Al-doped ZnO-MgAl-LDH photocatalytic heterojunction as well as preparation method and application thereof
By doping Al elements in ZnO and combining with MgAl-LDH, Al-doped ZnO-MgAl-LDH nanoheterojunction photocatalyst is formed, which solves the problem of low photocatalytic efficiency of pure ZnO and achieves efficient photocatalytic activity and loading The efficiency of flow-coil separation improves the effect of water treatment.
Patent Information
- Application Number
- CN202410919629.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-10
- Publication Date
- 2024-11-22
AI Technical Summary
The photocatalytic efficiency of pure ZnO is insufficient, the carrier recombination rate is high and the photocatalytic activity is low, making it difficult to effectively absorb light energy in the visible light band, which limits its application in water quality purification.
By doping Al elements in ZnO, an Al-doped ZnO-MgAl-LDH nanoheterojunction photocatalyst is formed, which increases the Fermi level of ZnO and combines it with the MgAl-LDH carrier mechanism to change it to a type II heterojunction , improve the separation efficiency of photogenerated carriers.
The photocatalytic activity and carrier separation efficiency are significantly improved, the degradation ability of the photocatalyst is enhanced, especially the absorption capacity in the visible light band, and the demand for industrial water treatment is met.
Smart Images

Figure CN118988279A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of photocatalysts, and in particular is an Al-doped ZnO-MgAl-LDH nano heterojunction photocatalyst and a preparation method and application thereof. Background Art
[0003] In recent years, ZnO has become a promising material candidate for solving environmental problems, especially water purification, due to its abundant natural reserves, excellent stability, high carrier mobility, outstanding thermal conductivity, excellent electrical properties, significant reactivity and large specific surface area. In addition, ZnO can be easily fixed on different carriers, which provides feasibility for large-scale water treatment operations. In order to enhance the photocatalytic activity of zinc oxide, researchers have proposed two main modification strategies: one is to promote the generation of free radicals by improving the separation efficiency of photogenerated charge carriers; the other is to expand the response range of ZnO to light so that it also has good absorption capacity in the visible light band. Given the high recombination rate of carriers and insufficient photocatalytic efficiency in pure ZnO, improving the optical properties of ZnO and inhibiting the recombination of photogenerated electron-hole pairs are the key to improving its photocatalytic performance. To this end, researchers have explored a variety of methods, including morphology regulation, element doping, noble metal modification, and coupling with other semiconductor materials, aiming to optimize the photodegradation efficiency of ZnO, thereby promoting its application in the fields of environmental protection and sustainable development.
[0004] Layered double hydroxides (LDHs) are a class of synthetic layered materials with adjustable properties and high specific surface area. In particular, magnesium-aluminum-based LDHs (MgAl-LDH) have a unique layered structure and excellent adsorption capacity. This material is characterized by containing highly basic magnesium ions (Mg 2+ ), which are not only cost-effective and resource-rich, but their anion exchange properties allow precise control of the particle size and distribution of embedded assemblies. At the same time, the chemical composition of the material sheets can be adjusted through doping techniques, further enhancing their application potential as semiconductor photocatalysts. Summary of the invention
[0005] One object of the present invention is to propose an Al-doped ZnO-MgAl-LDH nano-heterojunction photocatalyst, which has the function of solving the problem of increasing the specific surface area of ZnO and transforming the carrier mechanism of MgAl-LDH. By doping Al elements in the ZnO component to increase the Fermi level of ZnO, the original type I ZnO-MgAl-LDH heterojunction is transformed into a type II heterojunction, so that efficient separation of photogenerated carriers in the heterojunction can be achieved under illumination. The raw materials of the present invention are easy to obtain, the process is simple, and the prepared photocatalytic heterojunction improves the separation efficiency of carriers and improves the photocatalytic activity, which can meet industrial needs; another object of the present invention is to propose a method for preparing an Al-doped ZnO-MgAl-LDH nano-heterojunction photocatalyst; the present invention also aims to propose an application of an Al-doped ZnO-MgAl-LDH nano-heterojunction photocatalyst.
[0006] To achieve the above object, the present invention provides a method for preparing an Al-doped ZnO-MgAl-LDH nanoheterojunction photocatalyst, comprising the following steps:
[0007] S1: Hydrothermal preparation of carbon nanosphere template using glucose at 170℃-190℃;
[0008] S2: Zn(NO 3 ) 2 6H 2 O was dissolved in deionized water to prepare the ZnO precursor. 3 ) 2 6H 2 O and Al(NO 3 ) 3 9H 2 O dissolved in deionized water to prepare the Al-doped ZnO precursor;
[0009] S3: injecting the carbon nanosphere template obtained in step S1 into the solution after S2 is dissolved, and after ultrasonic stirring, standing for 36 hours to allow the zinc source to be fully adsorbed on the surface of the carbon nanosphere, washing with deionized water and anhydrous ethanol three times alternately, drying, calcining at 500°C, keeping the temperature for 4 hours, and then naturally cooling to room temperature to obtain ZnO and Al-doped ZnO hollow nanospheres;
[0010] S4: Mg(NO 3 ) 2 6H 2 O, Al(NO 3 ) 3 9H 2 O was dissolved in deionized water by ultrasonic dissolution and then slowly poured into the Na 2 CO 3 and NaOH in a deionized water solution to obtain a MgAl-LDH precursor.
[0011] S5: The MgAl-LDH precursor in S4 was subjected to a hydrothermal reaction at 120° C. for 12 h, and after cooling to room temperature, it was centrifugally washed three times with deionized water to obtain MgAl-LDH.
[0012] S6: The ZnO and Al-doped ZnO prepared in S3 are purified and redissolved in deionized water, and then the MgAl-LDH precursor prepared in S4 is added and hydrothermaled at 120°C for 12 hours. After the reaction is completed, it is cooled to room temperature to obtain an Al-doped ZnO-MgAl-LDH heterojunction, wherein the diameter of the ZnO hollow nanospheres is 200nm-300nm, and the thickness of the LDH is 7nm-10nm.
[0013] In the step S2, the concentration of the Al solution is 0.5%-2% of the concentration of the zinc source.
[0014] In the step S3, the ultrasonic time and the stirring time are both 30 min-40 min, and the mixture is allowed to stand for 24 h-36 h. Finally, the temperature is raised to 500° C. at a heating rate of 2° C. / min and maintained for 4 h.
[0015] In the step S6, the mass volume ratio of Al-doped ZnO and MgAl-LDH is 1:0.05, 1:0.10, and 1:0.15.
[0016] The ZnO prepared in the method for preparing the Al-doped ZnO-MgAl-LDH photocatalytic heterojunction is in the morphology of hollow nanospheres, and the MgAl-LDH is in the morphology of layered nanosheets, thereby forming a binary heterojunction.
[0017] The Al-doped ZnO-MgAl-LDH nano-heterojunction photocatalyst is used for photocatalytic degradation of tetracycline, and the main active free radical of the degradation is -OH.
[0018] The Al-doped ZnO-MgAl-LDH nano-heterojunction photocatalyst and its preparation method and application described in the present invention have the following beneficial effects:
[0019] 1) The Al-doped ZnO-MgAl-LDH nano-heterojunction photocatalyst prepared by the present invention has excellent photocatalytic degradation activity;
[0020] 2) The Al-doped ZnO-MgAl-LDH photocatalytic heterojunction prepared by the present invention changes the carrier transfer mechanism of the ZnO-MgAl-LDH photocatalytic heterojunction, improves the carrier separation efficiency, and enhances the photocatalytic activity.
[0021] In summary, the Al-doped ZnO-MgAl-LDH photocatalytic heterojunction prepared by the present invention skillfully introduces donor energy levels in the band gap of ZnO by precisely controlling the aluminum (Al)-doped ZnO hollow nanospheres, thereby effectively improving the Fermi level of ZnO and increasing the concentration of carriers. On this basis, a heterojunction in which MgAl-LDH nanosheets are attached to ZnO hollow nanospheres is constructed with MgAl-LDH, and a photocatalytic material with excellent light absorption ability, high carrier generation efficiency, and excellent charge separation and transport performance is developed.
[0022] The technical principle of the present invention is that in the Al-doped ZnO-MgAl-LDH photocatalytic heterojunction photocatalysis with high-efficiency photocatalytic degradation performance, the Al-doped ZnO-MgAl-LDH photocatalytic heterojunction is easily fixed on the carbon nanosphere template, which can enhance the contact between the Al-doped ZnO and MgAl-LDH interfaces, and serve as a "bridge" for the directional transmission of photogenerated electrons, thereby promoting the transfer of photogenerated electrons from Al-doped ZnO to MgAl-LDH, thereby accelerating the separation of interface charges and improving the activity of photocatalytic degradation of organic pollutants.
[0023] The catalyst prepared by the method has high catalytic efficiency, high photocatalytic degradation activity and stability. In addition, the preparation method of the composite photocatalyst of the present invention has the advantages of being simple, easy to control preparation conditions, and no secondary pollution, and has certain research and application value. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 XRD comparison diagram of Al-doped ZnO-MgAl-LDH photocatalytic heterojunctions prepared in Examples 1 to 5 and pure ZnO and MgAl-LDH;
[0025] Figure 2 This is a SEM image of the Al-doped ZnO-MgAl-LDH photocatalytic heterojunction prepared in Example 1;
[0026] Figure 3 The photocatalytic degradation curves of tetracycline by the heterojunction photocatalysts prepared in Examples 1 to 5 and the pure sample are shown. DETAILED DESCRIPTION
[0027] Example 1
[0028] The method for preparing an Al-doped ZnO-MgAl-LDH photocatalytic heterojunction of the present invention comprises the following steps:
[0029] S1: Weigh 20.81 g of glucose and dissolve it in 70 mL of deionized water. Ultrasonicate for 15 min and then hydrothermally heat in a drying oven at 180 °C for 8 h to prepare a carbon nanosphere template.
[0030] S2: Zn(NO 3 ) 2 6H 2 O was dissolved in 40 mL of deionized water to prepare a ZnO precursor. 3 ) 2 6H 2 O and Al(NO 3 ) 3 9H 2 O was dissolved in 40 mL of deionized water to prepare the Al-doped ZnO precursor;
[0031] S3: injecting the carbon nanosphere template obtained in step S1 into the solution after S2 is dissolved, and after ultrasonic stirring, standing for 36 hours to allow the zinc source to be fully adsorbed on the surface of the carbon nanosphere, washing with deionized water and anhydrous ethanol three times alternately, drying, calcining at 500°C at a heating rate of 2°C / min, keeping the temperature for 4 hours, and then naturally cooling to room temperature to obtain ZnO and Al-doped ZnO hollow nanospheres;
[0032] S4: 29 mg Mg(NO 3 ) 2 6H 2 O, 14 mg Al(NO 3 ) 3 9H 2 O was dissolved in deionized water by ultrasonic dissolution and then slowly poured into a solution containing 4 mg Na 2 CO 3 and 2 mg NaOH in a deionized water solution to obtain a MgAl-LDH precursor;
[0033] S5: The MgAl-LDH precursor in S4 was subjected to a hydrothermal reaction at 120° C. for 12 h, and after cooling to room temperature, it was centrifugally washed three times with deionized water to obtain MgAl-LDH;
[0034] S6: The ZnO and Al-doped ZnO prepared in S3 are purified and redissolved in deionized water, and then the MgAl-LDH precursor prepared in S5 is added and hydrothermaled at 120°C for 12 hours. After the reaction is completed, it is cooled to room temperature to obtain an Al-doped ZnO-MgAl-LDH heterojunction.
[0035] Example 2
[0036] The method for preparing an Al-doped ZnO-MgAl-LDH photocatalytic heterojunction of the present invention comprises the following steps:
[0037] S1: Weigh 20.81 g of glucose and dissolve it in 70 mL of deionized water. Ultrasonicate for 15 min and then hydrothermally heat in a drying oven at 180 °C for 8 h to prepare a carbon nanosphere template.
[0038] S2: Zn(NO 3 ) 2 6H 2 O was dissolved in 30 mL of deionized water and 10 mL of anhydrous ethanol to prepare a ZnO precursor. 3 ) 2 6H 2 O and Al(NO 3 ) 3 9H 2 O was dissolved in 40 mL of deionized water to prepare the Al-doped ZnO precursor;
[0039] S3: injecting the carbon nanosphere template obtained in step S1 into the solution after S2 is dissolved, stirring with ultrasound, standing for 24 hours, washing three times with deionized water and anhydrous ethanol alternately, drying, calcining at 500°C at a heating rate of 5°C / min, keeping the temperature for 4 hours, and then naturally cooling to room temperature to obtain ZnO and Al-doped ZnO hollow nanospheres;
[0040] S4: 58 mg Mg(NO 3 ) 2 6H 2 O, 29mg Al(NO 3 ) 3 9H 2 O was dissolved in deionized water by ultrasonic dissolution and then slowly poured into a solution containing 8 mg Na 2 CO 3 and 4 mg NaOH in a deionized water solution to obtain a MgAl-LDH precursor;
[0041] S5: The MgAl-LDH precursor in S4 was subjected to a hydrothermal reaction at 120° C. for 12 h, and after cooling to room temperature, it was centrifugally washed three times with deionized water to obtain MgAl-LDH;
[0042] S6: The ZnO and Al-doped ZnO prepared in S3 are purified and redissolved in deionized water, and then added to the MgAl-LDH precursor prepared in S4 and hydrothermaled at 120°C for 12 hours. After the reaction is completed, it is cooled to room temperature to obtain an Al-doped ZnO-MgAl-LDH heterojunction.
[0043] Example 3
[0044] The method for preparing an Al-doped ZnO-MgAl-LDH photocatalytic heterojunction of the present invention comprises the following steps:
[0045] S1: Weigh 20.81 g of glucose and dissolve it in 70 mL of deionized water. Ultrasonicate for 15 min and then hydrothermally heat in a drying oven at 180 °C for 8 h to prepare a carbon nanosphere template.
[0046] S2: Zn(NO 3 ) 2 6H 2 O was dissolved in 20 mL of deionized water and 20 mL of anhydrous ethanol to prepare a ZnO precursor. 3 ) 2 6H 2 O and Al(NO 3 ) 3 9H 2 O was dissolved in 40 mL of deionized water to prepare the Al-doped ZnO precursor;
[0047] S3: injecting the carbon nanosphere template obtained in step S1 into the solution after S2 is dissolved, stirring with ultrasound, standing for 24 hours, washing three times with deionized water and anhydrous ethanol alternately, drying, calcining at 500°C at a heating rate of 5°C / min, keeping the temperature for 4 hours, and then naturally cooling to room temperature to obtain ZnO and Al-doped ZnO hollow nanospheres;
[0048] S4: 87 mg Mg(NO 3 ) 2 6H 2 O, 42mg Al(NO 3 ) 3 9H 2 O was dissolved in deionized water by ultrasonic dissolution and then slowly poured into a solution containing 12 mg Na 2 CO 3 and 6 mg NaOH in a deionized water solution to obtain a MgAl-LDH precursor;
[0049] S5: The MgAl-LDH precursor in S4 was subjected to a hydrothermal reaction at 120° C. for 12 h, and after cooling to room temperature, it was centrifugally washed three times with deionized water to obtain MgAl-LDH;
[0050] S6: The ZnO and Al-doped ZnO prepared in S3 are purified and redissolved in deionized water, and then added to the MgAl-LDH precursor prepared in S4 and hydrothermaled at 120°C for 12 hours. After the reaction is completed, it is cooled to room temperature to obtain an Al-doped ZnO-MgAl-LDH heterojunction.
[0051] Test example
[0052] In this specific embodiment: the structural characteristics of the sample were analyzed by X-ray diffraction (XRD, D8 Advane), the morphology and crystal structure of the sample were evaluated by thermal field emission scanning electron microscopy (FESEM, QUANTA FEG 450), and the optical properties of the sample were studied by UV-visible DRS (U-3900H).
[0053] Depend on Figure 1 It can be seen that 2θ shows the X-ray diffraction (XRD) patterns of ZnO, MgAl-LDH and their composite samples. It can be clearly observed from the figure that MgAl-LDH shows good diffraction peaks at diffraction angles 2θ of 11.5°, 23.2°, 39°, 46.5°, 60.1° and 61.5°, and the corresponding crystal planes are (003), (006), (012), (015), (018), (110) and (113), respectively, indicating that the sample has typical characteristic diffraction peaks of magnesium aluminum hydrotalcite ((PDF#22-0700)). In addition, the diffraction peaks of ZnO also coincide with the standard card of wurtzite ZnO (PDF#36-1451). The XRD pattern of the composite sample shows the characteristic peaks of ZnO and MgAl-LDH, confirming the successful preparation of the composite photocatalyst.
[0054] Depend on Figure 2 It can be seen that the ZnO hollow nanospheres and the MgAl-LDH layered nanosheets, and the ZnO hollow nanospheres covered on the MgAl-LDH layered nanosheets, further confirmed the successful composite of the heterojunction. It can also be proved that the composite photocatalyst contains Al-doped ZnO-MgAl-LDH, and the chemical structure and crystal form of the two are not changed during the composite process.
[0055] Figure 3 This is the photocatalytic degradation activity curve of tetracycline. After 30 minutes of dark treatment, the Al-doped ZnO-MgAl-LDH photocatalytic heterojunction showed the best photocatalytic degradation activity. Al-doped ZnO-MgAl-LDH has the highest catalytic activity;
[0056] It can be seen that Al-doped ZnO-MgAl-LDH can greatly improve the activity of the catalyst.
Claims
1. A method for preparing a third group metal-doped ZnO-MgAl-LDH nanoheterojunction photocatalyst, Features: The following steps are involved: S1: using glucose to hydrothermally prepare carbon nanosphere templates at a temperature range of 170°C-190°C for 7h-9h; S2: Zn(NO 3 ) 2 6H 2 O was dissolved in deionized water to prepare the ZnO precursor. 3 ) 2 6H 2 O and Al(NO 3 ) 3 9H 2 O dissolved in deionized water to prepare the Al-doped ZnO precursor; S3: injecting the carbon nanosphere template obtained in step S1 into the solution after S2 is dissolved, and after ultrasonic stirring, standing for 36 hours to allow the zinc source to be fully adsorbed on the surface of the carbon nanosphere, washing with deionized water and anhydrous ethanol three times alternately, drying, calcining at 500°C, keeping the temperature for 4 hours, and then naturally cooling to room temperature to obtain ZnO and Al-doped ZnO hollow nanospheres; S4: Mg(NO 3 ) 2 6H 2 O, Al(NO 3 ) 3 9H 2 O was dissolved in deionized water by ultrasonic dissolution and then slowly poured into the Na 2 CO 3 and NaOH in a deionized water solution to obtain a MgAl-LDH precursor; S5: The MgAl-LDH precursor in S4 was subjected to a hydrothermal reaction at 120° C. for 12 h, and after cooling to room temperature, it was centrifugally washed three times with deionized water to obtain MgAl-LDH; S6: The ZnO and Al-doped ZnO prepared in S3 are purified and redissolved in deionized water, and then the MgAl-LDH precursor prepared in S5 is added and hydrothermaled at 120°C for 12 hours. After the reaction is completed, it is cooled to room temperature to obtain an Al-doped ZnO-MgAl-LDH heterojunction, wherein the diameter of the ZnO hollow nanospheres is 200nm-300nm, and the thickness of the LDH is 7nm-10nm.
2. The method for preparing the Al-doped ZnO-MgAl-LDH photocatalytic heterojunction according to claim 1, Features: In the step S2, the concentration of the Al solution is 0.5%-2% of the concentration of the zinc source.
3. The method for preparing the Al-doped ZnO-MgAl-LDH photocatalytic heterojunction according to claim 1, Features: In the step S3, the ultrasonic time and stirring time are 30 min-40 min, the mixture is allowed to stand for 24 h-36 h, and finally the temperature is raised to 500° C. at a heating rate of 2° C. / min and maintained for 4 h.
4. The method for preparing the Al-doped ZnO-MgAl-LDH photocatalytic heterojunction according to claim 1, It is characterized in that In the step S6, the mass volume ratio of Al-doped ZnO and MgAl-LDH is 1:0.05, 1:0.10, and 1:0.
15.
5. The ZnO prepared in the method for preparing the Al-doped ZnO-MgAl-LDH photocatalytic heterojunction according to claim 1 is in the morphology of nano hollow spheres, and the MgAl-LDH is in the morphology of layered nano sheets, forming a binary heterojunction in which the MgAl-LDH nano sheets are attached to the ZnO nano hollow spheres.
6. The Al-doped ZnO-MgAl-LDH heterojunction photocatalyst prepared according to any one of claims 1 to 5.
7. The Al-doped ZnO-MgAl-LDH heterojunction photocatalyst according to claim 6, It is characterized by: The photocatalyst is a photocatalyst in which ZnO is a hollow nanosphere grown on the surface of MgAl-LDH is a layered nanosheet.
8. The Al-doped ZnO-MgAl-LDH heterojunction photocatalyst according to claim 6, Features: The photocatalyst has absorption in the full-band visible light range of 380nm-780nm.
9. Use of the Al-doped ZnO-MgAl-LDH heterojunction photocatalyst according to claim 6 in photocatalytic degradation of tetracycline.
10. The use according to claim 9, It is characterized in that The catalyst can be recycled repeatedly. In a single degradation process within 30 minutes, the mass ratio of the catalyst to tetracycline is 100:1, and the reaction temperature is 15°C-30°C.
Citation Information
Patent Citations
Zinc oxide nano-rod / magnalium laminar double-hydroxide preparation method and use thereof
CN101391201A
Flaky Mg-Al composite oxide for loading ZnO nano particles as well as preparation and application thereof
CN101708454A
Preparation method of Al-ZnO-AC (Active Carbon) electrode and nano electro-adsorption brackish water salinity removing device
CN103626357A
Photo-assisted regenerable non-carbon-based adsorbent following two-stage rate increasing mechanism as well as preparation method and application thereof
CN113058544A
An alkaline earth metal doped zinc oxide nanosheets and method of preparation thereof
IN201811044916A