Composite polyamide permselective membrane as well as preparation method and application thereof
By introducing boron nitride-magnesium aluminum metal hydroxide combination (BN-LDH) into the polyamide film, the problem of dense structure and violent exothermicity in the polyamide film is solved, and the CO2/light air selection and permeability is improved and stability, achieving higher gas molecules throughput and membrane stability.
Patent Information
- Application Number
- CN202411257696.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-09
- Publication Date
- 2024-11-22
AI Technical Summary
The dense structure of the existing polyamide films leads to a small permeability of gas molecules, and the violent exothermic reaction during polymerization makes the membrane separation performance unstable.
The composite polyamide selection permeable membrane is prepared by introducing boron nitride-magnesium aluminum metal hydroxide combination (BN-LDH), which improves the microstructure porosity of the membrane and alleviates the exothermic reaction during polymerization.
The CO2/light gas selection permeability and membrane stability are improved, making gas molecules easier to pass through, and the internal microstructure of the polyamide layer is more uniform.
Smart Images

Figure CN118988013A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of selective permeability membranes, in particular to a composite polyamide selective permeability membrane and a preparation method and application thereof. Background Art
[0002] Polyamide membranes can be used in the field of selective permeation, such as selective permeation of CO2 from a mixture of carbon dioxide (CO2) / light gas (such as hydrogen H2, nitrogen N2, methane CH4) (Chem. Mater., 2024, 36, 461), selective permeation of H2 from a mixture containing H2 (Chem. Eng. J., 2023, 478, 147263) and selective permeation of seawater to obtain desalinated water (J. Membr. Sci., 2019, 570-571, 112), etc. Pure polyamide membranes are usually prepared by interfacial polymerization, that is, amine compounds (such as phenylamines, linear amines, branched amines, etc.) are dissolved in deionized water and recorded as solution A, and acyl chloride compounds (such as trimesoyl chloride, phthaloyl chloride, isophthaloyl chloride, terephthaloyl chloride, etc.) are dissolved in organic solvents (such as alkanes) or ionic liquids and recorded as solution B. The porous substrate is first immersed in solution A for a certain period of time, taken out and dried, and then immersed in solution B for a certain period of time. Then, a polymerization reaction occurs under a specific temperature (40-90°C). After a certain period of time, a dense polyamide layer is generated on the porous substrate layer to obtain a pure polyamide membrane. The prepared pure polyamide membrane consists of two layers, namely the upper polyamide layer and the lower porous substrate layer. The upper polyamide layer actually plays a selective permeation role. However, the polyamide layer in the pure polyamide membrane prepared by this method has a dense structure, which is not conducive to the selective permeation of mixed gas molecules, so the permeability of mixed gas molecules is relatively small. At the same time, the polymerization process of amine compounds and acyl chloride compounds is a violent exothermic reaction, and the surface of the generated polyamide layer presents leaf-like protrusions, which makes the separation performance of the pure polyamide membrane unstable.
[0003] Therefore, it is necessary to prepare a polyamide membrane with a sparse structure that allows gas molecules to pass through easily and has good stability. Summary of the invention
[0004] In order to solve the deficiencies in the prior art, the present invention provides a composite polyamide selective permeable membrane and a preparation method and application thereof. The polyamide selective permeable membrane prepared by the present invention can greatly improve the CO2 / light gas selective permeability by introducing a boron nitride-magnesium aluminum metal hydroxide complex BN-LDH, and the polyamide selective permeable membrane exhibits good stability.
[0005] In order to achieve the above object, the specific scheme adopted by the present invention is: In one aspect, the present invention provides a method for preparing a composite polyamide selective permeable membrane, which mainly comprises the following steps: step (1), adding 0.1 to 2 g of an amine compound into 30 mL of deionized water, and subjecting the mixture to ultrasonic treatment to completely dissolve the amine compound to obtain a solution A; immersing a porous substrate in the solution A for 2 min, taking the porous substrate out and drying the porous substrate naturally to obtain a first intermediate membrane; Step (2), adding 3% to 12% BN-LDH by mass to 30 mL of deionized water, and ultrasonically dispersing it to obtain a C solution; immersing the first intermediate film in the C solution for 2 minutes, taking it out and naturally drying it to obtain a second intermediate film; Step (3), adding 0.1 to 2 g of an acyl chloride compound to 30 mL of n-hexane, sealing it to prevent its volatilization, and ultrasonically dissolving it to obtain a B solution; immersing the second intermediate film in the B solution for 1 minute, taking it out and naturally drying it to obtain a third intermediate film; Step (4), placing the third intermediate membrane in a constant temperature oven at 40-100° C. and drying for 3 minutes to promote the polymerization reaction, and finally obtaining a composite polyamide selective permeable membrane.
[0006] Furthermore, in step (1), the pore size of the porous substrate is 10 to 50 nm.
[0007] Furthermore, the porous substrate is made of any one of polyethersulfone, alumina or nylon.
[0008] Furthermore, in step (1), the amine compound is a phenylamine compound, a straight-chain amine compound or a branched-chain amine compound.
[0009] Furthermore, in step (3), the acyl chloride compound is any one of trimesoyl chloride, phthaloyl chloride, isophthaloyl chloride and terephthaloyl chloride.
[0010] On the other hand, the present invention provides a composite polyamide selective permeable membrane, which is prepared by the above method.
[0011] In another aspect, the present invention provides an application of a composite polyamide selective permeable membrane in CO2 / light gas selective permeability.
[0012] Beneficial effects:
[0013] (1) The composite polyamide selective permeable membrane prepared by the present invention improves the microstructure of the pure polyamide membrane by introducing BN-LDH, thereby increasing the porosity of the membrane structure to make it looser, which is conducive to the passage of gas molecules, thereby improving the CO2 permeability; at the same time, the BN-LDH structure contains a large number of hydroxyl groups, which interact with CO2 molecules and can improve the CO2 / light gas selectivity. In summary, the composite polyamide selective permeable membrane exhibits better CO2 / light gas selective permeability.
[0014] (2) In the present invention, the addition of BN-LDH alleviates the intense heat release during the polymerization of amine compounds and acyl chloride compounds, so that the internal microstructure of the generated composite polyamide layer is more uniform and consistent, and the prepared polyamide membrane has good stability. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] Figure 1 This is the FESEM image of the product prepared in Example 2.
[0016] Figure 2 This is the FESEM image of the product prepared in Comparative Example 3. DETAILED DESCRIPTION
[0017] The technical solution of the present invention will be clearly and completely described below in conjunction with specific embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0018] The BN-LDH used in the present invention is a boron nitride-magnesium aluminum hydroxide combination, which is a combination of boron nitride (BN) nanosheets and magnesium aluminum hydroxide (LDH) nanosheets. The BN-LDH combination contains a large number of hydroxyl groups, which makes it have good compatibility and is often used as a filler to act with a polymer matrix to prepare a composite material (Composites Part B, 2021, 207, 108568).
[0019] Example 1
[0020] A method for preparing a composite polyamide selectively permeable membrane mainly comprises the following steps: Step (1), adding 0.8 g of p-phenylenediamine to 30 mL of deionized water, and ultrasonically treating for 20 min to completely dissolve it, to obtain a solution A; the polyethersulfone porous substrate is immersed in the solution A for 2 min, taken out and placed in air to dry for 10 min, to obtain a first intermediate film; Step (2), adding 3% BN-LDH by mass to 30 mL of deionized water, and ultrasonically treating for 20 min to make it uniformly dispersed, to obtain C solutions of different concentrations; immersing the first intermediate film in the C solution for 2 min, taking it out and placing it in the air to dry for 10 min, to obtain a second intermediate film; Step (3), adding 0.2 g of trimesoyl chloride to 30 mL of n-hexane, sealing to prevent volatilization, and ultrasonically treating for 20 min to completely dissolve it, which is solution B; soaking the second intermediate film in solution B for 1 min, taking it out and placing it in air to dry for 5 min, to obtain a third intermediate film; Step (4), placing the third intermediate membrane in a 60° C. constant temperature oven to dry for 3 minutes to promote the polymerization reaction, and finally generating a composite polyamide selective permeable membrane.
[0021] Example 2
[0022] The difference between Example 2 and Example 1 is that in step (2), 9% by mass of BN-LDH is added to 30 mL of deionized water.
[0023] Example 3
[0024] The difference between Example 3 and Example 2 is that in step (1), 0.4 g of p-phenylenediamine is added to 30 mL of deionized water.
[0025] Example 4
[0026] The difference between Example 4 and Example 2 is that in step (3), 0.4 g of trimesoyl chloride is added to 30 mL of n-hexane.
[0027] Example 5
[0028] The difference between Example 5 and Example 4 is that in step (3), 0.4 g of isophthaloyl chloride is used instead of 0.4 g of trimesoyl chloride.
[0029] Example 6
[0030] The difference between Example 6 and Example 1 is that in step (2), 12% by mass of BN-LDH is added to 30 mL of deionized water.
[0031] Comparative Example 1
[0032] The difference between Comparative Example 1 and Example 1 is that in step (2), 2% by mass of BN-LDH is added to 30 mL of deionized water.
[0033] Comparative Example 2
[0034] The difference between Comparative Example 2 and Example 1 is that in step (2), 14% by mass of BN-LDH is added to 30 mL of deionized water.
[0035] Comparative Example 3
[0036] The difference between Comparative Example 3 and Example 1 is that step (2) is not included.
[0037] The microstructures of Example 2 and Comparative Example 3 were analyzed. Figure 1 Compared with the FSEM image of the product obtained in Example 2, Figure 2The FSEM image of the product obtained in Example 3 shows a large number of axon structures on the surface, which is caused by the large amount of heat released during the reaction of p-phenylenediamine and trimesoyl chloride to form a pure polyamide membrane. Because BN-LDH was added in Example 2, the process of forming the membrane was smoother, so the surface of the product obtained in Example 2 was relatively smoother.
[0038] The polyamide membranes prepared in Examples 1-6 and Comparative Examples 1-3 were used to conduct CO2 permeability and CO2 / N2 selectivity tests. The results are shown in Table 1 below.
[0039] Table 1 Test results of CO2 permeability and CO2 / N2 selectivity of polyamide membranes prepared in Examples 1-6 and Comparative Examples 1-3 <![CDATA[CO2 Permeability (Barrer)]]> <![CDATA[CO2 / N2 selectivity]]> Example 1 6.7 14 Example 2 18.9 32.6 Example 3 24.7 19.9 Example 4 16.5 30.3 Example 5 21.5 25.6 Example 6 20.1 29.5 Comparative Example 1 6.1 12.3 Comparative Example 2 23.9 26.1 Comparative Example 3 2.1 3.3
[0040] As can be seen from Table 1, the composite polyamide selective permeable membranes prepared in Examples 1-6 exhibit good CO2 selective permeability. Comparison between Example 2 and Example 1 shows that the amount of BN-LDH is increased, and both the CO2 permeability and CO2 / N2 selectivity are improved. Comparison between Example 3 and Example 2 shows that reducing the amount of p-phenylenediamine makes the microstructure of the prepared composite polyamide selective permeable membrane looser, which is conducive to the passage of gas molecules, that is, the CO2 permeability increases, but the CO2 / N2 selectivity decreases. Comparison between Example 4 and Example 2 shows that increasing the amount of trimesoyl chloride makes the microstructure of the prepared composite polyamide selective permeable membrane denser, which is conducive to screening mixed gases, that is, the CO2 / N2 selectivity increases, but the denser structure is not conducive to the passage of gas molecules, that is, the CO2 permeability decreases. Comparison between Example 5 and Example 4 shows that isophthaloyl chloride contains fewer acyl chloride groups than trimesoyl chloride, which makes the microstructure of the prepared composite polyamide selective permeable membrane loose, that is, the CO2 permeability increases, and the low content of acyl chloride groups causes defects in the structure of the prepared composite polyamide selective permeable membrane, which is not conducive to screening mixed gases, that is, the CO2 / N2 selectivity decreases. Comparison between Example 6 and Comparative Example 2 shows that the CO2 permeability continues to increase with a moderate increase in the amount of BN-LDH, but excessive BN-LDH may agglomerate inside the membrane material, so compared with Example 6, the CO2 / N2 selectivity of the product obtained in Comparative Example 2 decreases. Comparison between Comparative Example 1 and Example 1 shows that when the amount of BN-LDH is too small (less than 3%), both the CO2 permeability and CO2 / N2 selectivity decrease. Comparison between Comparative Example 3 and Example 1 shows that BN-LDH is not added, so a denser pure polyamide membrane is obtained, and both the CO2 permeability and CO2 / N2 selectivity decrease. Based on the above performances, it can be seen that the composite polyamide selective permeability membrane prepared by the present invention exhibits good CO2 / N2 selective permeability and has certain application value in the field of CO2 / light gas selective permeability.
[0041] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Any equivalent changes or modifications made according to the essence of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a composite polyamide selective permeable membrane, characterized in that: The main steps are as follows: Step (1), adding 0.1-2 g of an amine compound to 30 mL of deionized water, and subjecting the mixture to ultrasonic treatment to completely dissolve the amine compound to obtain a solution A; immersing the porous substrate in the solution A for 2 min, taking the porous substrate out and drying it naturally to obtain a first intermediate film; Step (2), adding 3% to 12% BN-LDH by mass to 30 mL of deionized water, and ultrasonically dispersing it to obtain a C solution; immersing the first intermediate film in the C solution for 2 min, taking it out and drying it naturally to obtain a second intermediate film; Step (3), adding 0.1-2 g of the acyl chloride compound to 30 mL of n-hexane, sealing to prevent volatilization, and ultrasonically dissolving it completely to obtain a B solution; immersing the second intermediate film in the B solution for 1 min, taking it out and drying it naturally to obtain a third intermediate film; Step (4), placing the third intermediate membrane in a constant temperature oven at 40-100° C. and drying for 3 min to promote the polymerization reaction, and finally obtaining a composite polyamide selective permeable membrane.
2. The method for preparing a composite polyamide selective permeable membrane according to claim 1, characterized in that: In step (1), the pore size of the porous substrate is 10-50 nm.
3. The method for preparing a composite polyamide selective permeable membrane according to claim 1, characterized in that: The porous substrate is made of any one of polyethersulfone, alumina or nylon.
4. The method for preparing a composite polyamide selective permeable membrane according to claim 1, characterized in that: In step (1), the amine compound is a phenylamine compound, a straight-chain amine compound or a branched-chain amine compound.
5. The method for preparing a composite polyamide selective permeable membrane according to claim 1, characterized in that: In step (3), the acyl chloride compound is any one of trimesoyl chloride, phthaloyl chloride, isophthaloyl chloride and terephthaloyl chloride.
6. A composite polyamide selective permeable membrane, characterized in that: The method is prepared by the method described in any one of claims 1 to 5.
7. Use of the composite polyamide selective permeable membrane according to claim 6 in CO2 / light gas selective permeability.