pulverized output material 18. The pulverized output material 18 may then be further treated and processed, as will be described in detail below. Typically, at least a portion of the pulverized output material 18 is passed through an extraction stage 20 to recover one or more valuable components 22 present in a stream rich in valuable components and waste materials 24 in a stream depleted of valuable components. In some embodiments, the waste materials 24 may include gangue materials. The extraction stage 20 may include various steps and treatments, depending on the nature of the raw material and the components to be extracted. In some embodiments, the extraction stage 20 may include a leaching stage 26, wherein a leachate 27 is added to the pulverized material 18 to produce a leachate 28 rich in the target component, followed by a recovery stage 30, wherein the leachate 28 is processed to recover the valuable components 22 from the liquid, which may be recycled as the leachate 27.

[0161] Go to Figure 2 , relative to the kinetic pulverizing stage 13, the method may also include one or more pre-processing stages 32 and one or more post-processing stages 34. For example, the pre-processing stage 32 may include a coarse sizing stage (e.g., using a crusher), a chemical addition stage, a drying stage, and / or a fragment separation stage to produce a pre-processed raw material 36. When the raw mined material includes larger lumps, it may be necessary to perform a coarse sizing stage to quickly reduce the size of the larger lumps into smaller lumps that can be easily transported to the crusher by solid handling equipment (e.g., a conveyor). For example, the coarse sizing stage may include using a secondary size reduction machine (e.g., a crusher) to reduce the size of the mined raw material. In addition, the raw mined material may have fragments, such as wood or metal. Fragments with higher flexibility and lower brittleness may be removed because they may not be reduced in size and / or may not be expected in the main processing flow. In addition, fragments such as metal lumps may cause problems in the kinetic pulverizer and may therefore be removed upstream. This pre-separation may include one or more methods, such as magnetic separation, manual separation, and other techniques.

[0162] In terms of chemical addition, the mined raw material may be contacted with various additives designed to release the valuable components 22. If the raw material has a certain moisture content, the pre-treatment stage 32 may also include drying or dewatering. The dewatering stage may be applied to the raw material, which is initially in a paste or slurry state, such as a byproduct stream, to remove moisture and produce a solids-rich feed material that is fed to the KP 16. In a preferred embodiment, the moisture content of the mined raw material 10 does not exceed 50%, 40%, 30% or 20%. The feed material provided to the kinetic pulverizer may have a moisture content between 10% and 35%, and the moisture content may be controlled by adding water and / or drying the feed material depending on the initial moisture content of the feed material.

[0163] Still refer to Figure 2 The post-processing stage 34 may include a dust collection stage, a chemical addition stage, a heating stage, a fragment separation stage, and / or a secondary size reduction stage to produce a processed sized material 38 that is provided to the extraction stage 20. The dust collection stage is also Fig.13 and 14 The dust collection stage can be particularly useful for mining raw materials that are dry and prone to generating fine dust particles.

[0164] A fragmentation separation stage may be performed to remove larger materials, including oversized ores and / or non-ore materials, such as wood. The fragmentation separation stage may be performed using a screen, such as a vibrating screen, a drum screen, a rotary screen, a gyratory screen, or a high frequency screen. Oversized materials that do not contain the target valuable component may be preferentially removed as waste material 24 prior to extraction. In some embodiments, the fragmentation separation stage may include flotation separation or flotation processing. For example, when the pulverized output material 18 is a homogeneous output material and / or the size is effectively reduced, making mechanical screening based on size impractical or challenging, flotation separation or flotation processing may be used to separate or classify the reduced size particles in the pulverized output material 18 based on the density of the particles. For example, waste material 35 (e.g., gangue material) may be separated from material in the pulverized output material 18 containing the valuable component 22 to produce waste material 35 and processed screened oversized material 38.

[0165] Another potential post-processing stage 34 is a heating stage for preheating the pulverized output material 18 in preparation for the extraction stage 20, which is particularly useful for extraction methods that operate at higher temperatures. In addition, the post-processing stage can include chemical additions that can be tailored to the extraction method to be used. For example, the pulverized output material 18 can be contacted with various additives intended to release the valuable components 22.

[0166] The post-processing stage 34 may also include one or more secondary size reduction stages to further reduce or pulverize the pulverized output material 18 prior to the extraction stage 20. The secondary size reduction stage may be performed in a kinetic pulverizer 16, a secondary size reducer, or a combination of the two. For example, in some embodiments, the pulverized output material 18 may undergo a fragment separation stage to sort the material in the pulverized output material 18 according to size. Any oversized material (i.e., material that does not have the required particle size for the extraction process to be used on the mining raw material 10) may be separated into an oversized portion. The oversized portion may then undergo a secondary size reduction stage to reduce the size of the oversized portion to the particle size required for the extraction stage 20 and produce a processed oversized material 38. In some embodiments, the entire pulverized output material 18 may be processed with one or more secondary size reduction stages. Conventional size reduction machines may be used for the secondary size reduction stage, such as a ball mill, an oscillating motion mill, a hammer mill, a high shear energy mill, a vibrating mill, an ultrafine pulverizer, a crusher, a grinding mill, and the like. Alternatively, the oversize fraction and / or the pulverized material may undergo a secondary size reduction stage in the same kinetic pulverizer as the kinetic pulverization stage or in a second or series of kinetic pulverizers.

[0167] Now go to Figure 3A As described above, a chemical additive 40 may be used in the process upstream of the extraction stage 20. The chemical additive 40 may be selected based on various factors and provided in an amount relative to the primary process stream. Furthermore, the chemical additive 40 may be added in the pre-processing stage 32 before or during the kinetic pulverization stage 13, or in the post-processing stage 34 after the kinetic pulverization stage 13. The chemical additive 40 may be added to the mined feedstock 10 (see additive stream 40-B), to the kinetic pulverizer 16 (see additive stream 40-A), to the pulverized output material 18 before the post-processing stage 34 (see additive stream 40-C), to the secondary size reducer during the post-processing stage 34 of secondary size reduction (see additive stream 40-D), and / or to the oversized material 38 after the post-processing stage 34 (see additive stream 40-E).

[0168] The additive stream may be provided in a variety of forms, depending on the nature of the chemical, the primary process stream with which the chemical additive is contacted, and other factors. For example, the additive stream may be in the form of a particulate solid, liquid, slurry, or emulsion; and it may be sprayed, dripped, pumped, or gravity fed into the process. For example, the mining material 10 may be supplied to the kinetic pulverizer 16 by being provided as a solid material onto a feed conveyor, and the chemical additive 40 may be sprayed in liquid form on the top surface of the mining material 10 during conveyance, or may be added as a solid powder or granular material, deposited, or spread on top of the mining material 10. In such a case, the mining material 10 and the chemical additive 40 would be fed together into the kinetic pulverizer 16 for processing.

[0169] The mining raw material 10 may include one or more materials from geological sources and include one or more valuable components identified to be extracted. The valuable components may be embedded or otherwise retained in the matrix of the material. The mining raw material 10 may be raw mined material supplied directly from the mine, pre-processed mined material and / or a by-product of the mining process, such as oversized material from other separation processes. The mining raw material 10 may also be a mixture of several materials from different sources and having different properties. The processing parameters may be adjusted based on the properties of the matrix and the valuable components.

[0170] The mining raw material 10 may be obtained at the mining site where the kinetic pulverizer is located, or the mining raw material 10 may be obtained and transported to another site for use in the kinetic pulverization stage 13 and the extraction stage 20. The composition of the mining raw material 10 may vary and will depend on factors such as the type of mining operation, the type of ore mined, etc. For example, the mining raw material 10 may include ores, rocks, minerals, slag, clinker, petroleum coke, clay minerals, oversized streams, waste streams, and / or soil minerals generated in mining and extraction operations. Valuable components may include metals as well as other species.

[0171] In some embodiments, the valuable component 22 comprises lithium and the mining raw material 10 comprises a lithium-containing clay mineral. In this case, the lithium-containing clay mineral can be contacted with a cation source (e.g., NaCl) and then subjected to kinetic pulverization and then to a leaching stage 26 to obtain a lithium-rich leachate. In other cases, the valuable component is at least one metal in an ore having a clay-rich matrix and the mining raw material is processed in a similar manner, adding a cation source, kinetic pulverization, and leaching. The metal may be present in the ore, depending on the composition and crystal structure of the ore.

[0172] It is also noted that the mining raw material 10 can be obtained from various mining operations, such as coal mining, metal mining, non-metallic mining, oil sands mining, quarrying, etc. The mining raw material 10 generally includes hard, brittle, easily broken pieces, so kinetic crushing facilitates crushing and significant size reduction, converting the mining raw material into a crushed material that includes a size-reduced portion and a possible oversize portion. For example, if the mining raw material 10 includes non-brittle and / or flexible materials, these materials may not be reduced in size and may constitute an oversize portion in the crushed material removed from the crusher. If necessary, the oversize portion can be separated from the size-reduced portion by screening before extraction. The mining raw material may include mixed materials that include materials containing valuable components, but also include fragments or unwanted materials that can be processed by the KP16 and can be reduced in size or separated depending on the nature of the fragments. The versatility of the KP16 in the overall process of processing mining raw materials and extracting valuable components is significant because it can receive feeds of multiple types and mixtures.

[0173] In the kinetic pulverizer 16, the mined feedstock 10 may be reduced in size, such as to sand or silt sized particles, and may optionally be uniformly mixed with any additives added upstream. Thus, the pulverized output material 18 may include the reduced size portion and optionally one or more chemical additives 40. In some embodiments, the ultra-high impact energy of the kinetic pulverizer 16 produces a finer particle size than a conventional ball mill and imparts higher energy to the material, which may produce a mechanochemical effect. In other embodiments, the pulverized output material 18 may be further reduced in size in a secondary size reduction machine (e.g., a conventional ball mill).

[0174] In an example embodiment, the mining feedstock 10 includes metal-bearing minerals with a stable mineral structure, which makes it difficult to efficiently extract valuable metals. By kinetic pulverizing the metal-bearing mineral, mechanochemical activation can be introduced to activate the transformation of inert structures (e.g., MO coordination structures, where M is a metal, such as Li) in the presence of additives (e.g., potassium sulfate). This pulverization-induced mechanochemical activation can be followed by leaching using a dilute acid leachate to promote the separation of metals. Although mechanochemical processing has been used to activate minerals to enhance extraction in some cases, it generally involves a unique step of ball milling, which may have disadvantages. Kinetic pulverization provides very high energy collisions between particles of the material and can promote enhanced mechanochemical activation by utilizing the relative impact energy of particle collisions, which can be two to three orders of magnitude greater than the relative impact energy of large conventional ball mills used in large-scale mining. For example, as shown in Table 1 below, when the kinetic pulverizer 16 is operated at a speed between 850 and 1100 RPM, the maximum linear velocity during vortex collision can reach 41% to 54% of the speed of sound. By modifying the operating conditions (eg, rotational speed and chemical additions), the kinetic pulverizer can be operated to provide certain target levels of mechanochemical activation depending on the feed material.

[0175] In some embodiments, the kinetic pulverizer 16 can be operated to reduce the size of the feed material so that the pulverized material includes micron-sized and / or submicron-sized particles in the size-reduced portion, which in turn can provide a greater total surface area exposed to the chemical additive 40 and enhance the extraction stage 20. The performance enhancement of the extraction stage 20 can include increasing the total yield of valuable components recovered, improving efficiency, and / or increasing the throughput of the extraction process. In some embodiments, the kinetic pulverization stage 13 produces pulverized material 18 having particle size characteristics ranging from dust-sized particles to larger particles, wherein the majority (e.g., more than 50%, 55%, 60%, 65%, 70%, 75%, 80%, 85%, or 90%; or between 50% and 95%, between 60% and 90%, or between 65% and 85%) passes through a 3 / 8 inch screen. The particle size distribution can vary depending on the size and physical characteristics of the feed material and the processing speed of the kinetic pulverizer. It is also noted that the pulverized output stream may be screened to produce at least two fractions, with the larger fraction being recycled back to the feed and / or sent to a secondary size reduction device, and the smaller fraction being supplied to the extraction stage.

[0176] Once the mined material 10 is comminuted and optionally chemical additives 40 are mixed, valuable components may be extracted from the mixture in an extraction stage 20, which may include a leaching stage 26 using a leachate 27, such as Figure 12. The leaching stage 26 may include acid leaching, water leaching, solvent-assisted leaching or other types of leaching, depending on the materials involved. The leaching stage 26 may also be performed in conjunction with heat activation if desired. The leachate 28 may then be sent to a recovery stage 30, which recovers valuable components from the leachate 28. The recovery stage 30 may utilize a variety of methods, such as crystallization, purification, etc. It is noted that a target component may be obtained as the final product of the valuable component 22, or multiple components may be recovered from the leachate 28. For example, a first metal may be crystallized from a solution in the leachate 28 in a first recovery stage, and then the remaining liquid may be passed through a second recovery stage to recover a second metal.

[0177] The extraction stage 20 may include adding a leachate 27 in various ways. For example, the leachate 27 may be added to the feed and / or leach vessel at least partially separately from the pulverized material. In some embodiments, the extracted valuable components (e.g., metals such as Li) have been ion exchanged with a chemical additive 40 (e.g., a cation source that may be from NaCl) to produce a solute or aqueous solution with the leachate 27, although other mechanisms for releasing the valuable components may be used.

[0178] Valuable components may include various elements or compounds present in the mining raw materials. For example, in some embodiments, the valuable components may include lithium, sodium, potassium, aluminum, silicon, magnesium, calcium, iron, nickel, and / or oxygen. In other embodiments, the valuable components may include carbon-based compounds, such as graphene; or rare earth minerals, such as neodymium, yttrium, cerium, scandium, lanthanum, praseodymium, promethium, samarium, europium, gadolinium, terbium, dysprosium, holmium, erbium, thulium, ytterbium, and / or lutetium.

[0179] See also Figure 3A, the leachate 27 may be introduced directly into the feedstock 10 prior to the comminution stage 13 (stream 27-A). The leachate 27 and chemical additives 40 may be mixed simultaneously with the mined feedstock 10 prior to (stream 27-B) and / or after (stream 27-C) the comminution stage 13. In some embodiments, the leachate 27 may be introduced directly into the kinetic pulverizer 16 as a separate stream (stream 27-D), or mixed with the pulverized output material 18 after the kinetic pulverization stage 13 (stream 27-E). In some embodiments, the leachate 27 may be introduced during the post-processing stage 34 (stream 27-F), such as into a secondary size reducer, or mixed directly with the oversized material 38 prior to the extraction stage 20 (stream 27-G). In other words, the leachate 27 can be mixed with the feedstock 10 (see stream 27-A), mixed with the chemical additive 40 before being provided to the feedstock 10 (see stream 27-B) and / or mixed with the pulverized output stream 18 (see stream 27-C), directly enter the kinetic pulverizer 16 (see stream 27-D), mixed with the pulverized output stream 18 (see stream 27-E), directly enter the secondary processing device (see stream 27-F), and / or mixed with the processed oversized material 38 (see stream 27-G).

[0180] The leachate 27 may include a variety of liquids selected to extract valuable components from the matrix material of the pulverized material. The extraction mechanism may vary and may include dissolution of the components or dissolution of solutes facilitated by the interaction of the components with cations, for example, to form an enriched leachate solution. In some embodiments, the leachate 27 may include, consist essentially of, or consist of water, and the water-based leachate may include water obtained from a processing operation, a fresh water source, make-up water, recycled water from a recovery stage, etc. In some embodiments, when the leachate 27 is added to stream 27-A or stream 27-B (i.e., added prior to the kinetic pulverization stage 13), the leachate 27 may comprise from about 20% to about 25% by weight of the mixture. For example, for every 3 to 4 parts of mined feedstock 13, 1 part of water may be added to stream 27-A or 27-B. In other embodiments, for example when leachate 27 is added after the kinetic comminution stage in streams 27-E, 27-F, 27-G, a greater amount of leachate may be used, for example between 5% and 80% by weight, or between 20% and 25% by weight.

[0181] In some embodiments, when the leachate 27 is mixed with the chemical additive 40 before being introduced into the mining material 10 (stream 27-B) or the pulverized output stream 18 (stream 27-C), the chemical additive 40 solute dissolves in the leachate 27 to form an aqueous solution. When the chemical additive 40 in the chemical additive-solvent solution contacts and ion-exchanges with the valuable components 22 in the geological material, a valuable component-rich leachate 28 is produced. The valuable component-rich leachate 28 can then be isolated from the geological material in the mining material 10 by the extraction stage 20, which can include a leaching stage 26 to produce a valuable component-rich stream 29a and a valuable component-depleted stream 29b. The valuable component-rich stream 29a can then be subjected to a recovery stage 30 to isolate the valuable components 22.

[0182] The extraction stage 20 can be performed in one or more stages, and various separation equipment can be used. For example, the leachate 27 can be mixed in one or more of the streams 27-A to 27-G to leach a valuable component-rich leachate 28 from the geological material in the mining feedstock 10. In some embodiments, the leachate 27 can be mixed in all of the streams 27-A to 27-G. In some embodiments, the final solvent wash (e.g., at streams 27-E, 27-F, and / or 27-G) can include one or more stirring stages. The stirring stage can include stirring the mixture of the crushed output stream 18 or the treated oversized material 38, the chemical additive 40, and the leachate 27 to increase the release of the valuable component 22 into the valuable component-rich leachate 28. In some embodiments, the stirring can be performed at a temperature above room temperature, such as between about 60°C and about 100°C, or about 90°C. In some embodiments, stirring can be performed in a conventional stirrer, such as a mechanical stirrer or a magnetic stirrer, at a speed between about 800 rpm and about 1200 rpm, or about 1000 rpm, for at least 10 minutes.

[0183] To filter or leach the crushed output stream 18, various types of filters or screens can be used, such as liquid filter screens, vibrating screens, drum screens, rotary screens, gyratory screens, high-frequency screens, etc. In some embodiments, mechanical screening can be performed using classification equipment, such as a classifier that classifies materials according to their size, shape, and / or density, including but not limited to air classifiers and hydrocyclones. Other types of separation or filtering equipment can also be used. The valuable component-rich leachate 28 is separated or filtered from the geological material in the mining raw material 10, and the valuable component 22 can be isolated from the valuable component-rich leachate 28 in the recovery stage 30.

[0184] When the valuable components 22 are released from the geological material in the mining feedstock 10 using the chemical additive 40, the pulverizing output stream 18 may contain the geological material depleted of the valuable components 22 and the leachate 28 enriched in the valuable components. In some embodiments, the pulverizing output stream 18 may be subjected to an additional leaching stage 26 or agitation stage to separate the leachate 28 enriched in the valuable components from the geological material.

[0185] In some embodiments, the friable additive 17 may be introduced into the mined feedstock 10 simultaneously with the kinetic pulverization stage 13 (stream 17-A) or prior to the kinetic pulverization stage 13 (stream 17-B) such that the friable additive 17 is reduced in size and uniformly mixed with the geological material in the mined feedstock 10 to form part of the pulverized output stream 18. In some embodiments, the friable additive 17 may be introduced directly into the kinetic pulverizer 16 as a separate stream from the mined feedstock 10 (stream 17-A).

[0186] Thus, the mined feedstock 10 may be fed directly to the kinetic comminution stage 13 after being mixed with the chemical additive 40, the friable additive 17, and / or the leachate 27. The leachate 27 may be mixed with the mined feedstock 10 prior to the kinetic comminution stage 13 because the kinetic pulverizer 16 is capable of efficiently processing wet feed material. For example, the mined feedstock 10 may have a moisture content of up to 50% or between 10% and 40% and may be fed directly to the kinetic pulverizer 16 to produce a pulverized output stream 18 comprising the mined feedstock 10 and the leachate 27.

[0187] Reference now Figure 3B , the mining feedstock 10 containing the geological material can be reduced in size and uniformly mixed with the additive 15 to produce the final product 25 and the waste material 24. The mining feedstock 10 can be mixed with the additive 15 at the same time as the mining feedstock 10 is introduced into the kinetic pulverizer 16 (stream 15-A) or before the mining feedstock 10 is introduced into the kinetic pulverizer 16 (stream 15-B). In some embodiments, the additive 15 can be introduced directly into the kinetic pulverizer 16 as a separate stream from the mining feedstock 10 (stream 15-A). In this embodiment, the pulverized output stream 18 can include a uniform mixture of the pulverized geological material and the additive 15 in the mining feedstock 10. The kinetic pulverizer 16 greatly reduces the size of the geological material and uniformly mixes the mixture of the pulverized geological material and the additive 15.

[0188] In some embodiments, the shredder output stream 18 may undergo an extraction stage 20 to separate the final product 25 from waste material 24 (e.g., particles that are too large and / or too small) in the shredder output stream 18. During the extraction stage 20, one or more mechanical screens 21 may be provided to facilitate or maximize a high purity or high yield of the final product 25 of a particular desired size.

[0189] In some embodiments, the final product 25 may include a building material, such as a cement mixture. The cement mixture may be processed using a kinetic pulverizer 16 by pulverizing clinker as the mining raw material 10 and uniformly mixing it with gypsum as the additive 15. Thus, the kinetic pulverizer 16 may simultaneously pulverize and uniformly mix the clinker and gypsum mixture to produce a cement mixture final product. In some embodiments, the mining raw material 10 may be mixed with a friable additive 17 to assist in pulverizing and produce a homogenous final product 25 including the friable additive 17.

[0190] Reference now Figure 3C , a kinetic pulverizer 16 may be used to produce a raw material stream 120 comprising raw material. Mined raw material 10 comprising geological material is introduced into a kinetic pulverizer 16 to undergo a kinetic pulverization stage 13 to pulverize and reduce the size of the geological material, thereby producing a pulverized output stream 18 comprising a raw material portion and an impurity portion. The pulverized output stream 18 may then undergo an extraction stage 20 to produce a raw material stream 120 and an impurity stream 122. In some embodiments, the mined raw material 10 comprises coal. The pulverized coal material may then undergo an extraction stage 20 to isolate impurities and intermediates (i.e., an impurity stream 122) from the purified coal (i.e., the raw material stream 120). During the extraction stage 20, the impurity stream 122 may be separated from the raw material stream 120 based on size and / or weight. For example, when the mined raw material 10 comprises coal, the impurity stream 122 comprises impurities and intermediates. Since the impurities are generally heavier than the intermediates, which are heavier than the pure coal (i.e., the raw material stream 120), a gravity separator (e.g., a mineral jig, a heavy media bath, a wash table, a spiral separator, or a cyclone separator) can be used to separate the impurity stream 122 from the raw material stream 120. In some embodiments, flotation processing can be used to separate finer particles in the raw material stream 120 from the impurity stream 122. In some embodiments, the raw material stream 120 and / or the impurity stream 122 can be sorted and classified by size, where particle sizes larger than a desired value can be redirected to the kinetic pulverization stage 13.

[0191] In some embodiments, the mined raw material 10 may be mixed with additives 15 and / or friable additives 17 in either stream 15-A or 15B and streams 17-A and 17-B, respectively. In these embodiments, the pulverized output stream 18 will include a homogeneous mixture of pulverized geological material (which includes a raw material portion and an impurity portion) and additives 15 and / or friable additives 17.

[0192] In some embodiments, the kinetic pulverizer 16 may be used to mechanochemically process materials to produce products such as metal nanoparticles, catalysts, magnets, γ-graphene, metal iodates, nickel-vanadium carbide, and molybdenum-vanadium carbide nanocomposite powders.

[0193] With respect to the kinetic pulverizing stage 13, a single kinetic pulverizer 16 may be implemented and operated as a single kinetic pulverizing stage. For example, the mining material 10 and optional chemical additives 40, additives 15, friable additives 17, and / or leachate 27 may be fed into the upper portion of the kinetic pulverizer 16, which includes a drum with baffles and an internal rotating rod with multiple arms that create a vortex within the drum cavity. The mining material 10 is conveyed into the vortex and undergoes self-collision, thereby pulverizing and reducing the size of the geological material. The geological material is passed to the bottom area of ​​the kinetic pulverizer 16 and discharged as a pulverized output stream 18 through a lower outlet. The rotational speed may be operated between 500RPM and 1200RPM, between 500RPM and 1300RPM, between 500RPM and 1500RPM, between 600RPM and 1100RPM, or between 700RPM and 1000RPM, and may be adjusted or maintained relatively constant in response to other processing parameters.

[0194] In some embodiments, the rotational speed is adjusted to control the size and quality of the output material. As shown below in Table 1, when the kinetic pulverizer 16 is operated at a rotational speed of 850 to 1100 RPM, respectively, the maximum linear velocity at the pad end of the baffle can range between 71.1 and 92.1 m / s. It should be noted that these maximum linear velocities observed at the pad end and vortex collision of the kinetic pulverizer 16 depend on the size and internal geometry of the kinetic pulverizer being evaluated, and are therefore non-limiting. In some embodiments, the linear velocities at the pad end and vortex collision can be greater or less than the velocities observed in Table 1.

[0195] Table 1

[0196]

[0197] In addition to the targeted size reduction of the geological material by the kinetic pulverizing stage 13, the kinetic pulverizing stage 13 can also promote mechanochemical fragmentation of the geological material, and the kinetic pulverizer 16 provides additional energy to increase the selective release of the valuable components 22 when the chemical additive 40 is mixed with the mining feedstock 10 simultaneously with or before the kinetic pulverizing stage 13. For example, the chemical additive 40 can be a cation source, such as a salt compound, which is configured to exchange ions with the valuable components 22 to be isolated. In some embodiments, the chemical additive 40 can include a cation source, which includes cations and anions. In some embodiments, the cations in the cation source can include alkali metals and / or alkaline earth metals. The anions in the cation source can include halides, SO4 - and / or NO3 -In some embodiments, the cation source includes at least one of NaCl, PCl3, KCl, Na2SO4, K2SO4, MgSO4, CaSO4, NaNO3, KNO3, CaCl2, MgCl2, Ca(NO3)2, and Mg(NO3)2. The chemical additive 40 may be in dry and / or powder form and allows separation of valuable components 22 in aqueous solution from the leachate 27 after the kinetic pulverization stage 13. In some embodiments, the chemical additive 40 may be mixed in solution with the leachate 27 prior to introduction into the mined feedstock 10, the pulverization output stream 18, and / or the processed oversized material 38. Depending on the nature of the chemical additive and the method of introduction into the process stream, the chemical additive 40 may be added, for example, in dry form, as a solution, an emulsion, or a dispersion.

[0198] When the chemical additive 40 is introduced into the kinetic pulverizer 16 along with the mining material 10 containing the geological material, the energy from the kinetic pulverizer 16 can enhance the rate and extent of ion exchange between the cations in the chemical additive 40 and the valuable components 22 embedded or retained in the geological material in the mining material 10. In addition, when the kinetic pulverization stage 13 is carried out in an inert environment, such as nitrogen, the rate and extent of ion exchange between the cations in the chemical additive 40 and the valuable components 22 in the mining material 10 will be increased. The inert environment can be achieved by an inert chamber (not shown) that operably surrounds at least one of the following: the kinetic pulverizer 16, the pulverizer conveyor system operably connected to the kinetic pulverizer 16, and the screen used during the extraction stage 20. The inert environment can include an anoxic environment, i.e., an oxygen-free environment, i.e., an oxygen-free environment. In some embodiments, the inert environment can include, consist of, or consist essentially of nitrogen.

[0199] When the mining material 10 is introduced into the kinetic pulverizer 16, the kinetic pulverizing stage 13 can advantageously utilize kinetic energy, vortex, and material-material collisions to achieve size reduction of the geological material, uniform mixing of the pulverized output stream 18, release of valuable components 22 when the chemical additive 40 is introduced into the kinetic pulverizer 16, and / or mixing or uniform mixing of the chemical additive 40, other additives (such as additive 15 or friable additive 17) and / or leachate 27 that can be combined with the mining material 10.

[0200] Once the pulverized output stream 18 is discharged from the lower outlet, the pulverized output stream 18 can be further processed to separate particles of reduced size or to leach valuable components 22 from the geological material in the mining feedstock 10. For example, during the extraction stage 20, the geological material can be separated from the leachate 28 rich in valuable components using filtration or size-based separation techniques (e.g., screening). Screening can be performed using various types of mechanical screens, such as liquid filter screens, vibrating screens, drum screens, rotary screens, gyratory screens, high-frequency screens, etc. Alternatively, mechanical screening can be performed using classification equipment, such as a classifier that classifies materials according to their size, shape, and / or density, including but not limited to air classifiers and hydrocyclones. The mechanical screen can be constructed or operated based on the composition and size distribution of the pulverized output stream 18 to filter out the leachate 28 rich in valuable components from the pulverized geological material. In other embodiments, the screen can be operated to classify the pulverized output stream 18 into multiple size-based streams by size. For example, depending on the processed oversized product to be produced, the screen and kinetic pulverizer 16 may be operated and designed in certain ways to generate a product having a maximum or minimum size. However, it is noted that the screen design may be market driven to provide a variety of size distributions of size-reduced material.

[0201] In some embodiments, the extraction stage 20 and the pulverization stage 13 are coordinated so that the operation of one can affect the other. For example, the screen or filter and the kinetic pulverizer 16 can be monitored and controlled by the controller 226 to achieve desired parameters, such as the pulverized output stream 18, the extract 28 rich in valuable components, or certain characteristics of the final product 25. For example, if a change in the mining feedstock 10 causes the kinetic pulverizer 16 to produce a larger particle size fraction in the pulverized output stream 18, the kinetic pulverizer 16 can be controlled, such as by controlling the motor 228 to increase the speed, to bring the particle size back into a target range, for example, to a range that facilitates the desired release of the valuable components 22, or a desired range for the final product 25. A monitoring unit or instrument, such as an inlet detector D, can be provided. I 230 and exit detector D O 232 to monitor characteristics of the input and output streams, respectively, such as maximum or minimum size, size distribution, composition, quality, moisture content, and / or volumetric flow rate.

[0202] In some embodiments, a conveyor system is used to transport the various streams between stages to facilitate continuous operation, although other transport methods may be used. The process may be continuous, batch-fed, or operated according to other schemes depending on the facility and other factors.

[0203] With respect to the kinetic pulverizer 16, it is noted that the unit may have various structural and operational features. In some embodiments, the kinetic pulverizer may have one or more features as described in PCT / CA2019 / 050967, which is incorporated herein by reference.

[0204] Reference now Figures 4 to 11 , which shows a pulverizer 50 according to one embodiment. The pulverizer 50 is adapted to receive input material as described herein (eg, mined material 10) and pulverize or crush the input material.

[0205] In the illustrated embodiment, the pulverizer 50 includes a base 52 and a housing 60 mounted on the base 52. Specifically, the housing 60 includes a bottom end 62 connected to the base 52 and a top end 64 opposite the bottom end 62. The housing 60 is hollow and includes a housing side wall 66 extending between the top and bottom ends 64, 62 to define an internal chamber 68 where pulverization is performed. Specifically, the housing 60 includes an inlet 70 located at the top end 64 to receive input material and an outlet 72 located at the bottom end 62, through which the pulverized material can be discharged once it is pulverized in the internal chamber 66. In the illustrated embodiment, the outlet 72 allows the pulverized material to be discharged in a tangential direction of the housing side wall 66. It will be understood that the outlet 72 can be configured in different ways. For example, the outlet 72 can be located at the bottom surface of the housing 60 so that the pulverized material can be discharged axially downward from the housing 60. It will also be understood that, alternatively, the outlet 72 can be located substantially close to the bottom end 62, but can be located loosely at the bottom end 62 of the housing 60. Similarly, the inlet 70 may not be strictly located at the upper end 64 of the housing 60 , but may be located generally proximate to the upper end 64 .

[0206] In the illustrated embodiment, the housing 60 is generally cylindrical and defines a central housing axis H extending between top and bottom ends 64, 62 of the housing 60. The housing 60 is suitably arranged such that the central housing axis H extends substantially vertically when the pulverizer 50 is in operation. In this configuration, input material fed into the inlet 70 will eventually tend to fall toward the outlet 72 under the action of gravity.

[0207] In the illustrated embodiment, the airflow generator 100 includes a pulverizing rotor assembly disposed within the internal chamber 68 and a rotary actuator 104 operatively coupled to the pulverizing rotor assembly for rotating the pulverizing rotor assembly to generate an airflow. Specifically, the pulverizing rotor assembly includes a rotatable shaft 106 disposed within the internal chamber 68 and extending along the central housing axis H between the top and bottom ends 64, 62 of the housing 60, and a plurality of pulverizing rotors 108a, 108b, 108c, which are fixed to the rotatable shaft 106 so as to rotate around the central housing axis H when the rotatable shaft 106 rotates.

[0208] Each pulverizing rotor 108a, 108b, 108c includes a rotor hub and a plurality of rotor arms 122 extending outwardly from the rotor hub and toward the housing sidewall 66. The rotatable shaft 106 extends through the rotor hub so that the rotor arms 122 are disposed in a rotation plane that extends orthogonally through the central housing axis H. In this configuration, when the rotatable shaft 106 rotates, the rotor arms 122 are thus maintained in and move along the rotation plane. Alternatively, the rotor arms 122 may instead be tilted upward or downward relative to the rotatable shaft 106, rather than being entirely disposed in the rotation plane. In yet another embodiment, the rotor arms 122 may instead be pivotally connected to the rotatable shaft 106, so that the rotor arms 122 may be selectively tilted upward and downward as desired, either manually, or automatically using one or more arm actuators to perform the tilting of the rotor arms 122.

[0209] In the illustrated embodiment, the plurality of airflow deflectors 200 includes six deflectors 200 that are substantially similar to one another and that are substantially evenly spaced from one another along an azimuth direction about the central housing axis H (i.e., along the circumference of the housing sidewall 66). Alternatively, all of the deflectors 200 may not be similar to one another, may be unevenly spaced from one another, and / or the pulverizer 50 may include more or less than six deflectors 202. For example, the pulverizer 50 may include between two and eight deflectors 200.

[0210] In the illustrated embodiment, each deflector 200 is elongated and extends substantially parallel to the housing axis H. Specifically, because the housing 60 is positioned such that the central housing axis H extends substantially vertically, the deflectors 200 also extend substantially vertically.

[0211] like Figures 8 to 10, each deflector 200 includes a top end 202 positioned proximate the top end 64 of the housing 60 and a bottom end 204 positioned proximate the bottom end 62 of the housing 60. In the illustrated embodiment, each deflector 200 is positioned so as to intersect the rotational plane of the upper pulverizing rotor 108a and the rotational plane of the intermediate pulverizing rotor 108c. More specifically, the top end 202 of the deflector 200 is located above the upper pulverizing rotor 108a, while the bottom end 204 of the deflector 200 is located below the intermediate pulverizing rotor 108b, and the deflector 200 extends continuously between the top end 202 and the bottom end 204 thereof.

[0212] It will be appreciated that the rotation of the rotor arm 122 will cause the air within the interior chamber 68 to move outwardly toward the housing sidewall 66. In the above configuration, since the deflector 200 is horizontally aligned with the upper and middle pulverizing rotors 108a, 108b, the upper pulverizing rotor 108a and the middle pulverizing rotor 108b cause the air to move outwardly toward the deflector 200, and the air is deflected by the deflector 200 to form a vortex V, as shown in FIG. Fig.11 and 12 Best shown in .

[0213] In the illustrated embodiment, each deflector 200 is generally wedge-shaped. Specifically, each deflector 200 has a generally triangular cross-section and includes a flow-facing deflection surface 206 and an opposite deflection surface 208, the surface 206 facing the airflow when the rotatable shaft 106 rotates, and the opposite deflection surface 208 facing away from the airflow. The flow-facing deflection surface 206 and the opposite deflection surface 208 extend away from the housing sidewall 126 and converge toward each other to meet at an apex 210 pointing toward the housing center axis H. The flow-facing deflection surface 206 is inclined at a first deflection angle θ1 relative to the inner surface of the housing sidewall 126, and the opposite deflection surface 208 is inclined at a second deflection angle θ2 relative to the inner surface 74 of the housing sidewall 76.

[0214] In the illustrated embodiment, each deflector 200 is symmetrical about an axis of symmetry S that extends along a radius of the housing 60. In this embodiment, the first deflection angle θ1 is thus substantially equal to the second deflection angle θ2. In one embodiment, the first and second deflection angles θ1, θ2 may be equal to about 1 degree to 89 degrees, and more specifically, equal to about 30 degrees to 60 degrees. Alternatively, the deflector 200 may be asymmetrical, and the first and second deflection angles θ1, θ2 may be different from each other.

[0215] In the illustrated embodiment, the apex 210 of each deflector 200 is spaced radially inwardly from the inner surface 74 of the housing sidewall by approximately 7 mm. 31 or about 4 inches or about 20 centimeters in radial distance. Still in the illustrated embodiment, the apex 210 is spaced radially outwardly from the end 130 of the rotor arm 122 by a radial distance of between about 1 / 2 inch or about 1 centimeter and about 2 inches or about 5 centimeters. In one embodiment, the radial distance or "gap" between the end 130 of the rotor arm 122 and the apex 210 can be selected so that when the rotatable shaft 106 rotates, the vortex V can be formed as desired.

[0216] Alternatively, the deflector 200 may have a different shape and / or size. For example, the flow-facing deflection surface 206 and the opposite deflection surface 208 may not be planar, but may be curved. In another embodiment, the deflector 200 may not include the opposite deflection surface 208. In yet another embodiment, the deflector 200 may have a rectangular cross-section instead of a wedge shape, or may have any other shape and size deemed suitable by a person skilled in the art.

[0217] Fig.12 is a schematic diagram of a vortex V generated within the internal chamber 68 when the pulverizer 50 is in operation.

[0218] During operation of the pulverizer 10, the rotatable shaft 106 rotates about the housing axis H, causing the rotor arms 122 to form an annular airflow that rotates about the housing axis H. Fig.12 In the example shown, the rotatable shaft 106 rotates in a clockwise direction when viewed from above to create a counterclockwise airflow within the interior chamber 68 .

[0219] The rotatable shaft 106 can be rotated at a relatively high speed to provide the desired pulverizing effect in the pulverizer. In one embodiment, the rotatable shaft 106 is rotated at a speed between about 700 rpm and about 1500 rpm, or between about 700 rpm and about 1100 rpm, or more specifically between about 1000 rpm and about 1100 rpm. Alternatively, the rotatable shaft 106 can be rotated at different speeds that allow the formation of a vortex as described below.

[0220] The airflow generally flows along the inner surface 34 of the housing sidewall 66 but is interrupted by the flow-facing deflection surface 206 of the deflector 200 which cooperates with the rotor arm 122, and more specifically, with the distal end of the rotor arm 122 to form the vortex V. Fig.12 As shown in , the vortex V may be further directed back inwardly toward the center housing axis H by adjacent deflectors 200 ′.

[0221] Still see Fig.12Each vortex V also overlaps with at least one adjacent vortex V1, V2, so that the input material particles suspended in the vortex V collide with the input material particles suspended in the adjacent vortex or multiple vortices V1, V2. More specifically, each vortex V generated generally includes an outward moving portion 500 and an inward moving portion 502, wherein the outward moving portion 500 is generally defined by the airflow circulating from the shaft 106 toward the housing side wall 66, and the inward moving portion 502 is generally defined by the airflow circulating from the housing side wall 126 toward the shaft 106. Fig.12 As shown in , the outwardly moving portion 500 of each vortex V overlaps with the inwardly moving portion 502 of the first adjacent vortex V1 , and the inwardly moving portion 502 of each vortex overlaps with the outwardly moving portion 500 of the second adjacent vortex V2 .

[0222] Thus, in this configuration, the input material particles in the vortex collide with the input material particles moving at twice the speed of the particles in the vortex V. For example, in one embodiment, the vortices V, V1, V2 rotate at about one-third the speed of sound. When the input material particles from the first and second adjacent vortices V1, V2 collide with the suspended input material particles in the vortex V moving at the same speed but in the opposite direction, the particles will collide with each other at about two-thirds the speed of sound.

[0223] In one embodiment, in addition to the collision of the input material particles through the airflow and the vortex V, the input material can be further pulverized by the rotor arms 122 striking the input material particles in the internal chamber 68 as the rotatable shaft 106 rotates. In this embodiment, the combined effect of the input material particles colliding with each other in the overlapping vortices V, V1, V2 and the rotor arms 122 striking the input material particles can improve the efficiency of the pulverizer 50. In addition, because the overlapping vortices V cause the particles to collide with each other rather than with the surfaces inside the housing 20, wear on the internal components of the housing 20 can be reduced.

[0224] It will be understood that Fig.11 and 12 The vortex V shown in FIG. 1 has been simplified for ease of understanding, and in practice, the vortex V may not be completely circular as shown, or may not be completely circular as shown. Fig.11 and 12 Positioning shown.

[0225] In the illustrated embodiment, the pulverizer 50 further includes a plurality of shelves 300a, 300b extending inwardly from the housing sidewall 126. Specifically, the plurality of shelves 300a, 300b include an upper shelf 300a and a lower shelf 300b spaced downwardly from the upper shelf 300a. Each shelf 300a, 300b extends circumferentially around the housing axis H and along the housing sidewall 126. It will be appreciated that the shelves thus extend substantially perpendicular to the deflector 200. Specifically, the deflector 200 extends substantially parallel to the housing axis H, and thus can be said to extend in an axial direction relative to the housing 60, while the shelves 300a, 300b can be said to extend in an azimuthal direction relative to the housing 60. In the illustrated embodiment, the deflector 200 extends substantially vertically, while each shelf 300a, 300b is disposed in a substantially horizontal plane, and thus extends substantially horizontally.

[0226] Still in the illustrated embodiment, each shelf 300a, 300b extends substantially continuously around the housing sidewall 66. Alternatively, the shelves 300a, 300b may not extend continuously around the housing sidewall 66, but may include a plurality of shelf segments spaced apart from each other to define gaps between adjacent shelf segments.

[0227] In the illustrated embodiment, the upper shelf 300a is substantially horizontally aligned with the upper pulverizing rotor 108a, while the lower shelf 300b is substantially horizontally aligned with the middle pulverizing rotor 108b. Alternatively, each shelf 300a, 300b may be positioned slightly lower than the corresponding pulverizing rotor 108a, 108b.

[0228] In the illustrated embodiment, each shelf 300a, 300b includes a top shelf face 302 that extends downwardly and away from the housing sidewall 66. Specifically, because the shelves 300a, 300b extend along the housing sidewall 66 and about the housing axis H, the top shelf face 302 is substantially conical. Still in the illustrated embodiment, the top shelf face 302 is inclined relative to the housing sidewall 66 at an angle between about 1 degree (wherein the top shelf face 302 will be almost flat against the housing sidewall 66) and about 89 degrees (wherein the top shelf face 302 will be almost perpendicular to the housing axis H). In one embodiment, the top shelf face 302 can be inclined relative to the housing sidewall 66 at an angle between 30 degrees and 60 degrees.

[0229] The shelves 300a, 300b are configured to deflect the airflow flowing toward the shelves upward. This allows the input material particles to be temporarily suspended above the shelves 300a, 300b. Therefore, the input material particles can be affected by the vortex and pulverized for a longer time by impact with the rotor arm 122, resulting in further size reduction and / or mechanochemical processing of the input material particles as they move downward toward the next rotor stage or toward the outlet 72.

[0230] The upward deflection of the airflow can further promote the vortex V in the inner chamber 68. More specifically, as Fig.11 As shown in Fig.12 In addition to rotating in a plane perpendicular to the housing axis H, the vortex V can also rotate in a plane substantially parallel to the housing axis, i.e., rotate up and down. Therefore, the combined action of the shelves 300a, 300b and the deflector 200 helps to form a three-dimensional vortex V, so that the air in the vortex V moves along a three-dimensional travel path, which can further promote collisions between the input material particles of adjacent overlapping vortices V.

[0231] This configuration also allows the number of vortices V generated by the deflectors 200 to be multiplied by the number of shelves 300a, 300b in the housing 60. For example, in the illustrated embodiment, the pulverizer 50 includes six deflectors 200, which can form six vortices above each shelf 300a, 300b, for a total of 12 vortices throughout the interior chamber 68.

[0232] The pulverizer 50 can be designed and sized to process a raw material stream for a single process. For example, the pulverizer can be sized to process a raw material stream of 5 to 40 tons per hour or 20 to 40 tons per hour, the raw material stream comprising a mixture of components as described above, while operating as a single unit at a speed between 500 RPM and 1,200 RPM, or between about 500 RPM and about 1,300 RPM, or between about 500 RPM and about 1500 RPM to produce one or more output size selected streams as described herein.

[0233] Reference now Fig.13, a system including a kinetic pulverizer 50, a processing unit, a pulverizer conveyor system 50a, and an extraction unit 20a is shown. The system receives a mining material 10 from a mining operation 12 and provides it to a kinetic pulverizer 50 for a kinetic pulverization stage to produce a pulverized output material 18. In some embodiments, the kinetic pulverizer 50 includes an additional unit, such as a processing unit, to introduce a chemical additive 40, an additive 15, a friable additive 17, or a leachate 27. For example, the chemical additive unit 40a, the additive unit 15a, the friable unit 17a, or the leachate unit 27a can be operatively connected to the kinetic pulverizer 50 and configured to introduce a stream into the kinetic pulverizer 50 and / or other units. For example, the chemical additive unit 40a can be operatively connected to the leachate unit 27a to mix the chemical additive 40 with the leachate 27 before introducing the chemical additive-leachate mixture into the mining material 10, the kinetic pulverizer 50, and / or the pulverized output stream 18. In some embodiments, the chemical additive unit and the leachate unit may be operably connected to an additional homogenizing unit 10a configured to homogenize the chemical additive 40 and the leachate 27 prior to introducing them into the mined material 10 , the kinetic pulverizer 50 and / or the pulverized output stream 18 .

[0234] In some embodiments, the extraction unit 20a includes a leaching unit 26a and a recovery unit 30a. The leaching unit 26a can be configured to receive the pulverized material, combine the leachate 27 into the pulverized material 18, and produce a leachate 28 containing valuable components 22 and solid-rich waste material 24. In some embodiments, the recovery unit 30a can be configured to receive the leachate 28 from the leaching unit 26a and produce a valuable component 22 product and a depleted leachate 27, which can be optionally recycled back to the leaching unit 26a.

[0235] Reference now Fig.14In some embodiments, the method includes a pre-separation stage including a magnetic separation stage 2000 or magnetic separation located upstream of the kinetic pulverization stage 13 to capture ferrous metals from the mined material 10. The separated metal 2002 can be supplied as scrap metal for resale, can be used as a mining byproduct, or can be disposed of. The metal-depleted mined material 2004 can be fed to the kinetic pulverizer 16 for kinetic pulverization stage 13. The magnetic separator can be designed and operated to remove tramp metals with high weight density to reduce wear and damage to the KP. For example, a magnetic separator can be provided based on the nominal size of the feed and the ferrous objects that are desired to be removed. For example, a magnetic separator can be provided to ensure the removal of solid ferrous objects with high weight in an overall smaller volume. While certain geometries (e.g., flat plates) may have little effect on the operation of the KP, other geometries, such as blocks, chunks, etc., may increase wear and damage, and therefore the magnetic separation stage 2000 facilitates removal to enhance downstream processing. The magnetic separator can be configured based on the size of the feed material, the size of the ferrous objects, and the material loading depth. The magnetic separator can be actively controlled or easily turned on to achieve separation. The magnetic separation stage 2000 helps reduce the risk of wear and damage to the kinetic pulverizer 16 during the kinetic pulverization stage 13, and also recovers the scrap metal material.

[0236] The magnetic separation stage 2000 can use various types of magnetic separators, which can be selected based on the feed and output. For example, the magnetic separator can be a dry magnetic separator or a wet magnetic separator, depending on the moisture content of the feed. The magnetic separator can have such a magnetic field strength that is designed to remove target ferrous metal objects that may cause problems to the dynamic pulverizer 16. The magnetic separator can also include permanent magnets and electromagnetic magnetic separators. The magnetic separator can also have various designs and structural features, such as drum, roller, disc, ring, belt, etc. The magnetic separator can also use a constant, alternating, pulsating or rotating magnetic field, depending on the design and construction of the system and the feed. The magnet itself can be composed of various materials.

[0237] While magnetic separation is the preferred mechanism for removing metal from the feedstock, there are various other metal removal methods that can be used in place of or in addition to magnetic separation. Additional metal removal stages can be designed to remove non-ferrous metals, for example, particularly metal fragments that have a high weight density and are therefore relatively heavy and thick. In some embodiments, the metal removal method (e.g., magnetic separation) is performed to remove all metal fragments having an average diameter of 1 inch or greater. While selectively removing metal fragments having a flat plate shape, blocky or elongated metal fragments are also removed.

[0238] Reference now Fig.16 and 17 , two example configurations of the magnetic separation stage 2000 are shown. Fig.16 A belt-type magnetic separator 2006 is shown, including a self-cleaning magnetic belt 2008 located above a conveyor 2010. The magnetic belt 2008 discharges ferrous metals into a bin 2012. The magnetic belt 2008 may be mounted to a magnet frame 2014 that spans the conveyor 2010. Fig.17 An alternative construction is shown that includes a fixed magnet 2018 mounted above the conveyor 2010 and on a track 2020 configured to move back and forth.

[0239] Reference Fig.14 The system may also include a dust collection stage 3000 for recovering dust in the pulverized output stream 18 exiting the kinetic pulverizer 16. The pulverized output stream 18 enters the dust control stage 3000, which recovers the dust stream 3002 and produces a dust-reduced pulverized stream 3004 that may be sent to the extraction stage 20. The dust collection stage 3000 facilitates dust control and may include various units, such as a settling chamber and a bag filter or cyclone filter unit.

[0240] Reference now Fig.15 The dust collection stage 3000 may include a dust collector 3006 coupled to the outlet 16 of the kinetic pulverizer and may include a settling chamber 3008 having a dust outlet 3010 at its top. The dust outlet may be in fluid communication with a dust recovery unit 3014 via a duct 3012, and the dust recovery unit 3014 may include a bag filter or a cyclone filter unit 3016 having a dedicated motor 3018. The dust recovery unit 3014 may also include a dust recovery container 3020, which receives dust from the bag filter or the cyclone filter unit, for example, through a hopper. In some embodiments, the dust collection stage may include a wet or dry electrostatic precipitator (ESP) that removes dust particles using an electrostatic charge to separate small particles from the pulverized output stream 18.

[0241] The settling chamber 3008 can receive all the output (crushed output flow 18) from the kinetic pulverizer 16, and thus receive relatively fine particles, which are deposited on the discharge conveyor 3022, thereby adding the crushed material to the transfer output or redirecting it to the extraction stage 20. The fine particles settle on the discharge conveyor 3022, while very fine dust particles accumulate and are discharged from the sedimentation through the dust outlet 3010. The settling chamber 3008 can extend to part or all of the length of the discharge conveyor 3022, depending on the process design and the target level of dust control. Since the kinetic pulverizer 16 may vibrate, the settling chamber 3008 can be connected to the outlet of the kinetic pulverizer 16 through a flexible tubular member.

[0242] The amount of dust in the pulverization output stream 18 is highly dependent on the type and dryness of the feedstock supplied to the kinetic pulverization stage 13. In some embodiments, the fine reclaimed material 3024 may be treated with chemical additives 40 and / or leachate 27 and redirected to the extraction stage 20 to obtain a leachate 28 enriched with valuable components.

[0243] It is noted that the power and suction of the dust collection stage 3000 can be adjusted to increase the amount of material captured in the dust collector. For example, the dust recovery unit 3014 can be controlled to provide a desired suction in the dust collector 3006. Thus, the dust collection stage 3000 can be designed and operated as a tool to separate the material from the kinetic pulverization stage 13.

[0244] Still see Fig.15 , bag filter filtration or cyclone filtration 3016 captures finer, lighter materials that can be stored in container 3020. This fine recovery material 3024 can be added back to the diverted output stream, disposed of, and / or retained as a fine product for sale. The fine recovery material 3024 can be recycled back to one or more stages of the system, such as the extraction stage 20 or the leaching stage 26. In some embodiments, the fine recovery material 3024 will be supplied to the dust reduction stream 3004 or the pulverization output stream 18, or will be retained as a separate product stream that can be sold or mixed with other materials to provide a commercial product. It is noted that the recovered dust material can be handled, transported, and used in a variety of ways, some of which are described herein.

[0245] Example processing

[0246] The processing described herein may be performed on a mined feedstock comprising a lithium-rich clay containing about 0.5 to about 5 g / kg of lithium. About 3% to 5% by weight NaCl (Example 1) or about 3% to 5% by weight MgCl2 (Example 2) may be mixed with the lithium-rich clay and the resulting mixture may be subjected to a kinetic pulverization stage in a kinetic pulverizer. Alternatively, the lithium-rich clay containing about 0.5 to about 5 g / kg of lithium may be directly subjected to a kinetic pulverization stage and about 3% to 5% by weight NaCl (Example 3) or about 3% to 5% by weight MgCl2 (Example 4) may be mixed with the pulverized output material during the leaching stage.

[0247] The kinetic pulverization stage may include a single continuous flow process, wherein the kinetic pulverizer is operated at a low speed of 750 rpm or a high speed of 1000 rpm. The pulverized output material leaving the kinetic pulverization stage may undergo one or more post-processing stages. For example, the pulverized output material may undergo a fragmentation separation stage, wherein the material is classified by size to produce an oversize portion. All of the pulverized output material, or if it undergoes a fragmentation separation stage, only the oversize material, may also be subjected to a secondary size reduction stage. The secondary size reduction stage may include placing the pulverized output material or the oversize material in a secondary size reduction machine (e.g., a ball mill) for about 2 to about 3 hours. The ball mill may be operated at a speed of about 500 rpm.

[0248] For all four examples, the pulverized output material leaving the kinetic pulverization stage or the processed oversized material leaving the secondary size reducer can be subjected to a leaching stage, in which 20% by weight water is added as a leachate. The leaching stage can be carried out at 90°C with stirring at a rotation speed of 1000 rpm for 20 minutes. In theory, the resulting leachate rich in valuable components contains about 2.7g / kg sodium lithium (NaLi) (Examples 1 and 3) or about 2.8g / kg magnesium lithium (MgLi) (Examples 2 and 4), resulting in a lithium extraction efficiency greater than 50%. In theory, the lithium extraction efficiency does not substantially change in the process of adding chemical additives before or after the kinetic pulverization stage. In theory, in each of Examples 1 to 4, the amounts of other elements that are also isolated from the lithium-rich clay are as shown in Table 2.

[0249] Table 2

[0250] element Solution concentration (ppm) lithium ≥100 aluminum ≤10 iron ≤10 Potassium ≤8000 calcium ≤3000 magnesium ≤3000

Claims

1. A method for extracting a valuable component from a mining feedstock comprising a geological material embedded with the valuable component, the method comprising: subjecting the mined material to a kinetic comminution stage, wherein the mined material is fed into a kinetic pulverizer and undergoes self-collision generated by a vortex within the kinetic pulverizer to produce comminuted material; mixing the mined feedstock or the comminuted material with a chemical additive configured to selectively release the valuable components from the geological material; as well as The comminuted material is subjected to an extraction stage to produce a stream enriched in valuable components and a stream depleted in valuable components.

2. The method of claim 1, wherein the chemical additive comprises a cation source configured to perform an ion exchange with the valuable component.

3. The method according to claim 1 or 2, wherein the chemical additive comprises a salt compound.

4. The method according to any one of claims 1 to 3, wherein the chemical additive is selected from the group consisting of NaCl, PCl3, KCl, Na2SO4, K2SO4, MgSO4, CaSO4, NaNO3, KNO3, CaCl2, MgCl2, Ca(NO3)2 and Mg(NO3)2.

5. The method of claim 4, wherein the chemical additive is NaCl.

6. A method according to any one of claims 1 to 5, wherein the chemical additive is mixed with the mined feedstock simultaneously with or before the mined feedstock undergoes the kinetic comminution stage.

7. The method of claim 6, wherein the chemical additive is introduced directly into the kinetic pulverizer simultaneously with and as a separate stream from the mined material.

8. A method according to claim 6 or 7, wherein the chemical additive is homogeneously mixed with the mined material to form part of the comminuted material.

9. A method according to any one of claims 1 to 5, wherein the chemical additive is mixed with the comminuted material after the mined feedstock has passed through the kinetic comminution stage.

10. The method of any one of claims 1 to 9, wherein a leachate is introduced into at least one of: the mined feedstock, the kinetic pulverizer, the pulverized material, and the chemical additive.

11. The method according to claim 10, wherein: Leachate is introduced into at least one of the chemical additive, the kinetic pulverizer, and the mined material at least one of concurrently with and prior to the mined material undergoing the kinetic pulverization stage.

12. The method of claim 11, wherein the leachate is introduced directly into the kinetic pulverizer simultaneously with the mined material and as a separate leachate stream from the mined material.

13. The method of claim 10, wherein the leachate is introduced into at least one of: the chemical additive and the comminuted material after the mined feedstock has passed through the kinetic comminution stage.

14. A method according to any one of claims 1 to 13, wherein the extraction stage comprises subjecting the comminuted stream to a leaching stage.

15. The method of claim 14, wherein the leaching stage comprises separating a stream enriched in valuable components from a stream depleted in valuable components.

16. The method of claim 15, wherein the valuable component-enriched stream is separated from the valuable component-depleted stream using a mechanical screen.

17. The method of claim 16, wherein the mechanical screen is a rotary screen.

18. The method of claim 16, wherein the mechanical screen is a trommel screen.

19. The method of claim 16, wherein the mechanical screen is a vibrating screen.

20. The method of claim 16, wherein the mechanical screen is a rotary screen.

21. The method of claim 16, wherein the mechanical screen is a high frequency screen.

22. The method of claim 16, wherein the mechanical screen is a sorting device.

23. The method of claim 22, wherein the classifying device is an air classifier.

24. The method of claim 22, wherein the classification device is a hydrocyclone.

25. The method of claim 15, wherein: The valuable component-enriched stream is separated from the valuable component-depleted stream using a filter.

26. The method of any one of claims 14 to 25, further comprising agitating the mixture of the comminuted material and the chemical additive with a leachate to produce a stream enriched in valuable components.

27. The method of claim 26, wherein the stirring comprises stirring at a temperature between 60°C and 100°C.

28. The method of claim 26 or 27, wherein the stirring comprises stirring at between 800 rpm and 1200 rpm.

29. The method of any one of claims 26 to 28, wherein the stirring comprises stirring for at least 10 minutes.

30. The method according to any one of claims 1 to 29, wherein the extraction stage further comprises subjecting the stream enriched in valuable components to a recovery stage in order to recover the valuable components.

31. A process according to any one of claims 1 to 30, wherein the kinetic comminution stage is carried out in an inert environment.

32. A method according to any one of claims 1 to 30, wherein the chemical additive is mixed with the mined feedstock or the comminuted material in an inert environment.

33. A method according to claim 31 or 32, wherein the inert environment substantially comprises an oxygen-deficient environment.

34. A method according to any one of claims 31 to 33, wherein the inert environment comprises nitrogen.

35. The method of any one of claims 1 to 34, wherein the mining feedstock comprises at least one of ore, rock, mineral, slag, clinker, petroleum coke, clay mineral and soil mineral.

36. The method of any one of claims 1 to 35, wherein the valuable component comprises at least one of lithium, sodium, potassium, aluminum, silicon, magnesium, calcium, iron, nickel, and oxygen.

37. The method according to any one of claims 1 to 35, wherein the valuable component comprises graphene.

38. A method according to any one of claims 1 to 35, wherein the valuable components comprise rare earth minerals.

39. The method of claim 38, wherein the rare earth mineral comprises at least one of neodymium, yttrium, cerium, scandium, lanthanum, praseodymium, promethium, samarium, europium, gadolinium, terbium, dysprosium, holmium, erbium, thulium, ytterbium, and lutetium.

40. A method according to any one of claims 1 to 36, wherein the mined feedstock comprises a lithium-rich clay mineral.

41. The method of claim 40, wherein the valuable component is lithium.

42. The method of any one of claims 1 to 41, wherein the mined material comprises material having a size less than 12 inches.

43. The method of any one of claims 1 to 41, wherein the mined material comprises material having a size less than 6 inches.

44. The method of any one of claims 1 to 41, wherein the mined feedstock comprises material having a size between about 1 inch and about 4 inches.

45. The method of any one of claims 1 to 44, wherein the kinetic pulverizer is operated at a speed between 500 RPM and 1500 RPM.

46. ​​The method of any one of claims 1 to 44, wherein the kinetic pulverizer is operated at a speed between 700 RPM and 1000 RPM.

47. A method according to any one of claims 1 to 46 wherein the kinetic pulverizer is operated such that the pulverized material is substantially sand or silt sized particles.

48. A method according to any one of claims 1 to 46, wherein the kinetic pulverizer is operated such that the pulverized material is substantially micron-sized particles.

49. A method according to any one of claims 1 to 46, wherein the kinetic pulverizer is operated such that the pulverized material is substantially sub-micron sized particles.

50. The method of any one of claims 1 to 49, wherein the mined material has a moisture content of between 10% and 50% when entering the kinetic pulverizer.

51. The method of any one of claims 1 to 49, wherein the mined material has a moisture content of between 15% and 40% when entering the kinetic pulverizer.

52. The method of any one of claims 1 to 49, wherein the pulverized material is a homogenous mixture in a pulverized output stream.

53. The method of any one of claims 1 to 52, further comprising incorporating a friable additive into the mined feedstock, whereby the friable additive is reduced in size and homogeneously mixed with the mined feedstock to form part of the comminuted material.

54. The method of claim 53, wherein the friable additive and the chemical additive are pulverized and uniformly mixed with the mining material simultaneously in the kinetic pulverizer.

55. A method as claimed in claim 53 or 54 wherein the friable additive is introduced into the mined material upstream of the kinetic comminution stage.

56. The method of claim 53 or 54, wherein the friable additive is introduced directly into the kinetic pulverizer as a friable stream separate from the mined material.

57. A method according to any one of claims 1 to 56, further comprising subjecting the mined material to a pre-treatment stage prior to the kinetic comminution stage.

58. A method as claimed in claim 57, wherein the pre-processing stage is a magnetic separation stage which separates ferrous material from the mined material before the mined material is subjected to the kinetic comminution stage.

59. A method as claimed in claim 58, wherein the magnetic separation stage is performed by one or more magnetic separators arranged relative to the feed of mining material.

60. The method of claim 57, wherein the pre-treatment stage comprises at least one of: a coarse screening stage, a chemical addition stage, a drying stage, and a fragment separation stage.

61. The method of any one of claims 1 to 60, further comprising subjecting the comminuted material to a post-processing stage.

62. The method of claim 61, wherein the post-processing stage comprises at least one of: a chemical addition stage, a heating stage, a fragment separation stage, an electrostatic separation stage, a dust collection stage, and a secondary size reduction stage.

63. The method of claim 62, wherein the dust collection stage comprises recovering a dust portion therefrom and producing a dust-reduced pulverized stream.

64. A method according to claim 63, wherein the dust-reduced pulverized stream passes through an extraction stage and, optionally, the dust fraction is also recovered and fed to the extraction stage.

65. The method of claim 62, wherein the electrostatic separation stage comprises electrostatically separating particulate material from the comminuted material.

66. The method of claim 62, wherein the secondary size reduction stage comprises subjecting the shredded material to a size reducer.

67. The method of claim 66, wherein the size reduction machine comprises at least one of a ball mill, an oscillating motion mill, a hammer mill, a high shear energy mill, a vibrating mill, an attritor, a crusher, and an attritor.

68. The method of claim 62, wherein the fragment separation stage comprises subjecting the comminuted material to flotation separation.

69. The method according to any one of claims 1 to 68, further comprising: Monitor at least one of the following: at least one feed parameter of the mined material; as well as at least one output parameter of the pulverized material; as well as The kinetic comminution stage is adjusted based on at least one of: the at least one feed parameter and the at least one output parameter.

70. The method of claim 69, wherein the at least one feed parameter comprises at least one of a feed rate of the mined feed, a moisture content of the mined feed, and a composition of the mined feed.

71. The method of claim 69 or 70, wherein the at least one output parameter comprises at least one of: size characteristics of the pulverized material, composition of the pulverized material, moisture content of the pulverized material, flow rate of the pulverized material, and composition of the pulverized material.

72. The method of any one of claims 69 to 71, wherein: Adjusting the kinetic pulverizing stage includes adjusting the rotation speed of the kinetic pulverizer.

73. The method of any one of claims 69 to 72, wherein: Adjusting the kinetic pulverizing stage includes adjusting the feed rate of the mined material into the kinetic pulverizer.

74. A method of producing a comminuted material comprising a homogeneous mixture of geological material from a mining feedstock and an additive, the method comprising: Providing mining raw materials including geological materials; mixing the additive with the mined raw material; subjecting the mined feedstock to a kinetic pulverizing stage, wherein the mined feedstock is fed into the kinetic pulverizer and subjected to vortex-generated self-collision within the kinetic pulverizer to produce a homogenous mixture of the geomaterial and the additive; and removing the homogeneous mixture from the kinetic pulverizer; Wherein, the additive is mixed with the mining raw material simultaneously with or before the kinetic comminution stage.

75. The method of claim 74, wherein the additive is introduced into the mined material upstream of the kinetic comminution stage.

76. The method of claim 74, wherein the additive is introduced directly into the kinetic pulverizer as an additive stream separate from the mined material.

77. The method of any one of claims 74 to 76 further comprising mixing a friable additive with the mined feedstock simultaneously with or prior to the kinetic comminution stage to reduce size and homogenously mix with the geological material.

78. The method of claim 77, wherein the friable additive is introduced into the mined material upstream of the kinetic comminution stage.

79. The method of claim 77, wherein the friable additive is introduced directly into the kinetic pulverizer as a friable stream separate from the mined material.

80. A method as claimed in any one of claims 74 to 79 further comprising subjecting the mined material to a magnetic separation stage prior to the kinetic reduction stage to remove ferrous metals therefrom and produce a metal depleted feed stream which is fed to the kinetic reduction stage.

81. The method of claim 80, wherein the magnetic separation is performed by one or more magnetic separators arranged relative to the feed of mining material.

82. A method according to any one of claims 74 to 81 further comprising subjecting the comminuted material to a dust collection stage to recover a dust portion therefrom and produce a dust-reduced comminuted stream.

83. The method of claim 82, wherein at least a portion of the dust fraction is combined with at least a portion of the dust-reduced pulverized stream.

84. The method of claim 83, wherein all of the dust fraction is combined with the dust-reduced pulverized stream.

85. The method of any one of claims 82 to 84, wherein the dust-reduced pulverized stream, the dust portion or both are subjected to an extraction stage to extract at least one valuable component therefrom.

86. A method according to any one of claims 82 to 85, wherein the dust collection stage comprises: a dust collector connected to an outlet of the kinetic comminution stage or to a solids conveying device, the solids conveying device being configured to convey the comminuted material out of the kinetic comminution stage; and A dust recovery unit is coupled to the dust collector and is configured to cause separation of the dust portion and transport the dust portion from the dust collector to a storage container.

87. The method of claim 86, wherein the dust collector comprises a settling chamber.

88. The method of claim 87, wherein the dust recovery unit comprises a baghouse in fluid communication with the settling chamber via a conduit.

89. The method of claim 87, wherein the dust recovery unit comprises a cyclone separator in fluid communication with the settling chamber via a conduit.

90. The method of any one of claims 86 to 89, wherein the solid transport device comprises a conveyor.

91. The method of any one of claims 86 to 90, wherein the dust collector surrounds the solids conveying device along a majority of its length.

92. The method of any one of claims 74 to 91, wherein the geological material is clinker.

93. The method of any one of claims 74 to 92, wherein the additive is gypsum.

94. A system comprising: a kinetic pulverizer configured to receive and process mining feedstock including geological material to produce pulverized material; A processing unit for processing the mined material, the pulverized material and / or the material in the kinetic pulverizer, the processing unit being configured to: Incorporating chemical additives, leachates, and / or frangible additives; subjecting the mined material to pre-treatment; and / or subjecting the comminuted material to post-processing; a pulverizer conveyor system configured to convey the pulverized material downstream; as well as An extraction unit is configured to receive the pulverized material from the pulverizer conveying system and extract valuable components therefrom.

95. The system of claim 94, wherein the processing unit is a chemical addition unit configured to incorporate the chemical additive into at least one of the mined feedstock and the comminuted material.

96. The system of claim 94 or 95, wherein the extraction unit comprises: a leaching unit configured to receive the comminuted material, combine the leachate into the comminuted material and produce a leachate comprising valuable components and a solids-rich depleted material; as well as A recovery device is configured to receive the leachate from the leaching unit and produce a valuable component product and a spent leachate that can be optionally recycled back to the leaching unit.

97. The system of claim 96, wherein the recovery unit is configured to cause crystallization of the valuable components in the leachate.

98. The system of claim 97, wherein spent leachate is treated and recycled back into the leaching unit.

99. The system of claim 97 or 98, wherein the recovery unit further comprises a screen to remove valuable components in solid form from the leachate.

100. The system of any one of claims 94 to 99, wherein the kinetic pulverizer is configured to operate at a rotational speed between 500 RPM and 1500 RPM.

101. The system of any one of claims 94 to 99, wherein the kinetic pulverizer is configured to operate at a rotational speed between 700 RPM and 1000 RPM.

102. The system of any one of claims 94 to 101, further comprising: A monitoring unit configured to monitor at least one of the following: at least one feed parameter of the mined material; and at least one output parameter of the pulverized material; as well as A control unit is coupled to the monitoring unit and is configured to regulate the kinetic pulverizer based on at least one of: the feed parameter and the output parameter.

103. The system of claim 102, wherein the monitoring unit and the control unit are configured such that the at least one feed parameter comprises at least one of: a feed rate of the mining material, a moisture content of the mining material, a composition of the mining material, and a feed rate of at least one unit.

104. The system of claim 102 or 103, wherein the control unit is configured to adjust the rotational speed of the kinetic pulverizer.

105. The system of any one of claims 102 to 104, wherein: The control unit is configured to regulate a feed rate of the mined material into the kinetic pulverizer.

106. The system of any one of claims 94 to 105, wherein the processing unit includes a magnetic separator for pre-processing to remove ferrous metals from the mined material and produce a metal-depleted feed stream, which is fed to the kinetic pulverizer.

107. The system of any one of claims 94 to 106, wherein the processing unit comprises a dust collection unit for post-processing to recover a dust fraction from the pulverized material and to produce a dust-reduced pulverized stream.

108. The system of claim 107, wherein the dust collection unit comprises: A dust collector connected to the outlet of the kinetic pulverizer or to the pulverizer conveyor; as well as A dust recovery unit is coupled to the dust collector and is configured to cause separation of the dust and transport the dust portion from the dust collector to a storage container.

109. The system of claim 108, wherein the dust collector comprises a settling chamber.

110. The system of claim 109, wherein the dust recovery unit comprises a baghouse in fluid communication with the settling chamber via a conduit.

111. The system of claim 109, wherein the dust recovery unit comprises a cyclone separator in fluid communication with the settling chamber via a conduit.

112. The system of any one of claims 108 to 111, wherein the dust collector surrounds the shredder conveyor system along a majority of its length.

113. The system of any one of claims 94 to 112, further comprising an inerting system operatively coupled to at least one of: the kinetic pulverizer, the pulverizer conveying system, the processing unit, and the extraction unit.

114. The system of claim 113, wherein the inerting system is configured to provide anoxic conditions.

115. The system of claim 113 or 114, wherein the inerting system is configured to provide nitrogen for inerting.

116. A method for mechanochemically processing a raw material, comprising: providing mining raw materials including said raw materials; as well as subjecting the mined feedstock to a kinetic comminution stage, wherein the mined feedstock is fed into a kinetic pulverizer and undergoes vortex-generated self-collision within the kinetic pulverizer to produce pulverized material, and operating the kinetic pulverizer to convert the raw material into a mechanochemically modified material; removing the pulverized material from the kinetic pulverizer, wherein the pulverized material comprises a mechanochemically modified material and a size-reduced matrix fraction; as well as The mechanochemically modified material is separated from the size-reduced matrix portion.

117. The method of claim 116, wherein the mechanochemically modified material comprises metal nanoparticles, catalysts, magnets, γ-graphene, metal iodates, nickel-vanadium carbide and molybdenum-vanadium carbide nanocomposite powders.

118. A method as claimed in claim 116 or 117, wherein the mined feedstock comprises a clay mineral which, upon comminution, forms part of the size-reduced matrix fraction.

119. A method for extracting valuable components from a mining material, the method comprising: subjecting the mined material to a kinetic comminution stage, wherein the mined material is fed into the kinetic pulverizer and subjected to self-collision generated by a vortex within the kinetic pulverizer to produce comminuted material; as well as The liberated valuable components are extracted from the comminuted material using a leachate.

120. A method for extracting valuable components from a mining material, the method comprising: subjecting the mined material to a kinetic comminution stage, wherein the mined material is fed into the kinetic pulverizer and undergoes vortex-generated self-collision within the kinetic pulverizer to produce comminuted material; contacting at least one of the mined feedstock and the comminuted material with a chemical additive to selectively release the valuable components from the size-reduced matrix material; as well as The liberated valuable components are separated from the size-reduced matrix material of the comminuted material.

121. The method of claim 120, wherein the kinetic comminution stage is a single kinetic comminution stage.

122. The method according to claim 120, wherein the kinetic comminution stage is a plurality of kinetic comminution stages, wherein the comminuted material is subjected to a second comminution stage in the kinetic pulverizer or in a second kinetic pulverizer.

123. The method of claim 120 or 121 further comprising subjecting the comminuted material to a secondary size reduction stage to produce an oversized material.

124. The method of claim 123, wherein the secondary size reduction stage comprises subjecting the shredded material to a secondary size reducer.

125. The method of claim 124, wherein the size reduction machine comprises at least one of a ball mill, an oscillating motion mill, a hammer mill, a high shear energy mill, a vibrating mill, an attritor, a crusher, and a grinder.

126. The method of any one of claims 120 to 125, wherein the chemical additive is contacted with the mined feedstock simultaneously with or before the mined feedstock undergoes the kinetic comminution stage.

127. The method of claim 126, wherein contacting at least one of the mined feedstock and the comminuted material with the chemical additive comprises at least one of: introducing the chemical additive directly into the kinetic pulverizer simultaneously with and as a separate stream from the mined material; uniformly mixing the chemical additive with the mined raw material to form a part of the comminuted material; and After the mined material has passed through the kinetic comminution stage, the chemical additive is mixed with the comminuted material.

128. The method of any one of claims 120 to 127, further comprising agitating the mixture of the comminuted material and the chemical additive with a leachate to produce a stream enriched in valuable components.

129. The method according to any one of claims 120 to 128, wherein separating the released valuable components from the size-reduced matrix material comprises subjecting the size-reduced matrix material to a recovery stage to recover the valuable components.

130. The method defined in any one of claims 120 to 129 further comprises subjecting the mined material to a pre-treatment stage prior to the kinetic comminution stage.

131. The method of claim 130, wherein the pre-treatment stage comprises at least one of: a coarse screening stage, a chemical addition stage, a drying stage, a fragment separation stage, and a magnetic separation stage.

132. The method according to any one of claims 120 to 131 , further comprising subjecting the comminuted material to a post-processing stage.

133. The method of claim 132, wherein the post-processing stage comprises at least one of: a chemical addition stage, a heating stage, a fragment separation stage, an electrostatic separation stage, and a dust collection stage.

134. A method according to claim 133, wherein the fragment separation stage comprises subjecting the comminuted material to flotation separation.

Citation Information

Patent Citations

  • Selective extraction of lithium from clay minerals

    WO2021138345A1