Positive electrode active material for lithium ion secondary battery, and method for producing positive electrode active material for lithium ion secondary battery

By adding aluminum oxide, titanium oxide and other added particles to the positive electrode active substance of the lithium-ion secondary battery, it is dispersed on the surface of lithium-metal composite oxide particles to form an artificial solid electrolyte interface, which solves the insufficient circulation characteristics of lithium-ion secondary battery Problem, achieving higher battery capacity and output performance.

CN118985053APending Publication Date: 2024-11-19SUMITOMO METAL MINING CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380031937.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-01
Filing Date
2023-03-30
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The circulation characteristics of existing lithium-ion secondary batteries are insufficient, making it difficult to meet the needs of high energy density and durability.

Method used

Using positive electrode active substances containing lithium metal composite oxide particles and aluminum oxide, titanium oxide, magnesium oxide, silicon oxide, zirconium oxide and other added particles, the artificial solid electrolyte interface is formed by dispersing and adding particles on the surface of lithium metal composite oxide particles. , inhibit side reactions between the electrolyte and lithium metal composite oxide particles and improve circulation characteristics.

Benefits of technology

The cycle characteristics of lithium-ion secondary batteries are significantly improved, the increase in positive electrode resistance is suppressed, and the battery characteristics are maintained or improved. It is suitable for electric vehicle batteries with high capacity and high output.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118985053A_ABST
    Figure CN118985053A_ABST
Patent Text Reader

Abstract

A positive electrode active material for a lithium ion secondary battery, which contains lithium metal composite oxide particles and one or more additive particles selected from alumina particles, titanium oxide particles, magnesium oxide particles, silicon oxide particles, and zirconia particles, and which has a specific surface area of 0.25-4.0 m2 / g (inclusive).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a positive electrode active material for a lithium ion secondary battery and a method for producing the positive electrode active material for a lithium ion secondary battery. Background Art

[0002] In recent years, with the popularity of portable electronic devices such as mobile phones and laptops, there is a strong desire for the development of small and lightweight secondary batteries with high energy density and durability. In addition, as batteries for electric vehicles starting with power tools and hybrid vehicles, there is a strong desire for the development of high-output secondary batteries. Furthermore, in addition to the above-mentioned required characteristics, there is a high demand for secondary batteries with high durability that are difficult to deteriorate even after repeated use.

[0003] As a secondary battery that meets such requirements, there is a lithium ion secondary battery. A lithium ion secondary battery is composed of a negative electrode, a positive electrode, and an electrolyte, etc., and a material that allows lithium to be separated and inserted is used as the active material of the negative electrode and the positive electrode. Lithium ion secondary batteries have high energy density, output characteristics, and durability as described above.

[0004] Research and development of lithium-ion secondary batteries is currently in full swing, and among them, lithium-ion secondary batteries using layered or spinel lithium metal composite oxides as positive electrode materials can obtain a high voltage of 4V and are therefore put into practical use as batteries with high energy density.

[0005] As positive electrode materials for such lithium-ion secondary batteries, lithium cobalt composite oxide (LiCoO2), which is relatively easy to synthesize, lithium nickel composite oxide (LiNiO2), which uses nickel that is cheaper than cobalt, and lithium nickel cobalt manganese composite oxide (LiNiO2) have been proposed. 1 / 3 Co 1 / 3 Mn 1 / 3 O2), lithium manganese composite oxide (LiMn2O4), lithium nickel manganese composite oxide (LiNi 0.5 Mn 0.5 O2) and other lithium metal composite oxides.

[0006] In recent years, lithium ion secondary batteries have been required to have further improved battery characteristics. Therefore, positive electrode active materials for lithium ion secondary batteries that have improved battery characteristics when used in lithium ion secondary batteries have been required, and various studies have been conducted.

[0007] For example, Patent Document 1 proposes a coated particle for a lithium-ion secondary battery, characterized in that it comprises a positive electrode active material particle and a metal sulfide complexed on the surface of the positive electrode active material particle, the total mass of the metal sulfide is 1.0 to 5.0 mass % relative to the total mass of the positive electrode active material particle, and the metal sulfide has a layer structure.

[0008] [Prior art literature]

[0009] [Patent Literature]

[0010] [Patent Document 1] Japanese Patent Application Publication No. 2016-100101 Summary of the invention

[0011] [Problems to be solved by the invention]

[0012] However, in recent years, when used in lithium ion secondary batteries, there is a demand for positive electrode active materials for lithium ion secondary batteries with improved cycle characteristics.

[0013] Therefore, in view of the above-mentioned problems of the prior art, an object of one aspect of the present invention is to provide a positive electrode active material for a lithium ion secondary battery, which can improve the cycle characteristics when used in a lithium ion secondary battery.

[0014]

Methods to solve the problem

[0015] In order to solve the above-mentioned problems, according to one embodiment of the present invention, there is provided a positive electrode active material for a lithium ion secondary battery.

[0016] The invention comprises lithium metal composite oxide particles and one or more additional particles selected from aluminum oxide particles, titanium oxide particles, magnesium oxide particles, silicon oxide particles and zirconium oxide particles.

[0017] The specific surface area is 0.25m 2 / g or more, 4.0m 2 / g or less.

[0018] [Effects of the Invention]

[0019] According to one embodiment of the present invention, there is provided a positive electrode active material for a lithium ion secondary battery which can improve the cycle characteristics when used in a lithium ion secondary battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 This is a diagram for explaining the structure of a laminated battery produced in an experimental example.

[0021] Figure 2A This is a SEM image of the positive electrode active material obtained in Experimental Example 4.

[0022] Figure 2B This is a SEM image of the positive electrode active material obtained in Experimental Example 8.

[0023] Figure 3A This is a SEM image of the positive electrode active material obtained in Experimental Example 13.

[0024] Figure 3B This is a SEM image of the positive electrode active material obtained in Experimental Example 16.

[0025] Figure 4 SEM image of the positive electrode active material obtained in Experimental Example 22.

[0026] Figure 5 This is a SEM image of the positive electrode active material obtained in Experimental Example 25.

[0027] Fig. 6A This is a SEM image of the positive electrode active material obtained in Experimental Example 26.

[0028] Figure 6B for Fig. 6A A partial enlarged view of .

[0029] Figure 7 This is a cross-sectional SEM image of the positive electrode active material obtained in Experimental Example 28.

[0030] Figure 8 This is a cross-sectional SEM image of the positive electrode active material obtained in Experimental Example 30.

[0031] Fig. 9A This is a SEM image of the positive electrode active material obtained in Experimental Example 32.

[0032] Fig. 9B for Fig. 9A A partial enlarged view of .

[0033] Fig. 9C This is a SEM image of the positive electrode active material obtained in Experimental Example 34.

[0034] Fig.9D for Fig. 9C A partial enlarged view of . DETAILED DESCRIPTION

[0035] Hereinafter, a mode for carrying out the present invention will be described with reference to the drawings, but the present invention is not limited to the following embodiment, and various modifications and substitutions may be added to the following embodiment without departing from the scope of the present invention.

[0036] [Positive electrode active material for lithium ion secondary batteries]

[0037] The positive electrode active material for lithium ion secondary battery of this embodiment (hereinafter simply referred to as "positive electrode active material") may contain lithium metal composite oxide particles and one or more additional particles selected from aluminum oxide particles, titanium oxide particles, magnesium oxide particles, silicon oxide particles and zirconium oxide particles.

[0038] In addition, the specific surface area of ​​the positive electrode active material of this embodiment is 0.25 m 2 / g or more, 4.0m 2 / g or less.

[0039] The positive electrode active material of this embodiment may contain the lithium metal composite oxide particles and the additive particles as described above. In addition, the positive electrode active material of this embodiment may also be composed only of lithium metal composite oxide particles and the additive particles. However, the presence of unavoidable impurities is not excluded at this time.

[0040] Hereinafter, the lithium metal composite oxide particles and the additive particles contained in the positive electrode active material of the present embodiment will be described.

[0041] (Lithium Metal Composite Oxide Particles)

[0042] The lithium metal composite oxide particles are particles of a lithium metal composite oxide which is an oxide containing lithium and an arbitrary metal component.

[0043] The specific composition of the lithium metal composite oxide is not particularly limited, and various lithium metal composite oxides that allow lithium ions to be inserted and desorbed, that is, that allow lithium ions to be adsorbed and desorbed, can be appropriately used. As the lithium metal composite oxide, for example, one or more selected from lithium metal composite oxides having a spinel structure, lithium metal composite oxides having a layered structure, lithium metal composite oxides having an olivine structure, etc. can be used.

[0044] The lithium metal composite oxide having a spinel structure may contain lithium (Li), manganese (Mn), nickel (Ni), and element M1 (M1) in a ratio of Li:Mn:Ni:M1=a1:2-x1-y1:x1:y1, for example, in terms of the amount of substance. Here, a1, x1, and y1 in the above formula preferably satisfy 0.96≦a1≦1.25, 0.40≦x1≦0.60, and 0≦y1≦0.20, respectively.

[0045] The element M1 may be one or more elements selected from the group consisting of magnesium (Mg), aluminum (Al), silicon (Si), titanium (Ti), chromium (Cr), iron (Fe), cobalt (Co), copper (Cu), and zinc (Zn).

[0046] The lithium metal composite oxide having a spinel structure can be represented by the general formula

[0047] Li a1 Mn 2-x1-y1 Ni x1 M1 y1 O 4+α In the above general formula, a1, x1, and y1 have been described, so their description is omitted here. In addition, α is preferably -0.2≦α≦0.2, for example.

[0048] The lithium metal composite oxide having a layered structure may contain, for example, lithium (Li), nickel (Ni), cobalt (Co), and element M2 (M2) in a ratio of Li:Ni:Co:M2=a2:1-x2-y2:x2:y2 in terms of the amount of substance. Here, a2, x2, and y2 in the above formula preferably satisfy 0.95≦a2≦1.50, 0≦x2≦0.35, and 0≦y2≦0.35, respectively. In addition, element M2 may be one or more elements selected from magnesium (Mg), calcium (Ca), aluminum (Al), silicon (Si), iron (Fe), chromium (Cr), manganese (Mn), vanadium (V), molybdenum (Mo), tungsten (W), niobium (Nb), titanium (Ti), zirconium (Zr), and tantalum (Ta).

[0049] The layered lithium metal composite oxide can be represented by the general formula Li a2 Ni 1-x2-y2 Co x2 M2 y2 O 2+β In the above general formula, a2, x2, and y2 are already described, so their description is omitted here. In addition, β is preferably 0≦β≦0.10, for example.

[0050] The lithium metal composite oxide having an olivine structure may contain, for example, lithium (Li), element M3 (M3), phosphorus (P), and oxygen (O), and may be represented by the general formula LiM3PO 4+γ The element M3 may be, for example, one or more elements selected from Co, Ni, Mn, Fe, Mg, Nb, Ti, Al, and Zr, or VO. γ is preferably -0.2≦γ≦0.2.

[0051] The average particle size of the lithium metal composite oxide particles is not particularly limited, but is preferably, for example, 2 μm or more and 20 μm or less, and more preferably 3 μm or more and 18 μm or less.

[0052] The reason is that by setting the average particle size of the lithium metal composite oxide particles to 20 μm or less, the surface area of ​​the lithium metal composite oxide particles can be sufficiently increased, and the absorption and release of lithium ions between the electrolyte can be sufficiently promoted.

[0053] When the average particle size of the lithium metal composite oxide particles is 2 μm or more, the handleability can be improved, which is preferable.

[0054] The average particle size of the lithium metal composite oxide particles can be evaluated in the same manner as in the case of the added particles described below.

[0055] (Add Particles)

[0056] The inventors of the present invention have studied positive electrode active materials for lithium ion secondary batteries that can improve cycle characteristics when used in lithium ion secondary batteries. As a result, it was found that positive electrode active materials containing lithium metal composite oxide particles and additive particles can improve cycle characteristics when used in lithium ion secondary batteries.

[0057] The reason for this is not clear, but the mechanism for improving the cycle characteristics is presumed to be as follows.

[0058] By adding additive particles to the lithium metal composite oxide particles, the additive particles can be dispersed and arranged on the surface of the lithium metal composite oxide particles. In addition, as additive particles, for example, one or more selected from aluminum oxide particles, titanium oxide particles, magnesium oxide particles, silicon oxide particles and zirconium oxide particles can be used. The aluminum oxide particles, titanium oxide particles, magnesium oxide particles, silicon oxide particles and zirconium oxide particles used as additive particles have corrosion resistance. Therefore, it is believed that by dispersing and arranging the additive particles on the surface of the lithium metal composite oxide particles, the reaction that occurs between the electrolyte and the surface of the lithium metal composite oxide particles and causes the lithium metal composite oxide to deteriorate can be suppressed. That is, it is believed that the additive particles act as an artificial SEI (artificial solid electrolyte interface) to suppress the above-mentioned side reactions that occur between the electrolyte and the surface of the lithium metal composite oxide particles.

[0059] Here, the added particles are only arranged on the surface of the lithium metal composite oxide particles, and thus the movement of lithium ions between the electrolyte and the lithium metal composite oxide particles is not substantially hindered. Therefore, compared with the case where the added particles are not added, the cycle characteristics can be improved while maintaining or improving other battery characteristics.

[0060] As the additional particles, one or more selected from aluminum oxide particles, titanium oxide particles, magnesium oxide particles, silicon oxide particles, and zirconium oxide particles can be used as described above. That is, the additional particles can be any one of aluminum oxide particles, titanium oxide particles, magnesium oxide particles, silicon oxide particles, and zirconium oxide particles, or a mixture of two or more selected from aluminum oxide particles, titanium oxide particles, magnesium oxide particles, silicon oxide particles, and zirconium oxide particles.

[0061] When titanium oxide particles are used as added particles, the type of crystalline phase of titanium oxide contained therein is not particularly limited. In addition, the crystalline phase can be any one of a single phase and a common phase, without particular limitation. Here, in particular, based on the viewpoint of improving cycle characteristics, the titanium oxide crystalline phase contained in the titanium oxide particles is preferably a single phase of rutile phase, anatase phase, or brookite phase, or the rutile phase is the main phase. In addition, the main phase mentioned here refers to the phase with the highest content ratio in terms of mass ratio.

[0062] When zirconium oxide particles are used as added particles, the type of crystal phase of zirconium oxide contained is not particularly limited. In addition, the crystal phase can be any one of a single phase and a common phase, without particular limitation, and calcium, magnesium, hafnium, etc. can be added to zirconium oxide as cubic stabilized zirconium. Here, in particular, based on the viewpoint of improving the cycle characteristics, the crystal phase of zirconium oxide contained in the zirconium oxide particles is preferably tetragonal as the main phase among monoclinic, tetragonal, and cubic. In addition, the main phase mentioned here refers to the phase with the highest content ratio in terms of mass ratio.

[0063] In the positive electrode active material of the present embodiment, the state of the added particles is not particularly limited, but it is preferred that the particles are dispersed on the surface of the lithium metal composite oxide particles to modify the surface of the lithium metal composite oxide particles.

[0064] The average particle size of the additive particles used in the positive electrode active material of the present embodiment is not particularly limited, but is preferably 300 nm or less, and more preferably 10 nm or more and 200 nm or less, for example.

[0065] By making the average particle size of the added particles used be less than 300nm, when adding to the lithium metal composite oxide particles, the added particles can be uniformly dispersed on the surface of the lithium metal composite oxide particles. At this time, the movement of lithium ions between the electrolyte and the lithium metal composite oxide particles is not hindered, and the cycle characteristics can be particularly improved while maintaining the battery characteristics. Furthermore, according to the research of the inventors of the present invention, the lithium ion secondary battery using the positive electrode active material of this embodiment can suppress the positive electrode resistance of SOC50% at low temperature and room temperature after repeated charge and discharge, compared with the lithium ion secondary battery using the positive electrode active material without the addition of the added particles. In addition, SOC refers to the state of charge, which can also be replaced by the charging rate.

[0066] The lower limit of the average particle size of the added particles used is not particularly limited, but is preferably 10 nm or more as described above because of excellent handleability.

[0067] There is no particular restriction on the method for obtaining the average particle size of the added particles, and it can be observed and measured using a scanning electron microscope (SEM) or a transmission electron microscope (TEM). For example, the added particles are first observed using a SEM or the like to obtain an image. In addition, there is no particular restriction on the magnification during observation, and it is preferably 50,000 times or more. There is no particular restriction on the upper limit of the magnification, and based on the viewpoint of efficient observation, it is preferably 1 million times or less, and more preferably 100,000 times or less. From the obtained image, 100 added particles are randomly selected, and a circumscribed circle circumscribed to the outline of each selected particle is drawn, and the diameter of such a circumscribed circle is used as the particle size of each particle. In addition, the average particle size of the 100 particles evaluated can be used as the average particle size of the added particles.

[0068] Furthermore, when one field of view does not contain 100 added particles, observation is performed in a plurality of fields of view, and a total of 100 particles can be selected from the plurality of fields of view.

[0069] The specific surface area of ​​the additional particles used is not particularly limited. When the additional particles are alumina particles, for example, a specific surface area of ​​20 m 2 / g or more, 180m 2 / g or less, more preferably 65m 2 / g or more, 180m 2 / g or less. By making the specific surface area of ​​the alumina particles 20m 2 / g or more, it can be made into sufficiently fine particles. Therefore, when added to lithium metal composite oxide particles, it can be uniformly dispersed on the surface of the lithium metal composite oxide particles. In addition, at this time, the movement of lithium ions between the electrolyte and the lithium metal composite oxide particles is not hindered, and the cycle characteristics can be improved while maintaining the battery characteristics.

[0070] In addition, by using alumina particles with a specific surface area of ​​180 m 2 / g or less is preferred because of excellent handleability.

[0071] When the added particles are titanium oxide particles, the specific surface area of ​​the titanium oxide particles is not particularly limited, but is preferably 30 m 2 / g or more, 180m 2 / g or less. By making the specific surface area of ​​titanium oxide particles 30m 2 / g or more, it can be made into sufficiently fine particles. Therefore, when added to lithium metal composite oxide particles, it can be evenly dispersed on the surface of the lithium metal composite oxide particles. In addition, at this time, the movement of lithium ions between the electrolyte and the lithium metal composite oxide particles will not be hindered, and the cycle characteristics can be improved while maintaining the battery characteristics.

[0072] In addition, by using titanium oxide particles with a specific surface area of ​​180 m 2 / g or less is preferred because of excellent handleability.

[0073] When the added particles are magnesium oxide particles, the specific surface area of ​​the magnesium oxide particles is not particularly limited, but is preferably 65 m 2 / g or more, 180m 2 / g or less. By making the specific surface area of ​​the magnesium oxide particles 65m 2 / g or more, it can be made into sufficiently fine particles. Therefore, when added to the lithium metal composite oxide particles, it can be uniformly dispersed on the surface of the lithium metal composite oxide particles. In addition, at this time, the movement of lithium ions between the electrolyte and the lithium metal composite oxide particles will not be hindered, and the cycle characteristics can be improved while maintaining the battery characteristics.

[0074] In addition, by using magnesium oxide with a specific surface area of ​​180 m 2 / g or less is preferred because of excellent handleability.

[0075] When the added particles are silicon oxide particles, the specific surface area of ​​the silicon oxide particles is not particularly limited, but is preferably 30 m 2 / g or more, 250m 2 / g or less. By making the specific surface area of ​​silicon oxide particles 30m 2 / g or more, it can be made into sufficiently fine particles. Therefore, when added to the lithium metal composite oxide particles, it can be uniformly dispersed on the surface of the lithium metal composite oxide particles. In addition, at this time, the movement of lithium ions between the electrolyte and the lithium metal composite oxide particles will not be hindered, and the cycle characteristics can be improved while maintaining the battery characteristics.

[0076] In addition, by using silicon oxide particles with a specific surface area of ​​250 m 2 / g or less is preferred because of excellent handleability.

[0077] When the added particles are zirconium oxide particles, the specific surface area of ​​the zirconium oxide particles is not particularly limited, but is preferably 30 m 2 / g or more, 250m 2 / g or less. By making the specific surface area of ​​the zirconium oxide particles 30m 2 / g or more, it can be made into sufficiently fine particles. Therefore, when added to lithium metal composite oxide particles, it can be evenly dispersed on the surface of the lithium metal composite oxide particles. In addition, at this time, the movement of lithium ions between the electrolyte and the lithium metal composite oxide particles will not be hindered, and the cycle characteristics can be improved while maintaining the battery characteristics.

[0078] In addition, by using zirconium oxide particles with a specific surface area of ​​250 m 2 / g or less is preferred because of excellent handleability.

[0079] The amount of the additional particles added to the lithium metal composite oxide particles is not particularly limited. For example, the ratio of the additional particles to the lithium metal composite oxide particles is preferably 0.025 mass % to 3.0 mass %, more preferably 0.05 mass % to 2.0 mass %.

[0080] When the ratio of the additive particles to the lithium metal composite oxide particles is 0.025 mass % or more, a sufficient amount of the additive particles are arranged on the surface of the lithium metal composite oxide particles, and the cycle characteristics can be particularly improved.

[0081] Here, the added particles do not allow lithium ions to be inserted or deintercalated, so excessive addition may reduce the battery capacity when used in lithium ion secondary batteries. Therefore, the ratio of the added particles to the lithium metal composite oxide particles is preferably 3.0 mass % or less.

[0082] The specific surface area of ​​the positive electrode active material in this embodiment can be 0.25 m 2 / g or more, 4.0m 2 / g or less, preferably 0.29m 2 / g or more, 3.8m 2 / g or less.

[0083] The reason is that by setting the specific surface area of ​​the positive electrode active material of this embodiment to 0.25 m 2 / g or more means that a sufficient amount of the additive particles are arranged on the surface of the lithium metal composite oxide particles. Therefore, the reaction between the electrolyte and the surface of the lithium metal composite oxide particles that deteriorates the lithium metal composite oxide is suppressed, and the cycle characteristics can be improved.

[0084] On the other hand, by setting the specific surface area of ​​the positive electrode active material of this embodiment to 4.0 m 2 / g or less, it is possible to suppress the excessive amount of added particles arranged on the surface of the lithium metal composite oxide particles, and when used in a lithium ion secondary battery, the battery capacity can be sufficiently increased.

[0085] The positive electrode active material of the present embodiment preferably has a specific surface area that is predetermined according to the particle structure of the lithium metal composite oxide serving as a base material.

[0086] For example, when the lithium metal composite oxide as the matrix material has a porous structure, the specific surface area of ​​the positive electrode active material of this embodiment is preferably 1.0 m 2 / g or more, 4.0m 2 / g or less, more preferably 1.2m 2 / g or more, 3.8m 2 / g or less.

[0087] For example, when the lithium metal composite oxide as the matrix material has a hollow structure, the specific surface area of ​​the positive electrode active material of this embodiment is preferably 0.50 m 2 / g or more, 2.5m 2 / g or less, more preferably 0.55m 2 / g or more, 2.3m 2 / g or less.

[0088] When the lithium metal composite oxide as the matrix material has a solid structure, the specific surface area of ​​the positive electrode active material of this embodiment is preferably 0.25 m 2 / g or more, 2.0m 2 / g or less, more preferably 0.29m 2 / g or more, 1.8m 2 / g or less.

[0089] In addition, a porous structure refers to a particle structure containing voids dispersed throughout the particle. In the case of a porous structure, the average value of the void ratio measured on the cross section of the lithium metal composite oxide particles is 15% or more. In the case of a porous structure, the upper limit of the average value of the void ratio measured on the cross section of the lithium metal composite oxide particles is not particularly limited, and is preferably 85% or less, for example.

[0090] The hollow structure refers to a particle structure having a hollow portion consisting of a space arranged in the center of the particle and an outer shell portion arranged outside the hollow portion. In the case of the hollow structure, the average value of the porosity measured on the cross section of the lithium metal composite oxide particle is 15% or more. In the case of the hollow structure, the upper limit of the average value of the porosity measured on the cross section of the lithium metal composite oxide particle is not particularly limited, for example, preferably 85% or less.

[0091] The solid structure refers to a particle having almost no voids inside the particle, and the average value of the void ratio measured on the particle cross section is less than 15%.

[0092] The average value of the porosity in the cross section of the lithium metal composite oxide particles can be determined by the following procedure.

[0093] First, after the particle group of lithium metal composite oxide as the measurement object is embedded in the resin, the cross section of the particle group is exposed by cutting with a cross-section polisher (CP) or the like, and the cross section of the exposed particle group is photographed with a scanning electron microscope. Next, the cross-sectional image of the obtained particle group is analyzed by using image analysis software, and the void portion is identified as a black area and the dense portion of the shell portion is identified as a white area. In addition, for more than 20 particle cross sections, the porosity of each particle is calculated by the following formula (A).

[0094] (Void ratio (%)) = [black region area / (black region area+white region area) × 100]···(A)

[0095] In addition, as particles for calculating the porosity, it is desirable to select particles whose particle diameter is consistent with D which can be confirmed from the particle size distribution, etc. 50 Particles with substantially the same particle size. Here, 50 Particles with substantially equal particle sizes refer to particles with a particle size preferably in the range of D 50 Particles within ±1.0μm.

[0096] By calculating the average of the calculated porosities of the individual particles, the average porosity of the lithium metal composite oxide can be obtained.

[0097] [Method for producing positive electrode active material for lithium ion secondary battery]

[0098] Next, a configuration example of a method for producing a positive electrode active material for a lithium ion secondary battery according to the present embodiment (hereinafter simply referred to as “a method for producing a positive electrode active material”) will be described.

[0099] According to the method for producing a positive electrode active material of the present embodiment, the positive electrode active material described above can be produced. Therefore, a part of the matters that have been described will be omitted.

[0100] The method for producing a positive electrode active material for a lithium ion secondary battery of the present embodiment may include a mixing step of mixing lithium metal composite oxide particles and one or more additional particles selected from aluminum oxide particles, titanium oxide particles, magnesium oxide particles, silicon oxide particles, and zirconium oxide particles.

[0101] In addition, the mixing step may be performed so that the specific surface area of ​​the obtained positive electrode active material is 0.25 m 2 / g or more, 4.0m 2 / g or less.

[0102] The lithium metal composite oxide particles and the additional particles have been described in the positive electrode active material for lithium ion secondary batteries, so their description is omitted here. In addition, as the additional particles, particles with an average particle diameter of 300 nm or less are preferably used.

[0103] In the mixing step, the lithium metal composite oxide particles and the added particles can be mixed using a general mixer, for example, one or more selected from a vibration mixer, a Roediger mixer, a Julia mixer, a V-type blender, etc. The mixing conditions in the mixing step are not particularly limited, but the conditions are preferably selected so that the components as the raw materials are fully mixed to a degree that the morphology of the raw material particles such as the lithium metal composite oxide particles is not destroyed.

[0104] The mixing ratio of the lithium metal composite oxide particles and the additive particles is not particularly limited. For example, as described above, the two materials are preferably weighed and mixed so that the ratio of the additive particles to the lithium metal composite oxide particles is 0.025 mass % or more and 3.0 mass % or less.

[0105] Here, in the mixing step, it is preferred that the specific surface area of ​​the positive electrode active material obtained after the mixing step is 0.25 m 2 / g or more, 4.0m 2 / g or less, the lithium metal composite oxide particles and the additive particles are selected, and their mixing ratio is selected.

[0106] [Lithium-ion secondary battery]

[0107] The lithium ion secondary battery (hereinafter also referred to as “secondary battery”) of the present embodiment may include a positive electrode including the positive electrode active material.

[0108] Hereinafter, each component is described separately with respect to a configuration example of a secondary battery of the present embodiment. The secondary battery of the present embodiment, for example, contains a positive electrode, a negative electrode and a non-aqueous electrolyte, and is composed of the same components as a general lithium-ion secondary battery. In addition, the embodiments described below are only examples, and the lithium-ion secondary battery of the present embodiment is based on the following embodiments as a starting point, and can be implemented in various modified and improved forms based on the knowledge of practitioners. In addition, the use of the secondary battery is not particularly limited.

[0109] (positive electrode)

[0110] The positive electrode included in the secondary battery of this embodiment may contain the positive electrode active material.

[0111] An example of a method for manufacturing a positive electrode is described below. First, the positive electrode active material (powder), a conductive material, and a binder are mixed to form a positive electrode composite material, and further, activated carbon, a solvent for viscosity adjustment, etc. may be added as needed, and the mixture is kneaded to prepare a positive electrode composite material slurry.

[0112] The mixing ratio of each material in the positive electrode composite material can be adjusted according to the application because it is a factor that determines the performance of the lithium ion secondary battery. The mixing ratio of the materials can be the same as that of the positive electrode of the known lithium ion secondary battery. For example, when the total mass of the solid components of the positive electrode composite material excluding the solvent is 100 mass%, it can contain the following proportions: 60 mass% or more and 95 mass% or less of the positive electrode active material, 1 mass% or more and 20 mass% or less of the conductive material, and 1 mass% or more and 20 mass% or less of the adhesive.

[0113] The obtained positive electrode composite slurry is applied on the surface of a current collector made of, for example, aluminum foil, and dried to disperse the solvent to produce a sheet-shaped positive electrode. If necessary, in order to increase the electrode density, pressure may be applied by roller pressing or the like. The sheet-shaped positive electrode thus obtained may be cut into appropriate sizes according to the intended battery and provided for battery production.

[0114] As the conductive material, for example, graphite (natural graphite, artificial graphite, expanded graphite, etc.), acetylene black, Ketjen Black (registered trademark), and other carbon black materials can be used.

[0115] As the adhesive (binder), which plays the role of connecting the active material particles, one or more selected from polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), fluororubber, ethylene propylene diene rubber, styrene butadiene, cellulose resin and polyacrylic acid can be used.

[0116] Positive electrode active material, conductive material, etc. can be dispersed as needed, and a solvent for dissolving the adhesive can be added to the positive electrode composite material. As the solvent, an organic solvent such as N-methyl-2-pyrrolidone can be used. In addition, activated carbon can be added to the positive electrode composite material in order to increase the double electric layer capacitance.

[0117] The method for manufacturing the positive electrode is not limited to the above examples, and other methods may be used. For example, the positive electrode composite material may be pressed into shape and then dried in a vacuum atmosphere.

[0118] (negative electrode)

[0119] The negative electrode can use metal lithium, lithium alloy, etc. In addition, the following negative electrode can be used, which is formed by coating the negative electrode composite material on the surface of a metal foil current collector such as copper, drying it, and compressing it as needed to increase the electrode density. The negative electrode composite material is a mixture of a negative electrode active material that allows lithium ions to be adsorbed and desorbed, a binder, and an appropriate solvent is added to make it a slurry.

[0120] As the negative electrode active material, for example, natural graphite, artificial graphite, phenol resin and other organic compound sintered bodies and carbon material powders such as coke can be used. At this time, as the negative electrode binder, as with the positive electrode, a fluorine-containing resin such as PVDF can be used, and as a solvent for dispersing these active materials and the binder, an organic solvent such as N-methyl-2-pyrrolidone can be used.

[0121] (Diaphragm)

[0122] A separator may be interposed between the positive electrode and the negative electrode as required. The separator separates the positive electrode and the negative electrode and contains electrolytes. A known film such as polyethylene, polypropylene, or a film having a large number of tiny pores may be used.

[0123] (Non-aqueous electrolyte)

[0124] As the nonaqueous electrolyte, for example, a nonaqueous electrolytic solution can be used.

[0125] As the non-aqueous electrolyte, for example, a lithium salt as a supporting salt dissolved in an organic solvent can be used. In addition, as the non-aqueous electrolyte, a lithium salt dissolved in an ionic liquid can be used. In addition, an ionic liquid refers to a salt that is composed of cations and anions other than lithium ions and is liquid at room temperature.

[0126] As the organic solvent, one selected from cyclic carbonates such as ethylene carbonate, propylene carbonate, butylene carbonate and trifluoropropylene carbonate, chain carbonates such as diethyl carbonate, dimethyl carbonate, ethyl methyl carbonate and dipropyl carbonate, further ether compounds such as tetrahydrofuran, 2-methyltetrahydrofuran and dimethoxyethane, sulfur compounds such as ethyl methyl sulfone and butane sultone, phosphorus compounds such as triethyl phosphate and trioctyl phosphate, etc. can be used alone, or two or more can be used in combination.

[0127] As supporting salts, LiPF6, LiBF4, LiClO4, LiAsF6, LiN(CF3SO2)2, and complex salts thereof can be used. Furthermore, the non-aqueous electrolyte solution can contain a radical scavenger, a surfactant, a flame retardant, and the like.

[0128] In addition, as the non-aqueous electrolyte, a solid electrolyte can be used. Solid electrolytes have the property of being able to withstand high voltages. Examples of solid electrolytes include inorganic solid electrolytes and organic solid electrolytes.

[0129] Examples of the inorganic solid electrolyte include oxide-based solid electrolytes and sulfide-based solid electrolytes.

[0130] There are no particular limitations on the oxide-based solid electrolyte, and for example, an oxide-based solid electrolyte containing oxygen (O) and having lithium ion conductivity and electronic insulation can be used appropriately. For example, lithium phosphate (Li3PO4), Li3PO4N X 、LiBO2N X , LiNbO3, LiTaO3, Li2SiO3, Li4SiO4-Li3PO4, Li4SiO4-Li3VO4, Li2O-B2O3-P2O5, Li2O-SiO2, Li2O-B2O3-ZnO, Li 1+X Al X Ti 2-X (PO4)3(0≦X≦1), Li 1+X Al X Ge 2-X (PO4)3(0≦X≦1), LiTi2(PO4)3, Li 3X La2 / 3-X TiO3(0≦X≦2 / 3), Li5La3Ta2O 12 、Li7La3Zr2O 12 、Li6BaLa2Ta2O 12 , Li 3.6 Si 0.6 P 0.4 One or more selected from O4, etc.

[0131] As sulfide-based solid electrolytes, there are no particular restrictions, and for example, those containing sulfur (S) and having lithium ion conductivity and electronic insulation can be appropriately used. As sulfide-based solid electrolytes, for example, one or more selected from Li2S-P2S5, Li2S-SiS2, LiI-Li2S-SiS2, LiI-Li2S-P2S5, LiI-Li2S-B2S3, Li3PO4-Li2S-Si2S, Li3PO4-Li2S-SiS2, LiPO4-Li2S-SiS, LiI-Li2S-P2O5, LiI-Li3PO4-P2S5, etc. can be used.

[0132] In addition, as the inorganic solid electrolyte, other than those mentioned above can be used, for example, Li3N, LiI, Li3N-LiI-LiOH, etc. can be used.

[0133] The organic solid electrolyte is not particularly limited as long as it is a polymer compound exhibiting ion conductivity, and for example, polyethylene oxide, polypropylene oxide, copolymers thereof, etc. can be used. In addition, the organic solid electrolyte may contain a supporting salt (lithium salt).

[0134] (Shape and structure of secondary battery)

[0135] The lithium ion secondary battery of the present embodiment as described above can be in various shapes such as cylindrical and stacked. In any shape, when a non-aqueous electrolyte is used as a non-aqueous electrolyte, the secondary battery of the present embodiment can be structured as follows: the positive electrode and the negative electrode are stacked into an electrode body through a separator, the obtained electrode body is impregnated with a non-aqueous electrolyte, and the positive electrode current collector and the positive terminal connected to the outside and the negative electrode current collector and the negative terminal connected to the outside are connected with a current collecting lead, etc., and are sealed in a battery case.

[0136] In addition, as described above, the secondary battery of this embodiment is not limited to the form of using a non-aqueous electrolyte as a non-aqueous electrolyte, and can be, for example, a secondary battery using a solid non-aqueous electrolyte, i.e., an all-solid-state battery. In the case of an all-solid-state battery, the structure other than the positive electrode active material can be changed as needed.

[0137] The secondary battery of this embodiment can be used for various purposes. The secondary battery of this embodiment can be used as a high-capacity, high-output secondary battery, and is therefore suitable for, for example, a power source for a small portable electronic device (laptop computer, mobile phone terminal, etc.) that usually requires a high capacity, and is also suitable for a power source for an electric vehicle that requires a high output.

[0138] In addition, the secondary battery of this embodiment is suitable as a power source for electric vehicles that are restricted by the carrying space because it can be miniaturized and have high output. In addition, the secondary battery of this embodiment is not only a power source for electric vehicles driven purely by electrical energy, but can also be used as a power source for so-called hybrid vehicles used in conjunction with combustion mechanisms such as gasoline engines and diesel engines.

[0139] [Example]

[0140] Hereinafter, the present invention will be further described in detail by way of examples, but the present invention is not limited by these examples.

[0141] First, the positive electrode active material and the evaluation method of the secondary battery obtained in the following experimental examples will be described.

[0142] (Evaluation of positive electrode active material)

[0143] The obtained positive electrode active material was evaluated as follows.

[0144] (a) Added particles, average particle size of lithium metal composite oxide particles

[0145] First, use a scanning electron microscope (SEM, Hitachi High-Tech Co., Ltd., scanning electron microscope S-4700) to observe the added particles contained in the positive electrode active material prepared in the following experimental example at 50,000 times to obtain an image. From the obtained image, select 100 added particles, draw a circumscribed circle circumscribed to the outline of each selected particle, and use such a circumscribed circle diameter as the particle size of each particle. Then, the average particle size of the 100 particles evaluated is used as the average particle size of the added particles possessed by the positive electrode active material.

[0146] The average particle size of the lithium metal composite oxide particles was measured in the same manner.

[0147] (b) Specific surface area

[0148] The specific surface areas of the positive electrode active material and the added particles of the raw material were measured using a flow-type gas adsorption method specific surface area measuring apparatus (Multisorb, manufactured by Yuasa Ionics Co., Ltd.).

[0149] (c) SEM observation

[0150] The positive electrode active materials prepared in the following Experimental Examples 4, 8, 13, 16, 22, 25, 26, 32, and 34 were observed using a scanning electron microscope (Scanning Electron Microscope S-4700 manufactured by Hitachi High-Technologies Corporation).

[0151] In addition, regarding the positive electrode active materials prepared in Experimental Examples 28 and 30, particle cross sections were observed.

[0152] (Evaluation of battery characteristics)

[0153] The positive electrode resistance and cycle characteristics before and after cycling were evaluated using the laminated batteries prepared in the following experimental examples. In addition, the positive electrode resistance was evaluated only for Experimental Examples 1 to 5, 8 to 21, and 24 to 34. For the samples for which the positive electrode resistance was not evaluated, the cycle characteristics were evaluated after conditioning in the same manner except that the positive electrode resistance was not measured.

[0154] The laminated batteries prepared in the following experimental examples were subjected to the following cycle conditioning for 5 times, and were heated in a thermostatic chamber maintained at 25°C at a current density of 0.3 mA / cm 2 , charged to a cut-off voltage of 4.2 V, rested for 10 minutes, and then discharged to a cut-off voltage of 2.5 V. In addition, the capacity when discharged to 2.5 V when one cycle was performed under the same conditions after adjustment was taken as the initial discharge capacity.

[0155] Next, the laminated battery was charged to 50% of the initial discharge capacity, rested for 10 minutes, and discharged at a 1C rate for 10 seconds, and the voltage change during the 10-second discharge at the 1C rate was measured.

[0156] According to Ohm's law, the resistance value (DC-IR) is calculated by dividing the voltage change by the current value, and is used as the battery DC resistance at SOC50%, 1C, 10 seconds, and 25°C. At this time, the laminated batteries prepared in the following multiple experimental examples use the same components except for the positive electrode active material, so the above battery DC resistance is regarded as the resistance of the positive electrode active material for evaluation.

[0157] Furthermore, after cooling the laminated battery to -10°C, the battery DC resistance, that is, the positive electrode resistance (positive electrode resistance before cycling) was measured in the same manner.

[0158] In Tables 1 and 2, the columns of positive electrode resistance before cycling indicate that the 25° C. column indicates the positive electrode resistance measured at 25° C., and the −10° C. column indicates the positive electrode resistance measured at −10° C. The same is true for the positive electrode resistance after cycling described later.

[0159] After measuring the positive electrode resistance before the cycle or the initial discharge capacity, the following cycle was repeated 500 times in a constant temperature chamber maintained at 45°C at a current density of 2.0 mA / cm 2 , charged to the specified cut-off voltage, rested for 10 minutes, and discharged at a 2C rate to a cut-off voltage of 2.5V. Then calculate and evaluate the ratio of the discharge capacity of the 500th cycle after adjustment to the discharge capacity of the first cycle, that is, the capacity retention rate. In addition, when performing the above-mentioned repeated charge and discharge, for Experimental Examples 1 to 9, 17, 18, 21 to 25, 28 to 31, the battery was charged to a cut-off voltage of 4.3V, and for Experimental Examples 10 to 16, 19, 20, 26, 27, 32 to 34, the battery was charged to a cut-off voltage of 4.2V. Table 1 shows the discharge capacity of the first cycle, the discharge capacity of the 500th cycle, and the cycle capacity retention rate (capacity retention rate).

[0160] After 500 cycles of charge and discharge, the battery DC resistance at 25° C. and −10° C., that is, the positive electrode resistance value (positive electrode resistance after cycles) was measured and calculated in the same manner as before the 500 cycles of charge and discharge.

[0161] The following describes the manufacturing conditions and evaluation results of the positive electrode active material in each experimental example. Experimental examples 1 to 7, 10, 11, 13 to 15, 17 to 26, 28, 30, 32, and 33 are examples, and Experimental examples 8, 9, 12, 16, 27, 29, 31, and 34 are comparative examples.

[0162] [Experimental Example 1]

[0163] (1) Production of positive electrode active material

[0164] The average particle size of LiNi 0.52 Mn 0.28 Co 0.20 100 g of a lithium metal composite oxide particle having a layered structure represented by O2 and having an average particle size of 54 nm and a specific surface area of ​​104 m 2 0.053 g of alumina particles of 0.1 g / g were mixed thoroughly with a vibration mixer to obtain the positive electrode active material of this experimental example (mixing process). As a vibration mixer, a model of TURBULA Type T2C manufactured by Willy A. Bachofen (WAB) was used. The same vibration mixer was also used to implement the mixing process in the following other experimental examples.

[0165] Regarding the particles of lithium metal composite oxide used in this experimental example, the particle cross-sectional structure was observed and the average value of the porosity in the cross section was calculated. Specifically, after the particle group of lithium metal composite oxide was embedded in the resin, it was cut by a cross-section polisher (CP) to expose the cross section of the particle group, and the cross section of the exposed particle group was photographed with a scanning electron microscope. As a result, it can be confirmed that the particles of lithium metal composite oxide contain almost no voids and have a solid structure.

[0166] The cross-sectional image of the obtained particle group was analyzed using image analysis and measurement software (WinRoof 6.1.1 manufactured by Mitani Shoji Co., Ltd.), and the void portion was identified as a black region and the dense portion as a white region, and the void ratio was determined for 20 particles.

[0167] As 20 particles for determining the porosity, 20 particles having a particle size of 50% of the volume cumulative value D in the particle size distribution determined in advance by a laser diffraction / scattering method for the lithium metal composite oxide particles were selected. 50 Particles with equal particle diameters. In addition, the particle diameter of each particle is the diameter of the circumscribed circle of the particle in the captured cross-sectional image. In the following other experimental examples, the particles for which the porosity is to be determined are selected in the same manner.

[0168] Then, the average porosity of the lithium metal composite oxide particles was calculated. As a result, it was confirmed that the average porosity of the lithium metal composite oxide particles used in this experimental example was 5% or less. Hereinafter, regarding the lithium metal composite oxide particles having a solid structure used in other experimental examples 1 to 27 and 32 to 34, it was also confirmed that the porosity was 5% or less.

[0169] In addition, when the average particle size of the lithium metal composite oxide particles and the aluminum oxide particles contained in the positive electrode active material obtained after the mixing step is measured by the above evaluation method, it can be confirmed that they are the same as before mixing. The following other experimental examples can confirm that in Experimental Examples 2 to Experimental Examples 34, the average particle size of the lithium metal composite oxide particles and the average particle size of the added particles do not change before and after mixing, and are the same.

[0170] Furthermore, when the specific surface area of ​​the positive electrode active material obtained after mixing was measured, it was confirmed to be 0.29 m 2 / g.

[0171] (2) Production of secondary batteries

[0172] Follow the steps below to make Figure 1 The above-mentioned evaluation was performed on a laminated battery having the structure shown.

[0173] like Figure 1As shown, the laminated battery 10 has the following structure, the electrolyte is impregnated into the stack of the positive electrode film 11, the separator 12, and the negative electrode film 13, and it is sealed with a laminate 14. In addition, the positive electrode film 11 is connected to the positive electrode tab 15, and the negative electrode film 13 is connected to the negative electrode tab 16, respectively, and the positive electrode tab 15 and the negative electrode tab 16 are exposed outside the laminate 14.

[0174] 20.0 g of the obtained positive electrode active material, 2.35 g of acetylene black, and 1.18 g of polyvinylidene fluoride were dispersed in N-methyl-2-pyrrolidone (NMP) to form a slurry, which was then applied to an Al foil at a rate of 1 cm per 1 cm. 2 There is 7.0 mg of positive electrode active material. Next, the product of the slurry containing the positive electrode active material coated on the Al foil is dried in the air at 120°C for 30 minutes to remove NMP. The Al foil coated with the positive electrode active material is cut into short strips of 66 mm in width and rolled with a load of 1.2 t to make a positive electrode film. Then, the positive electrode film is cut into a rectangle of 50 mm × 30 mm, dried in a vacuum dryer at 120°C for 12 hours, and used as the positive electrode film 11 of the laminated battery 10.

[0175] In addition, a negative electrode composite slurry which is a mixture of graphite powder and polyvinylidene fluoride having an average particle size of about 20 μm is applied on a copper foil to prepare a negative electrode film 13. A polyethylene porous film having a film thickness of 20 μm is used as the separator 12, and a 3:7 mixed solution of ethylene carbonate (EC) and diethyl carbonate (DEC) (manufactured by Ube Industries, Ltd.) with 1M LiPF6 as a supporting electrolyte is used as the electrolyte.

[0176] The laminate of the positive electrode film 11, the separator 12, and the negative electrode film 13 was immersed in an electrolyte in a dry room controlled at a dew point of -60°C and sealed with a laminate 14 to produce a laminated battery 10, which was then evaluated.

[0177] The evaluation results are shown in Table 1.

[0178] [Experimental Example 2 to Experimental Example 7]

[0179] A positive electrode active material and a secondary battery were prepared and evaluated in the same manner as in Experimental Example 1 except that the amount of aluminum oxide particles added was the amount shown in Table 1. The evaluation results are shown in Table 1.

[0180] The SEM image of the positive electrode active material obtained in Experimental Example 4 is as follows: Figure 2A shown.

[0181] [Experimental Example 8]

[0182] Without adding alumina particles, a layered structure with an average particle size of 13.0 μm and LiNi 0.52 Mn0.28 Co 0.20 The particles of lithium metal composite oxide represented by O2 were used as positive electrode active materials. In addition, the particles of lithium metal composite oxide used had a solid structure. Then, the positive electrode active materials were evaluated in the same manner as in Experimental Example 1.

[0183] In addition, a secondary battery was produced and evaluated in the same manner as in Experimental Example 1 except that the above-mentioned positive electrode active material was used. The evaluation results are shown in Table 1.

[0184] The SEM image of the positive electrode active material obtained in Experimental Example 8 is as follows: Figure 2B shown.

[0185] [Experimental Example 9]

[0186] Alumina particles with an average particle size of 46.2 μm were used as alumina particles pulverized by a jet mill to have an average particle size of 3.1 μm and a specific surface area of ​​0.92 m 2 / g of aluminum oxide particles. Then, the amount of the above aluminum oxide particles added was 0.26g relative to 100g of lithium metal composite oxide particles. In addition to the above points, the positive electrode active material and the secondary battery were prepared in the same manner as in Experimental Example 1 and evaluated. The evaluation results are shown in Table 1.

[0187] [Experimental Example 10]

[0188] The average particle size is 13.0 μm, and the LiNi 0.82 Mn 0.10 Co 0.05 Al 0.03 100 g of a lithium metal composite oxide particle having a layered structure represented by O2 and having an average particle size of 54 nm and a specific surface area of ​​104 m 2 0.26 g of aluminum oxide particles of 0.17 g / g were added and mixed thoroughly with a vibration mixer to obtain the positive electrode active material of this experimental example (mixing step). The particles of the lithium metal composite oxide used had a solid structure.

[0189] Furthermore, when the specific surface area of ​​the positive electrode active material obtained after mixing was measured, it was confirmed to be 0.51 m 2 / g.

[0190] A secondary battery was produced and evaluated in the same manner as in Experimental Example 1 except that the obtained positive electrode active material was used. The evaluation results are shown in Table 1.

[0191] [Experimental Example 11]

[0192] A positive electrode active material and a secondary battery were prepared and evaluated in the same manner as in Experimental Example 10, except that the amount of aluminum oxide particles added was the amount shown in Table 1. The evaluation results are shown in Table 1.

[0193] [Experimental Example 12]

[0194] Without adding alumina particles, LiNi 0.82 Mn 0.10 Co 0.05 Al 0.03 Particles of lithium metal composite oxide having a layered structure represented by O2 were used as positive electrode active materials. Then, such positive electrode active materials were evaluated in the same manner as in Experimental Example 10. The particles of lithium metal composite oxide used had a solid structure.

[0195] In addition, a secondary battery was produced and evaluated in the same manner as in Experimental Example 10 except that the above-mentioned positive electrode active material was used. The evaluation results are shown in Table 1.

[0196] [Experimental Example 13]

[0197] The average particle size is 14.7 μm, based on LiNi 0.85 Mn 0.1 Co 0.05 100 g of a lithium metal composite oxide particle having a layered structure represented by O2 and having an average particle size of 54 nm and a specific surface area of ​​104 m 2 0.13 g of aluminum oxide particles of 0.13 g / g were mixed thoroughly with a vibration mixer to obtain the positive electrode active material of this experimental example (mixing step). The particles of the lithium metal composite oxide used had a solid structure.

[0198] Furthermore, when the specific surface area of ​​the positive electrode active material obtained after mixing was measured, it was confirmed to be 1.03 m 2 / g.

[0199] A secondary battery was produced and evaluated in the same manner as in Experimental Example 1 except that the obtained positive electrode active material was used. The evaluation results are shown in Table 1.

[0200] The SEM image of the positive electrode active material obtained in Experimental Example 13 is as follows: Figure 3A shown.

[0201] [Experimental Examples 14 and 15]

[0202] A positive electrode active material and a secondary battery were prepared and evaluated in the same manner as in Experimental Example 13 except that the amount of aluminum oxide particles added was the amount shown in Table 1. The evaluation results are shown in Table 1.

[0203] [Experimental Example 16]

[0204] Without adding alumina particles, the average particle size of LiNi 0.85 Mn 0.1 Co 0.05 Particles of lithium metal composite oxide having a layered structure represented by O2 were used as the positive electrode active material. Then, such a positive electrode active material was evaluated in the same manner as in Experimental Example 13. The particles of the lithium metal composite oxide used had a solid structure.

[0205] In addition, a secondary battery was produced and evaluated in the same manner as in Experimental Example 13 except that the above-mentioned positive electrode active material was used. The evaluation results are shown in Table 1.

[0206] The SEM image of the positive electrode active material of Experimental Example 16 is as follows: Figure 3B shown.

[0207] [Experimental Example 17]

[0208] As an alternative to alumina particles, a particle size of 84 nm and a specific surface area of ​​55 m 2 The lithium metal composite oxide particles and the titanium oxide particles were mixed in the same manner as in Experimental Example 1 except that 0.41 g of the titanium oxide particles were added. Thus, the positive electrode active material of this Experimental Example was obtained (mixing step).

[0209] In addition, as the lithium metal composite oxide particles, LiNi 0.52 Mn 0.28 Co 0.20 Particles of lithium metal composite oxide having a layered structure represented by O2. The particles of lithium metal composite oxide used have a solid structure.

[0210] Furthermore, it was confirmed that the crystal phase of titanium oxide contained in the titanium oxide particles as the added particles was a single phase of the rutile phase.

[0211] When the average particle diameters of the lithium metal composite oxide particles and titanium oxide particles contained in the positive electrode active material obtained after the mixing step were measured by the above evaluation method, it was confirmed that they were the same as before mixing. As described in Experimental Example 1, the same was also confirmed in the following other experimental examples.

[0212] Furthermore, when the specific surface area of ​​the positive electrode active material obtained after mixing was measured, it was confirmed to be 0.45 m 2 / g.

[0213] A secondary battery was produced and evaluated in the same manner as in Experimental Example 1 except that the above-mentioned positive electrode active material was used. The evaluation results are shown in Table 1.

[0214] [Experimental Example 18]

[0215] A positive electrode active material and a secondary battery were prepared and evaluated in the same manner as in Experimental Example 17 except that the amount of titanium oxide particles added was the amount shown in Table 1. The evaluation results are shown in Table 1.

[0216] [Experimental Example 19]

[0217] As an alternative to alumina particles, a particle size of 84 nm and a specific surface area of ​​55 m 2 The lithium metal composite oxide particles and the titanium oxide particles were mixed in the same manner as in Experimental Example 13 except that 0.20 g of titanium oxide particles of 0.1 g / g were added to obtain the positive electrode active material of this Experimental Example (mixing step).

[0218] In addition, as the lithium metal composite oxide particles, LiNi 0.85 Mn 0.1 Co 0.05 Particles of lithium metal composite oxide having a layered structure represented by O2. The particles of lithium metal composite oxide used have a solid structure.

[0219] It was confirmed that the crystal phase of titanium oxide contained in the titanium oxide particles as the added particles was a single phase of rutile phase.

[0220] Furthermore, when the specific surface area of ​​the positive electrode active material obtained after the mixing step was measured, it was confirmed to be 1.11 m 2 / g.

[0221] A secondary battery was produced and evaluated in the same manner as in Experimental Example 13 except that the obtained positive electrode active material was used. The evaluation results are shown in Table 1.

[0222] [Experimental Example 20]

[0223] As an alternative to alumina particles, a particle size of 84 nm and a specific surface area of ​​55 m 2 The lithium metal composite oxide particles and the titanium oxide particles were mixed in the same manner as in Experimental Example 13 except that 0.20 g of titanium oxide particles of 0.1 g / g were added to obtain the positive electrode active material of this Experimental Example (mixing step).

[0224] In addition, as the lithium metal composite oxide particles, LiNi 0.85 Mn 0.1 Co 0.05 Particles of lithium metal composite oxide having a layered structure represented by O2. The particles of lithium metal composite oxide used have a solid structure.

[0225] It was confirmed that the titanium oxide crystal phase contained in the titanium oxide particles as the added particles was a common phase containing a rutile phase and anatase phase in a mass ratio of rutile phase:anatase phase=8:2. The rutile phase was the main phase.

[0226] Furthermore, when the specific surface area of ​​the positive electrode active material obtained after the mixing step was measured, it was confirmed to be 1.05 m 2 / g.

[0227] A secondary battery was produced and evaluated in the same manner as in Experimental Example 13 except that the obtained positive electrode active material was used. The evaluation results are shown in Table 1.

[0228] [Experimental Example 21]

[0229] As the added particles, in addition to the aluminum oxide particles, the titanium oxide particles used in Experimental Example 17 were used. 0.13 g of aluminum oxide particles and 0.17 g of titanium oxide particles were used respectively. Except for the above points, the lithium metal composite oxide particles, aluminum oxide particles, and titanium oxide particles were mixed in the same manner as in Experimental Example 1 to obtain the positive electrode active material of this Experimental Example (mixing step).

[0230] In addition, as the lithium metal composite oxide particles, LiNi 0.52 Mn 0.28 Co 0.20 Particles of lithium metal composite oxide having a layered structure represented by O2. The particles of lithium metal composite oxide used have a solid structure.

[0231] Furthermore, when the specific surface area of ​​the positive electrode active material obtained after the mixing step was measured, it was confirmed to be 0.40 m 2 / g.

[0232] A secondary battery was produced and evaluated in the same manner as in Experimental Example 1 except that the obtained positive electrode active material was used. The evaluation results are shown in Table 1.

[0233] [Experimental Example 22]

[0234] As an alternative to alumina particles, a 30 nm average particle size and a specific surface area of ​​65 m 2 The lithium metal composite oxide particles and the magnesium oxide particles were mixed in the same manner as in Experimental Example 1 except that 0.102 g of magnesium oxide particles were added at 100 g / g to obtain the positive electrode active material of this Experimental Example (mixing step).

[0235] In addition, as the lithium metal composite oxide particles, LiNi0.52 Mn 0.28 Co 0.20 Particles of lithium metal composite oxide having a layered structure represented by O2. The particles of lithium metal composite oxide used have a solid structure.

[0236] As described in Experimental Example 1, when the average particle diameters of the lithium metal composite oxide particles and magnesium oxide particles contained in the positive electrode active material obtained after the mixing step were measured by the above-mentioned evaluation method, it was confirmed that they were the same as those before mixing.

[0237] Furthermore, when the specific surface area of ​​the positive electrode active material obtained after mixing was measured, it was confirmed to be 0.62 m 2 / g.

[0238] A secondary battery was produced and evaluated in the same manner as in Experimental Example 1 except that the above-mentioned positive electrode active material was used. The evaluation results are shown in Table 2.

[0239] The SEM image of the positive electrode active material obtained in Experimental Example 22 is as follows: Figure 4 shown.

[0240] [Experimental Example 23]

[0241] A positive electrode active material and a secondary battery were prepared and evaluated in the same manner as in Experimental Example 22 except that the amount of magnesium oxide particles added was the amount shown in Table 2. The evaluation results are shown in Table 2.

[0242] [Experimental Example 24]

[0243] As an alternative to alumina particles, a quartz crystal with an average particle size of 167 nm and a specific surface area of ​​207 m 2 The lithium metal composite oxide particles and the silicon oxide particles were mixed in the same manner as in Experimental Example 1 except that 0.155 g of silicon oxide particles was added to the lithium metal composite oxide to obtain the positive electrode active material of this Experimental Example (mixing step).

[0244] In addition, as the lithium metal composite oxide particles, LiNi 0.52 Mn 0.28 Co 0.20 Particles of lithium metal composite oxide having a layered structure represented by O2. The particles of lithium metal composite oxide used have a solid structure.

[0245] As described in Experimental Example 1, when the average particle diameters of the lithium metal composite oxide particles and silicon oxide particles contained in the positive electrode active material obtained after the mixing step were measured by the above-mentioned evaluation method, it was confirmed that they were the same as those before mixing.

[0246] Furthermore, when the specific surface area of ​​the positive electrode active material obtained after mixing was measured, it was confirmed to be 0.38 m 2 / g.

[0247] A secondary battery was produced and evaluated in the same manner as in Experimental Example 1 except that the above-mentioned positive electrode active material was used. The evaluation results are shown in Table 2.

[0248] [Experimental Example 25]

[0249] A positive electrode active material and a secondary battery were prepared and evaluated in the same manner as in Experimental Example 24 except that the added amount of silicon oxide particles was changed to the amount shown in Table 2. The evaluation results are shown in Table 2.

[0250] The SEM image of the positive electrode active material obtained in Experimental Example 25 is as follows: Figure 5 shown.

[0251] [Experimental Example 26]

[0252] 100 g of a lithium metal composite oxide particle having a layered structure represented by LiNiO2 and an average particle size of 12.9 μm and a particle size of 10 nm and a specific surface area of ​​221 m 2 0.82 g of zirconium oxide particles with a density of 0.1447 W / g were placed in a nitrogen-purged container and mixed thoroughly with a vibration mixer to obtain the positive electrode active material of this experimental example (mixing step). The particles of the lithium metal composite oxide used had a solid structure.

[0253] It was confirmed that the crystal phase of zirconium oxide contained in the zirconium oxide particles as the added particles was a tetragonal single phase.

[0254] The specific surface area of ​​the positive electrode active material obtained after mixing was measured and found to be 1.68 m 2 / g.

[0255] A secondary battery was produced and evaluated in the same manner as in Experimental Example 1 except that the obtained positive electrode active material was used. The evaluation results are shown in Table 2.

[0256] The SEM image of the positive electrode active material obtained in Experimental Example 26 is as follows: Fig. 6A , Figure 6B shown. Figure 6B for Fig. 6A A partial enlarged view of .

[0257] [Experimental Example 27]

[0258] The positive electrode active material was evaluated in the same manner as in Experimental Example 26, without adding zirconium oxide particles, but with an average particle size of 12.9 μm, particles of a lithium metal composite oxide represented by LiNiO 2 having a layered structure.

[0259] In addition, a secondary battery was produced and evaluated in the same manner as in Experimental Example 26 except that the above-mentioned positive electrode active material was used. The evaluation results are shown in Table 2.

[0260] [Experimental Example 28]

[0261] The average particle size is 5.2 μm, based on LiNi 0.50 Mn 0.30 Co 0.20 100 g of a lithium metal composite oxide particle having a layered structure represented by O2 and having an average particle size of 54 nm and a specific surface area of ​​104 m 2 0.32 g of alumina particles of 0.1477 g / g were mixed thoroughly with a vibration mixer to obtain the positive electrode active material of this experimental example (mixing step).

[0262] Regarding the particles of lithium metal composite oxide used in this experimental example, the particle cross-sectional structure was observed and the average value of the porosity in the cross section was calculated. Specifically, after the particle group of lithium metal composite oxide was embedded in the resin, it was cut by a cross-section polisher (CP) to expose the cross section of the particle group, and the cross section of the exposed particle group was photographed with a scanning electron microscope. As a result, it can be confirmed that the particles of lithium metal composite oxide have a hollow structure, which has the following particle structure, having a hollow part composed of a space arranged in the center and an outer shell part arranged outside the hollow part.

[0263] Based on the obtained cross-sectional image of the particle group, the average porosity of the lithium metal composite oxide particles was calculated according to the method and conditions described in Experimental Example 1. As a result, it was confirmed that the average porosity of the hollow structure lithium metal composite oxide used in this Experimental Example was 15% or more.

[0264] The specific surface area of ​​the positive electrode active material obtained after mixing was measured and found to be 2.05 m 2 / g.

[0265] A secondary battery was produced and evaluated in the same manner as in Experimental Example 1 except that the obtained positive electrode active material was used. The evaluation results are shown in Table 2.

[0266] The SEM image of the cross section of the positive electrode active material obtained in Experimental Example 28 is as follows: Figure 7 shown.

[0267] [Experimental Example 29]

[0268] Without adding alumina particles, the LiNi 0.50 Mn 0.30 Co 0.20As the positive electrode active material, particles of lithium metal composite oxide having a layered structure represented by O2 were used. Then, evaluation was performed in the same manner as in Experimental Example 28 on such a positive electrode active material.

[0269] In addition, a secondary battery was produced and evaluated in the same manner as in Experimental Example 1 except that the above-mentioned positive electrode active material was used. The evaluation results are shown in Table 2.

[0270] [Experimental Example 30]

[0271] The average particle size is 5.2 μm, based on LiNi 0.50 Mn 0.30 Co 0.20 100 g of a lithium metal composite oxide particle having a layered structure represented by O2 and having an average particle size of 54 nm and a specific surface area of ​​104 m 2 0.32 g of alumina particles of 0.1477 g / g were mixed thoroughly with a vibration mixer to obtain the positive electrode active material of this experimental example (mixing step).

[0272] Regarding the particles of lithium metal composite oxide used in this experimental example, the particle cross-sectional structure was observed and the average value of the porosity in the cross section was calculated. Specifically, after the particle group of lithium metal composite oxide was embedded in the resin, it was cut by a cross-section polisher (CP) to expose the cross section of the particle group, and the cross section of the exposed particle group was photographed with a scanning electron microscope. As a result, it can be confirmed that the particles of lithium metal composite oxide have a porous structure in which the voids are dispersed throughout the particles.

[0273] Based on the obtained cross-sectional image of the particle group, the average porosity of the lithium metal composite oxide particles was calculated using the method and conditions described in Experimental Example 1. As a result, it was confirmed that the average porosity of the porous lithium metal composite oxide used in this Experimental Example was 15% or more.

[0274] The specific surface area of ​​the positive electrode active material obtained after mixing was measured and found to be 3.18 m 2 / g.

[0275] A secondary battery was produced and evaluated in the same manner as in Experimental Example 1 except that the obtained positive electrode active material was used. The evaluation results are shown in Table 2.

[0276] The SEM image of the cross section of the positive electrode active material obtained in Experimental Example 30 is as follows: Figure 8 shown.

[0277] [Experimental Example 31]

[0278] Without adding alumina particles, the porous LiNi0.50 Mn 0.30 Co 0.20 As the positive electrode active material, particles of lithium metal composite oxide having a layered structure represented by O2 were used. Then, evaluation was performed in the same manner as in Experimental Example 30 with respect to such a positive electrode active material.

[0279] In addition, a secondary battery was produced and evaluated in the same manner as in Experimental Example 1 except that the above-mentioned positive electrode active material was used. The evaluation results are shown in Table 2.

[0280] [Experimental Example 32]

[0281] The average particle size is 2.3 μm, based on LiNi 0.88 Mn 0.07 Co 0.05 100 g of lithium metal composite oxide particles having a layered structure represented by O2 and an average particle size of 54 nm and a specific surface area of ​​104 m 2 0.26 g of aluminum oxide particles of 0.17 g / g were added and mixed thoroughly with a vibration mixer to obtain the positive electrode active material of this experimental example (mixing step). The particles of the lithium metal composite oxide used had a solid structure.

[0282] The specific surface area of ​​the positive electrode active material obtained after mixing was measured and found to be 1.33 m 2 / g.

[0283] A secondary battery was produced and evaluated in the same manner as in Experimental Example 1 except that the obtained positive electrode active material was used. The evaluation results are shown in Table 2.

[0284] The SEM image of the positive electrode active material obtained in Experimental Example 32 is as follows: Fig. 9A , Fig. 9B shown. Fig. 9B for Fig. 9A A partial enlarged view of .

[0285] [Experimental Example 33]

[0286] A positive electrode active material and a secondary battery were prepared and evaluated in the same manner as in Experimental Example 32 except that the amount of aluminum oxide particles added was the amount shown in Table 2. The evaluation results are shown in Table 1.

[0287] [Experimental Example 34]

[0288] Without adding alumina particles, LiNi 0.88 Mn 0.07 Co 0.05As the positive electrode active material, particles of lithium metal composite oxide having a layered structure represented by O2 were used. Then, evaluation was performed in the same manner as in Experimental Example 32 with respect to such a positive electrode active material.

[0289] In addition, a secondary battery was produced and evaluated in the same manner as in Experimental Example 32 except that the above-mentioned positive electrode active material was used. The evaluation results are shown in Table 2.

[0290] The SEM image of the positive electrode active material obtained in Experimental Example 34 is as follows: Fig. 9C , Fig.9D shown. Fig.9D for Fig. 9C A partial enlarged view of .

[0291]

Table 1

[0292]

[0293]

Table 2

[0294]

[0295] According to the results shown in Tables 1 and 2, in Experimental Examples 1 to 7 in which aluminum oxide particles were added, it was confirmed that the cycle characteristics were improved compared to the case of Experimental Example 8 in which aluminum oxide particles were not added. The same tendency can be confirmed between other Experimental Examples in which aluminum oxide particles were added and Experimental Examples in which aluminum oxide particles were not added. Specifically, it can be confirmed between Experimental Examples 10 and 11 and Experimental Example 12, between Experimental Examples 13 to 15 and Experimental Example 16, between Experimental Example 28 and Experimental Example 29, between Experimental Example 30 and Experimental Example 31, and between Experimental Examples 32, 33 and Experimental Example 34. In addition, the same tendency was confirmed for the case where titanium oxide particles, magnesium oxide particles, silicon oxide particles, and zirconium oxide particles were used as added particles. Specifically, the same tendency can be confirmed between Experimental Examples 17 and 18 in which titanium oxide particles were added and Experimental Example 8 in which titanium oxide particles were not added, and between Experimental Examples 19 and 20 in which titanium oxide particles were added and Experimental Example 16 in which titanium oxide particles were not added. The same tendency was also observed between Experimental Examples 22 and 23 in which magnesium oxide particles were added and Experimental Example 8 in which magnesium oxide particles were not added, and between Experimental Examples 24 and 25 in which silicon oxide particles were added and Experimental Example 8 in which silicon oxide particles were not added. The same tendency was also observed between Experimental Example 26 in which zirconium oxide particles were added and Experimental Example 27 in which zirconium oxide particles were not added.

[0296] Furthermore, the same tendency was observed between Experimental Example 21 in which aluminum oxide particles and titanium oxide particles were added as additive particles and Experimental Example 8 in which no additive particles were added.

[0297] It can be confirmed that before cycling, the positive electrode resistance of the secondary batteries of Experimental Examples 1 to 5 is the same as that of the secondary battery of Experimental Example 8, but after cycling, the positive electrode resistance is suppressed from increasing and can be maintained at a significantly lower level than that of Experimental Example 8. The same tendency can be confirmed between Experimental Examples 10 and 11 and Experimental Example 12, between Experimental Examples 13 to 15 and Experimental Example 16, between Experimental Examples 17, 18, and 21 and Experimental Example 8, between Experimental Examples 19 and 20 and Experimental Example 16, Experimental Example 24, between Experimental Example 25 and Experimental Example 8, between Experimental Example 26 and Experimental Example 27, between Experimental Example 28 and Experimental Example 29, between Experimental Example 30 and Experimental Example 31, and between Experimental Examples 32 and 33 and Experimental Example 34.

[0298] It is believed that the reason is that in Experimental Examples 1 to 5, 10, 11, 13 to 15, 17 to 21, 24 to 26, 28, 30, 32, and 33, the added particles are dispersed on the surface of the lithium metal composite oxide particles, and the reaction between the lithium metal composite oxide particles and the electrolyte that causes the lithium metal composite oxide to deteriorate can be suppressed.

[0299] In Experimental Examples 19 and 20 in which titanium oxide particles were added, in Experimental Example 19, titanium oxide particles whose crystalline phase of titanium oxide contained was a single phase of rutile phase were used. On the other hand, in Experimental Example 20, titanium oxide particles whose crystalline phase of titanium oxide contained was a co-phase of rutile phase and anatase phase, and rutile phase was the main phase were used. Comparing the results of the two experimental examples, it can be confirmed that the cycle characteristics of the case of Experimental Example 19 were improved. Based on this result, it can be confirmed that when titanium oxide particles are used as an added element, the titanium oxide particles preferably contain a rutile phase, and particularly preferably a rutile phase as the main phase.

[0300] In addition, according to Figure 2A , Figure 2B Comparing the SEM images of Experimental Examples 4 and 8 disclosed above with those of Experimental Example 4 in which alumina particles were added and Experimental Example 8 in which alumina particles were not added, it can be confirmed that in Experimental Example 4, fine alumina particles were dispersed on the surface of the lithium metal composite oxide particles to modify the lithium metal composite oxide particles.

[0301] based on Figure 3A , Figure 3B The SEM images of the disclosed Experimental Examples 13 and 16 also confirm that in the positive electrode active material of Experimental Example 13 in which aluminum oxide particles are added, the added particles are dispersed and modified on the surface of the lithium metal composite oxide particles. Figure 4 SEM image of the published experimental example 22, Figure 5 SEM image of the published experimental example 25, Fig. 6A , Figure 6B SEM image of the published experimental example 26, Fig. 9A , Fig. 9B The same situation can also be confirmed from the SEM image of the published experimental example 32. Figure 4 , Figure 5 The SEM images of Experimental Example 22 and Experimental Example 25 can be compared with Figure 2B SEM image comparison of Experimental Example 8 is shown. Fig. 9A , Fig. 9B The SEM image of the disclosed experimental example 32 can be compared with Fig. 9C , Fig.9D Comparison of SEM images of the disclosed experimental example 34.

[0302] according to Figure 7 The disclosed SEM image of Experimental Example 28 confirms that the lithium metal composite oxide particles included in the positive electrode active material obtained in Experimental Example 28 have a hollow structure including a hollow portion and an outer shell portion disposed around the hollow portion.

[0303] according to Figure 8 From the disclosed SEM image of Experimental Example 30, it can be confirmed that the lithium metal composite oxide particles included in the positive electrode active material obtained in Experimental Example 30 have a porous structure in which voids are dispersed throughout the particles.

[0304] The positive electrode active material for lithium ion secondary batteries and the method for producing the positive electrode active material for lithium ion secondary batteries are described above by using embodiments and examples, but the present invention is not limited to the above embodiments and examples. Various modifications and changes are possible within the scope of the gist of the present invention described in the patent claims.

[0305] This application claims the priority based on Japanese Patent Application No. 2022-061916 filed with the Japan Patent Office on April 1, 2022, and all the contents of Japanese Patent Application No. 2022-061916 are hereby incorporated by reference into this international application.

Claims

1. A positive electrode active material for a lithium ion secondary battery, comprising lithium metal composite oxide particles and one or more additional particles selected from aluminum oxide particles, titanium oxide particles, magnesium oxide particles, silicon oxide particles and zirconium oxide particles, The specific surface area is 0.25m 2 / g above 4.0m 2 / g or less. 2 . The positive electrode active material for a lithium ion secondary battery according to claim 1 , wherein the average particle size of the added particles is 300 nm or less. 3 . The positive electrode active material for a lithium ion secondary battery according to claim 1 , wherein the ratio of the added particles to the lithium metal composite oxide particles is 0.025 mass % or more and 3.0 mass % or less.

4. A method for producing a positive electrode active material for a lithium ion secondary battery, comprising a mixing step of mixing lithium metal composite oxide particles and one or more additive particles selected from aluminum oxide particles, titanium oxide particles, magnesium oxide particles, silicon oxide particles and zirconium oxide particles, In the mixing step, the mixing is performed so that the specific surface area of ​​the positive electrode active material for lithium ion secondary battery obtained after the mixing step is 0.25 m 2 / g above 4.0m 2 / g or less.