Method for producing graphite-containing metal oxide electrode, graphite-containing metal oxide electrode, use of graphite-containing metal oxide electrode, and electrolytic cell

By using carbonyl-free and cyano-free solutions in the electrolytic cell to deposit graphite-loaded metal oxides, complex problems in the prior art are solved, and simple manufacturing of electrochemical water decomposition electrodes and efficient hydrogen production and oxygen production are realized. They are suitable for Large-scale industrial application.

CN118984891APending Publication Date: 2024-11-19ENINNO GMBH
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202380030180.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-11-15
Filing Date
2023-02-01
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The existing methods for manufacturing metal chalcogenide electrodes are complex, and it is difficult to achieve simple and easy production of electrochemical water decomposition electrodes.

Method used

Using carbonyl and cyano groups-free aqueous or non-aqueous solutions, graphite-loaded precious metal oxides are added to the electrolytic cell, and graphite-containing metal oxide electrodes are deposited on the electrodes by applying voltage, and the old battery material of the electric vehicle is recycled. As substantia nigra, chemical modification is performed to optimize electrode performance.

Benefits of technology

It realizes simple manufacturing of electrochemical water decomposition electrodes and efficient hydrogen production and oxygen production, improves the durability and current density of the electrodes, and is suitable for large-scale industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118984891A_ABST
    Figure CN118984891A_ABST
Patent Text Reader

Abstract

The invention relates to a method for producing a graphite-containing metal oxide electrode, comprising the following steps: a) preparing (1) an electrolytic cell (10) containing an electrode (11), another electrode (12) and an aqueous and / or non-aqueous carbon-and cyano-free solution (14), b) introducing (2) a nigra (15) and a proton source into the solution (14) in the electrolytic cell (10), and c) applying (3) a voltage to the electrode (11) and the other electrode (12) such that the noble metal-free metal oxide and graphite provided by the black substance (15) are deposited on the electrode (11), thereby forming a graphite-containing metal oxide coating (17) on the electrode (11) to produce a graphite-containing metal oxide electrode. In addition, the invention also relates to a graphite-containing metal oxide electrode manufactured according to the method. Furthermore, the invention relates to the use of a graphite-containing metal oxide electrode for producing hydrogen and / or oxygen in water electrolysis and / or photoelectrochemical water electrolysis, and to an electrolytic cell (20) for producing hydrogen and / or oxygen in water electrolysis and / or photoelectrochemical water electrolysis, it comprises a graphite-containing metal oxide electrode as a cathode (22) and / or a graphite-containing metal oxide electrode as an anode (21).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for manufacturing a graphite-containing metal oxide electrode, a graphite-containing metal oxide electrode, a use of a graphite-containing metal oxide electrode and an electrolyzer. The present invention particularly relates to an easy-to-implement method for manufacturing a graphite-containing metal oxide electrode, a graphite-containing metal oxide electrode manufactured using the method, a use of the graphite-containing metal oxide electrode in electrochemical hydrogen and / or oxygen production, and an electrolyzer using the graphite-containing metal oxide electrode for hydrogen and oxygen production. Background Art

[0002] A method for producing a carbon-containing metal oxide electrode has been disclosed in WO 2015 / 082626 A1, which describes a method for producing a metal chalcogenide thin film electrode.

[0003] The method for manufacturing a metal chalcogenide thin film electrode comprises the following steps:

[0004] (a) contacting a metal or a metal oxide with an elemental halogen in a non-aqueous solvent to generate a metal halide in a solution;

[0005] (b) applying a negative voltage to a conductive or semiconductive substrate in contact with the solution in step (a); and

[0006] (c) during and / or after step (b), contacting the substrate with an elemental chalcogenide element to form a metal chalcogenide layer on the substrate.

[0007] A metal capable of forming a metal halide is used, wherein the oxidation state of the metal is +2 or higher, in particular Fe, Co, Ni, Cr, Mn or a mixture or alloy thereof. The halogen is in particular iodine or bromine. The chalcogenide is in particular O2, S or Se. An organic solvent is used as a non-aqueous solvent, preferably an organic solvent containing a carbonyl (CO) or cyano (CN) group. The metal chalcogenide thin film electrode prepared by this method can be used for (photo) electrochemical water splitting, in particular for an oxygen evolution electrode for electrochemical water splitting under application of an external potential or under light irradiation. However, the method is complicated because a precursor for deposition must first be generated. Therefore, there is an urgent need to provide an electrode that can be used for electrochemical water splitting and is easy to manufacture. Summary of the invention

[0008] It is therefore an object of the present invention to provide a simple and easy method for producing electrodes which are suitable for electrochemical water splitting.

[0009] This object is achieved by a production method having the features of claim 1, a graphite-containing metal oxide electrode having the features of claim 7, the use of a graphite-containing metal oxide electrode having the features of claim 8, and an electrolysis cell having the features of claim 9. Advantageous developments and modifications are described in the dependent claims.

[0010] The invention relates to a method for manufacturing a graphite-containing metal oxide electrode, comprising the following steps:

[0011] a) providing an electrolytic cell comprising an electrode, another electrode and an aqueous and / or non-aqueous solution free of carbonyl groups and free of cyanide groups;

[0012] b) adding a black substance and a proton source to a solution in an electrolytic cell, wherein the black substance comprises a metal oxide free of noble metal supported on graphite;

[0013] c) applying a voltage to the electrode and another electrode, so that the noble metal-free metal oxide and graphite provided by the black matter are deposited on the electrode, thereby forming a graphite-containing metal oxide coating on the electrode, and generating a graphite-containing metal oxide electrode.

[0014] To produce graphite-containing metal oxide electrodes, the precursors for producing chalcogenides are not used, but the metal oxides present in the black matter are directly used, and the percentage ratio of these metal oxides can be adjusted as needed. Among them, carbonyl-free and cyanide-free solutions are used. It is preferred to use cyclic ethers such as tetrahydrofuran and azeotropic alcohol-water mixtures under the condition that the battery voltage is less than 10V. Examples of electrode materials include nickel or steel materials.

[0015] The protons are derived from a weak Bronsted acid proton source (solvent molecules containing OH-, CH- and NH- groups). A preferred proton source is generated by the reaction of bromine and iodine with the solvent. Alternatively, highly diluted hydrogen bromide or hydrogen iodide solutions (concentrations of 10 -4 to 10 -6 molar), this solution can be prepared by adding hydrogen bromide or hydrogen iodide to an appropriate solvent. The protons act as a mediator when fixing the catalyst on the electrode.

[0016] In a preferred embodiment, the black matter is a recyclate. The recyclate preferably comes from old drive batteries of electric vehicles (especially electric cars). Black matter is a material obtained from old batteries of electric vehicles, which are used for electric drive of electric vehicles. In particular, the black matter is obtained by mechanically recycling old batteries of electric vehicles that are disassembled and recycled. Mechanical recycling includes multiple steps of crushing, sorting and classification after disassembling the shell and electronic parts of the old batteries to obtain and process materials such as black matter from the remainder. The black matter is provided by Duesenfeld GmbH (a limited company located in Winderberg, Germany). The black matter preferably contains layered materials, electrode materials and / or electrolyte materials of old batteries, usually in the form of a particle mixture. In the black matter, active materials rich in electrodes, such as graphite and lithium transition metal mixed oxides, such as cobalt, nickel and manganese, are preferably present. The composition of the black matter depends on the chemical composition of the recycled old batteries. Different types of electric vehicle drive batteries have different chemical compositions.

[0017] The black mass contains, in addition to metal(s) and metal(s) oxide(s), graphite as a carrier for the metal(s) and metal(s) oxide(s). The black mass preferably contains a plurality of metal oxides. The black mass preferably comprises mixed metal oxides, such as Ni, Co and Mn oxides. Alternatively, the black mass preferably comprises Ni, Co and Al oxides. Alternatively, the black mass preferably comprises a mixture of metal oxides, such as ... x (PO4) y The metal oxides in the black mass can be mixed Ni, Co, Mn oxides, Ni, Co, Al oxides or (multiple) iron oxides, all of which are supported by graphite. These metals (oxides) do not contain precious metals.

[0018] Preferably, the graphite-supported metal oxide or oxides are mixed with Ni, Co and / or Mn and at least one oxide of Ni, Co and / or Mn. The ratio of Ni, Mn and Co in the black mass can vary depending on the wet chemical treatment method for removing lithium and other components in the battery cathode, and also depends on the particle size of the black mass after recovery.

[0019] Well-known materials for making black materials for lithium batteries for electric vehicles, such as those described by Harper, G. et al. in Nature 575, 75-86 (2019), include: LiFePO4, LiMn2O4, Li(Ni,Co,Al)O2, LiNi 0.33 Mn 0.33 Co 0.33 O2、LiNi 0.5 Mn 0.3 Co 0.2 O2、LiNi 0.6 Mn 0.2 Co0.2 O2 and LiNi 0.8 Mn 0.1 Co 0.1 O2. Particularly preferred materials include: LiFePO4, Li(Ni,Co,Al)O2, LiNi 0.33 Mn 0.33 Co 0.33 O2、LiNi 0.5 Mn 0.3 Co 0.2 O2、LiNi 0.6 Mn 0.2 Co 0.2 O2 and LiNi 0.8 Mn 0.1 Co 0.1 O2.

[0020] A recyclate obtained from recycled materials of old electric vehicle drive batteries by Duesenfeld GmbH (a company located in Winderberg, Germany) is preferably used as black mass, which is based on NMC batteries (lithium nickel cobalt manganese oxide batteries). The recyclate contains 48.04% C, 16.16% O, 2.91% Ni, 0.52% Co, 0.30% Fe and 32.07% N by weight. Its morphology has a microscopic and / or nanostructure, and the morphology and particle size are not uniform.

[0021] Alternatively, a recyclate obtained from the recycled material of old drive batteries for electric vehicles by Duesenfeld GmbH (a company located in Winderberg, Germany) is preferably used as black mass, which is based on LFP batteries (lithium iron phosphate batteries). The recyclate contains 31.90% by weight of C, 36.87% by weight of O, 19.30% by weight of Fe and 11.94% by weight of P. Its morphology has a microscopic and / or nanostructure, and the morphology and particle size are not uniform.

[0022] In a preferred embodiment, the following steps are performed before step a) or step b):

[0023] - determine the composition and morphology of the substantia nigra, and

[0024] - Chemical modification of the substantia nigra according to the determined composition and morphology, including adjusting the percentage of metals (oxides) in the substantia nigra.

[0025] The percentage of elements in the black mass is preferably pre-set to a maximum value by wet chemical treatment of the lithium battery cathode material. Since the percentage may vary between batches and battery types, it is preferred to first determine the exact composition and morphology of the black mass and then chemically modify it, which is beneficial to improve the performance of the manufactured graphite-containing metal oxide electrode. The percentage of metal oxide in the black mass is preferably adjusted by chemical modification.

[0026] The composition and morphology of the substantia nigra can be known from data provided by the manufacturer and / or from the safety data sheet and / or can be determined by the following methods: solid state analysis (e.g., X-ray photoelectron spectroscopy (XPS), energy dispersive X-ray spectroscopy (EDX), scanning electron microscopy (SEM), transmission electron microscopy (TEM)), powder X-ray diffraction (PXRD), and wet chemical analysis (e.g., plasma ion chromatography (ICP)).

[0027] X-ray photoelectron spectroscopy (XPS) can be used for chemical analysis of black matter, and core energy level spectral lines can be associated with specific oxidation states by referring to information such as that published in the Handbook of X-Ray Photoelectron Spectroscopy edited by Chastain and King (Physical Electronics Press, Minnesota, USA, 1995).

[0028] Energy dispersive X-ray analysis (EDX) can be used for chemical elemental analysis, either globally (i.e. through the entire sample surface of the substantia nigra) or locally (i.e. through the lateral resolution of the scanning electron microscope), where the range of excitation energies should be chosen to detect the expected characteristic K or L lines of the elements, for example between 3keV and 10keV. The measured X-ray spectral lines can be automatically matched using, for example, the NSS2.2 database values ​​and control software from Thermo Fisher Scientific.

[0029] In a preferred embodiment, the chemical modification of the black matter includes adjusting the percentage of metal (oxide) in the black matter. According to the literature published by Cao X. et al. (Journal of American Chemical Society Catalysis, Vol. 8, 8273-8289 (2018)) and Lu Z. et al. (Nature Communications, Vol. 5, 4345 (2014)) on the use of mixed ternary metal oxides (i.e., pure metal oxides without graphite) obtained from recycled lithium batteries, it is advantageous to optimize the percentage composition of the metal oxide.

[0030] Chemical modification includes, for example, the addition of metals (oxides) to obtain an optimal ratio of metals and an optimized surface of the black matter particles. The added metals (oxides) can be the same as the metals (oxides) already present in the black matter to adjust the relative ratios in the black matter. The added metals (oxides) can also be different metals (oxides) from the metals (oxides) present in the black matter. The composition of the black matter can also be changed by treating the black matter with molecular hydrogen as a reducing agent at 300-400°C, which may partially form metal alloys such as NiCo, thereby improving the efficiency of the black matter in water splitting.

[0031] Metals (oxides) used for chemical modification can also be generated in situ. For example, Ni(OAc)2 (nickel(II) acetate) can be added to the black mass and reaction conditions applied to decompose the Ni(OAc)2 to generate nickel(II) oxide and nickel.

[0032] In addition, modification of the black matter can be achieved by modifying the metal oxide structure and / or the carrier material in which the black matter exists through anion / cation exchange under acidic or alkaline conditions. For example, the black matter can be heated in an aqueous solution containing formic acid and H2O2 to achieve anion / cation exchange under acidic conditions. Anion / cation exchange under alkaline conditions can be achieved by heating the black matter in a KOH aqueous solution.

[0033] The chemical modification of the black substance may also include chemical modification of the graphite as a carrier. Preferably, the following steps are performed before step a) or b):

[0034] - Adding one or more exogenous atoms (promoting atoms) to the graphite carrier of the black matter.

[0035] These exogenous atoms are preferably selected from nitrogen, sulfur, phosphorus and / or boron. More preferred exogenous atoms are nitrogen and / or sulfur.

[0036] In a preferred embodiment, the exogenous atom is nitrogen. By adding nitrogen to graphite, the performance and current density of hydrogen electrolysis using, for example, Ni / Co / Mn-containing black matter can be increased by at least 50%. The amount added can be in the substoichiometric range. In order to add nitrogen to graphite, the black matter is preferably heated in a stream of ammonia as a nitrogen source for 1 hour or more, preferably 1 to 10 hours, at a temperature between 200 and 400°C, more preferably 300-350°C. In this way, nitrogen is effectively incorporated into the graphite carrier. The presence of nitrogen in the material can be detected by XPS (X-ray photoelectron spectroscopy) emission spectroscopy. The addition of nitrogen can also be achieved by using N2, urea or hydrazine.

[0037] As an alternative or additional preferred exogenous atom, sulfur is preferred. Adding sulfur significantly increases the activity of the black matter in the hydrogen production process. When sulfur is added, if the black matter contains metals, a small amount of metal sulfides such as NiS, CoS and MnS will be generated in the black matter, which helps to produce hydrogen by electrolysis. The addition of sulfur can be achieved by using S8 or hydrogen sulfide.

[0038] The addition of equal amounts of sulfur and nitrogen can be achieved by reacting the black mass with thiourea, which serves as a source of both nitrogen and sulfur. For example, 0.1-0.3% by weight of thiourea can be used. The reaction can be carried out at 150-200°C for several hours.

[0039] Alternatively or additionally preferably the exogenous atom is phosphorus. The addition of phosphorus can be achieved by using red phosphorus.

[0040] Alternatively or additionally preferably the exogenous atom is boron. The addition of boron can be achieved by using boric acid or boron trioxide.

[0041] In a preferred embodiment, the solution is selected from cyclic ethers and / or azeotropic alcohol-water mixtures. Studies have shown that even cyclic ethers and azeotropic alcohol-water mixtures that are difficult to oxidize, such as tetrahydrofuran, can be used in the process at a cell voltage below 10V.

[0042] The present invention also relates to a graphite-containing metal oxide electrode manufactured according to one or more of the above embodiments.

[0043] This graphite-containing metal oxide electrode includes the electrode originally used as a conductor or semiconductor substrate in the method of the present invention, and the graphite-supported metal oxide layer deposited by the method, and under certain conditions, may also include exogenous atoms and / or metals (alloys). The graphite support provides the required strength and sealing for the layer deposited on the substrate. The charge transfer from the substrate to the metal oxide is optimized, and the stability of the substrate is also improved.

[0044] The graphite-containing metal oxide electrode preferably has a layer deposited on the substrate with a thickness of up to several micrometers, more preferably up to 10 μm. The thicker the layer, the more durable the electrode is in operation and the higher the current density.

[0045] Graphite-containing metal oxide electrodes can also be provided in the form of modules, which contain multiple electrode layers. Such electrode modules are available in sizes with a maximum dimension of 1 cm 2 The preferred graphite-containing metal oxide electrode size is greater than 1 cm 2 , more preferably greater than 16cm 2 , and more preferably 0.16 to 2.5 m 2 within the range.

[0046] The present invention also relates to the use of a graphite-containing metal oxide electrode for producing hydrogen and / or oxygen in (photo) electrochemical water splitting. The graphite-containing metal oxide electrode can be used as both an anode and a cathode in electrochemical water splitting. That is, the graphite-containing metal oxide electrode can be used to produce oxygen and / or hydrogen by water splitting by electrolysis. The above content should be understood as that in electrochemical water splitting, one graphite-containing metal oxide electrode is not used as anode and cathode at the same time, but one graphite-containing metal oxide electrode prepared according to the above method is used as an anode, and another graphite-containing metal oxide electrode prepared according to the above method is used as a cathode.

[0047] Large-scale industrial applications of graphite-containing metal oxide electrodes are feasible. Graphite-containing metal oxide electrodes are particularly suitable for large-scale hydrogen production. This hydrogen is also called green hydrogen, because it can be produced in an environmentally friendly manner from renewable energy (electricity). After all, it is advantageous to produce a plurality of graphite-containing metal oxide electrodes according to the above method and to use one of the graphite-containing metal oxide electrodes for hydrogen production and another graphite-containing metal oxide electrode as an anode for oxygen production in electrochemical total water splitting.

[0048] The present invention also relates to an electrolyzer for producing hydrogen and oxygen in a (photo) electrochemical water splitting process, which comprises a graphite-containing metal oxide electrode as a cathode and / or a graphite-containing metal oxide electrode as anode according to one or more of the above embodiments.

[0049] In a preferred embodiment, the electrolyzer uses an alkaline solution as the electrolyte. The alkaline solution preferably contains 0 to 6 molar potassium hydroxide (KOH), wherein in the case of a 0 molar KOH aqueous solution, the electrolyzer is equipped with an alkali exchange membrane (AEM). The electrolyzer is preferably designed to perform electrolysis in a temperature range from room temperature to a maximum of 80°C. The total cell voltage required for complete water decomposition is in the range of 1.23 to 2.5 V, and the current density is 100-1000 mA per square centimeter (cm -2 ).

[0050] The electrolyzer is preferably designed for large-scale hydrogen production. The graphite-containing metal oxide electrode can be manufactured into a large-area electrode of 0.16 to 2.5 square meters according to the method of the present invention. -2 At a current density of 2.5 m 2 Large graphite-containing metal oxide electrodes can generate up to 8 tons of H2 (=4x10 6 Moore). BRIEF DESCRIPTION OF THE DRAWINGS

[0051] Figure 1 a to 1c are process flow charts according to one embodiment,

[0052] Figure 2 is a process flow chart according to another embodiment,

[0053] Figure 3 is a cross-sectional view of an electrolytic cell according to the present invention,

[0054] Figure 4 is the powder diffraction pattern of black matter,

[0055] Figure 5 This is another powder diffraction pattern of black matter.

[0056] Figure 6 is the cyclic voltammogram of the graphite-containing metal oxide electrode of the present invention, and

[0057] Figure 7 yes Figure 6 Chronopotentiometry of graphite-containing metal oxide electrodes shown in . DETAILED DESCRIPTION

[0058] Figure 1 a to 1c show a process flow chart according to one embodiment, each cross-sectional view of an electrolytic cell for manufacturing the graphite-containing metal oxide electrode of the present invention is shown in the figure. Figure 1 a shows the steps of providing an electrolytic cell 10 with an electrode 11, another electrode 12 and an aqueous and / or non-aqueous carbonyl-free and cyanide-free solution 14. Figure 1 b shows the step of introducing a black mass 15 into the solution 14 in the electrolytic cell 10, wherein the black mass 15 comprises a graphite-supported metal oxide free of precious metals. Figure 1 c shows applying a voltage to one electrode 11 and the other electrode 12 so that the noble metal-free metal oxide and graphite obtained by using the black matter 15 are deposited on the electrode 11, thereby forming a graphite-containing metal oxide coating 17 on the electrode 11 to manufacture a graphite-containing metal oxide electrode.

[0059] Figure 2A process flow chart of another embodiment is shown. The method first includes a step 4, i.e., determining the composition and morphology of the black matter, and then a step 5, i.e., chemically modifying the black matter according to the composition and morphology determined in step 4, and adjusting the proportion based on the composition ratio of the metal oxide in the black matter to improve the application performance and stability of the manufactured graphite-containing electrode in electrochemical water splitting. After that, step 6 can be optionally performed, i.e., one or more exogenous atoms (promoting atoms), such as nitrogen, sulfur and / or phosphorus, are added to the graphite carrier of the black matter. Next, after step 5 or step 6, step 1 is performed to prepare an electrolytic cell with one electrode, another electrode and an aqueous and / or non-aqueous carbonyl-free and cyanide-free solution. Next, step 2 is performed to introduce the black matter into the solution in the electrolytic cell. After step 2, step 3 is performed to apply voltage to one electrode and another electrode so that the metal oxide and graphite obtained by using the black matter are deposited on the electrode, thereby forming a graphite-containing metal oxide coating on the electrode to manufacture a graphite-containing metal oxide electrode.

[0060] Figure 3 20 is used for producing hydrogen and oxygen in a (photo) electrochemical water splitting process. The electrolyzer comprises two Figure 1 A graphite-containing metal oxide electrode manufactured by the method shown in a-1c or 2. One of them is used as a cathode 22 and the other is used as an anode 21. The cathode 22 comprises a substrate 27 coated with a graphite-supported metal oxide coating 17. The anode 21 comprises another substrate 28 coated with the coating 17. The electrolytic cell 20 also comprises an alkaline solution 24 and a diaphragm 25, such as an ion exchange membrane (AEM), for separating the anode chamber and the cathode chamber.

[0061] In operation, an electric current is applied to the cathode 22 and the anode 21, thereby decomposing water. Oxygen is generated at the anode 21 and hydrogen is generated at the cathode 22.

[0062] Figure 4 The powder diffraction pattern of the black substance is shown. The powder diffraction pattern shows the composition of the black substance as a recovered material as described in Example 2 below.

[0063] Figure 5 Another powder diffraction pattern of black substance is shown. This powder diffraction pattern shows the composition of black substance as a recovered material as described in Example 3 below.

[0064] Figure 6The cyclic voltammogram of the graphite-containing metal oxide electrode of the present invention is shown, with a scan rate of 5 mV / s. The measurement was carried out in a three-electrode configuration, using a Hg / HgO reference electrode, and its potential was based on a reversible hydrogen electrode (RHE). In order to manufacture the graphite-containing metal oxide electrode of the present invention, the black substance prepared in the following Examples 2-5 was used, and the black substance was treated with nickel foam as described in Example 1. The prepared graphite-containing metal oxide electrode was used as a working electrode for oxygen production.

[0065] Figure 7 Shown is a chronopotentiometry graph performed at 100 mA / cm² on the above graphite-containing metal oxide electrode.

[0066] Example 1

[0067] Manufacturing of graphite-containing metal oxide electrodes

[0068] In order to manufacture the graphite-containing metal oxide electrode of the invention, an electrolytic cell is prepared, with an electrode based on Ni, Fe and / or Cu foam, another steel electrode, and 10 mL of a cyclic ether (e.g., tetrahydrofuran) solution. 25 mg of black matter and 2 mg of iodine are added to the solution. Then a 10 V voltage is applied to the electrodes in air at room temperature for 30 seconds to 10 minutes. 2 mg of iodine and 25 mg of black matter are sufficient to manufacture 10 to 15 graphite-containing metal oxide electrodes. The graphite-containing metal oxide electrode prepared in this way is washed with an organic solvent and dried in air.

[0069] Example 2

[0070] Determine the composition and morphology of the substantia nigra

[0071] Black mass is a recycled material obtained from old driving batteries of electric vehicles, especially electric vehicles. The recycled material is a recycled material based on NMC batteries (lithium nickel cobalt manganese oxide batteries) provided by Duesenfeld GmbH (a limited company located in Winderberg, Germany). One or more graphite-supported metal oxides free of precious metals in the black mass contain Ni, Co and Mn and at least one of their oxides. In addition to different types of graphite, the recycled material also contains (Li 0.98 Ni 0.02 )(Li 0.05 Ni 0.75 Co 0.10 Mn 0.10 )O2, aluminum and Al2O3. Figure 4 The powder diffraction pattern of this black substance is shown.

[0072] Example 2-1

[0073] Chemical modification of substantia nigra

[0074] 500 mg of the black substance used in Example 2 was added to an autoclave containing 0.05 g of Ni(OAc)2 and 30 mL of water and heated at 180°C for 16 hours. The suspension was then cooled naturally in an oven, washed with water and acetone, and then dried in air.

[0075] Example 2-2

[0076] Chemical modification of substantia nigra

[0077] 500 mg of the black substance used in Example 2 was placed in an autoclave together with 0.1 g of Ni(OAc)2 and 30 mL of water and heated at a temperature of 180° C. for 16 hours. The suspension was then cooled naturally in an oven, washed with water and acetone, and then dried in air.

[0078] Example 2-3

[0079] Chemical modification of substantia nigra

[0080] 100 mg of the black substance used in Example 2 was ground, placed in an aqueous solution containing 2M formic acid and 6% H2O2, and heated at a temperature of 80°C for 2 hours. Subsequently, the material was washed with water and acetone and dried in air.

[0081] Example 2-4

[0082] Chemical modification of substantia nigra

[0083] 100 mg of the black substance used in Example 2 was ground, put into a 1 M KOH aqueous solution, and heated at a temperature of 80° C. for 2 hours. Then, the material was washed with water and acetone, and dried in air.

[0084] Example 2-5

[0085] Adding nitrogen as an exogenous atom

[0086] 100 mg of the black mass used in Example 2 was first flushed with NH3 gas in a tube furnace for 2 hours and then heated to 300°C (heating rate of 300°C / h). After 6 hours, the material was naturally cooled to room temperature.

[0087] Example 2-6

[0088] Adding nitrogen as an exogenous atom

[0089] 100 mg of the black material used in Example 2 was first flushed with NH3 gas in a tube furnace for 2 hours and then heated to 400°C (heating rate of 300°C / h). After 6 hours, the material was naturally cooled to room temperature.

[0090] Example 2-7

[0091] Adding nitrogen as an exogenous atom

[0092] 100 mg of the black substance used in Example 2 was first flushed with NH3 gas in a tube furnace for 2 hours and then heated to 200°C (heating rate of 300°C / h). After heating for 6 hours, it was naturally cooled to room temperature.

[0093] Example 2-8

[0094] Adding nitrogen as an exogenous atom

[0095] 100 mg of the black substance used in Example 2 was first flushed with NH3 gas in a tube furnace for 2 hours and then heated to 350°C (heating rate of 300°C / h). After heating for 6 hours, it was naturally cooled to room temperature.

[0096] Example 2-9

[0097] Adding nitrogen as an exogenous atom

[0098] 100 mg of the black substance used in Example 2 was first flushed with NH3 gas in a tube furnace for 2 hours and then heated to 250°C (heating rate of 300°C / h). After heating for 6 hours, it was naturally cooled to room temperature.

[0099] Example 2-10

[0100] Adding nitrogen as an exogenous atom

[0101] 100 mg of the black substance used in Example 2 was added to a solution containing 40 mL of ethanol and 1.5 g of urea and suspended in an ultrasonic cleaner for 2 hours. Subsequently, the solution was evaporated under a stream of N2 for 2 hours. The resulting substance was ground and placed in a tube furnace and flushed with N2 for 1 hour. The black substance obtained in this way was then heated to 300°C (heating rate of 300°C / h), maintained at this temperature for 2 hours, and then naturally cooled to room temperature.

[0102] Example 2-11

[0103] Adding nitrogen as an exogenous atom

[0104] 100 mg of the black substance used in Example 2 was ground and placed in a tube furnace. It was flushed with N2 for 1 hour. Subsequently, the black substance treated in this way was heated to 300°C (heating rate of 300°C / h), maintained at this temperature for 2 hours, and then cooled naturally to room temperature.

[0105] Example 2-12

[0106] Adding nitrogen and sulfur as exogenous atoms

[0107] 500 mg of the black substance used in Example 2 was placed in an autoclave together with 1.5 g of urea and 30 mL of water and heated at 180° C. for 16 hours. The suspension was cooled naturally in an oven, washed with water and acetone, and dried in air.

[0108] Example 2-13

[0109] Adding nitrogen and sulfur as exogenous atoms

[0110] 500 mg of the black substance used in Example 2 was placed in an autoclave together with 1.5 g of thiourea and 30 mL of water, and heated at 180° C. for 16 hours. The suspension was cooled naturally in an oven, then washed with water and acetone, and dried in air.

[0111] Example 2-14

[0112] Adding sulfur as an exogenous atom

[0113] 500 mg of the black substance used in Example 2 was placed in an autoclave together with 50 mg of elemental sulfur (S8) and 30 mL of water and heated at 180°C for 16 hours. The suspension was cooled naturally in an oven, then washed with water and acetone, and dried in air.

[0114] Example 2-15

[0115] Adding phosphorus as an exogenous atom

[0116] 500 mg of the black substance used in Example 2 was placed in an autoclave together with 50 mg of red phosphorus and 30 mL of water, and heated at 180° C. for 16 hours. The suspension was cooled naturally in an oven, then washed with water and acetone, and dried in air.

[0117] Example 2-16

[0118] Adding sulfur as an exogenous atom

[0119] 100 mg of the black substance used in Example 2 was ground and placed in a tube furnace, heated to 300° C. (heating rate 300° C. / h) under H 2 S gas flow, and maintained at the temperature for 3 hours, and then cooled naturally.

[0120] Example 2-17

[0121] Adding Boron as an Exogenous Atom

[0122] 500 mg of the black substance used in Example 2 was placed in an autoclave together with 700 mg of boric acid or diboric acid oxide and 30 mL of water and heated at 180° C. for 16 hours. The suspension was cooled naturally in an oven, washed with water and acetone, and dried in air.

[0123] Example 2-18

[0124] Adding nitrogen as an exogenous atom

[0125] 500 mg of the black substance used in Example 2 was placed in an autoclave together with 3 ml of hydrazine and 27 mL of water and heated at 180° C. for 16 hours. The suspension was cooled naturally in an oven, washed with water and acetone, and dried in air.

[0126] Example 3

[0127] Recyclate from old drive batteries of electric vehicles (especially electric cars) is used as black mass. This recyclate is a recycled material based on lithium iron phosphate (LFP) batteries and is provided by Duesenfeld GmbH (a limited company located in Winderberg, Germany). The graphite-supported one or more noble metal-free metal oxides in the black mass include (multiple) iron oxides. The powder diffraction pattern of the black mass is as follows Figure 5 shown.

[0128] Example 3-1

[0129] Adding nitrogen as an exogenous atom

[0130] 100 mg of the black substance used in Example 3 was first flushed with NH 3 in a tube furnace for 2 hours, then heated to 300° C. (heating rate 300° C. / h), and after 6 hours, naturally cooled to room temperature.

[0131] Example 3-2

[0132] Chemical modification of substantia nigra

[0133] 100 mg of the black substance used in Example 3 was ground and heated in an aqueous solution containing 2M formic acid and 6% H2O2 at 80°C for 2 hours. After heating, the material was washed with water and acetone and dried in air.

[0134] Example 3-3

[0135] Chemical modification of substantia nigra

[0136] 100 mg of the black substance used in Example 3 was ground and heated in a 1 M KOH aqueous solution at 80° C. for 2 hours. The material was then washed with water and acetone and dried in air.

[0137] Reference numeral sequence:

[0138] 1 Preparation

[0139] 2 Introduction

[0140] 3 Apply

[0141] 4 OK

[0142] 5 Modification

[0143] 6 Add

[0144] 10Electrolyzer

[0145] 11-electrode

[0146] 12 Another electrode

[0147] 14 Solution

[0148] 15 Black substance

[0149] 16 Voltage Source

[0150] 17 Coating

[0151] 20 Another electrolytic cell

[0152] 21 Anode

[0153] 22 cathode

[0154] 24 Alkaline solution

[0155] 25 Diaphragm

[0156] 26 Another voltage source

[0157] 27 Base material

[0158] 28 Another substrate

Claims

1. A method for manufacturing a graphite-containing metal oxide electrode, comprising the following steps: a) preparing (1) an electrolytic cell (10) comprising an electrode (11), another electrode (12) and an aqueous and / or non-aqueous carbon-free and cyanide-free solution (14), b) introducing (2) a black mass (15) comprising a graphite-supported metal oxide free of noble metals and a proton source into a solution (14) in an electrolytic cell (10), c) applying (3) voltage to the electrode (11) and another electrode (12) to deposit the noble metal-free metal oxide and graphite provided by the black substance (15) on the electrode (11), thereby forming a graphite-containing metal oxide coating (17) on the electrode (11) to produce a graphite-containing metal oxide electrode.

2. The method according to claim 1, characterized in that The black mass (15) is a recyclate, wherein the recyclate preferably comes from recycled material of old drive batteries for electric vehicles, in particular electric cars.

3. The method according to claim 1 or 2, characterized in that: The graphite-supported one or more noble metal-free metal oxides include a mixture of Ni, Co and / or Mn and at least one oxide thereof, or a mixture of (multiple) iron oxides or Ni, Co, Al oxides.

4. A method according to any preceding claim, characterised in that Before step a) or step b), perform the following steps: - determine the composition and morphology of the substantia nigra (15) and - Chemically modifying (5) the substantia nigra (15) according to the determined composition and morphology, including adjusting the percentage of metal (oxide) present in the substantia nigra.

5. A method according to any preceding claim, characterised in that Before step a) or b), perform the following steps: - Adding (6) one or more exogenous atoms (promoting atoms) to the graphite carrier of the black mass (15), wherein the exogenous atoms are preferably nitrogen, sulfur, phosphorus and / or boron, more preferably nitrogen and / or sulfur.

6. A method according to any preceding claim, characterised in that The solution (14) is selected from cyclic ethers and / or azeotropic alcohol-water mixtures.

7. A graphite-containing metal oxide electrode produced according to a method as claimed in any preceding claim.

8. Graphite-containing metal oxide electrodes are used for (photo)electrochemical water splitting to produce hydrogen and / or oxygen.

9. Electrolyser (20) for producing hydrogen and oxygen by (photo)electrochemical water splitting, comprising a graphite-containing metal oxide electrode according to claim 7 as cathode (22) and / or a graphite-containing metal oxide electrode according to claim 7 as anode (21).

10. The electrolytic cell (20) according to claim 9, characterized in that The electrolyte is an alkaline solution.

Citation Information

Patent Citations

  • Metal chalcogenide thin layer electrode, method for production thereof and use thereof