Preparation methods of dechlorination catalysts and carbon-based supported noble metal palladium catalysts
By preparing a core-shell structured carbon-based material supported on a noble metal palladium catalyst, the problem of insufficient activity and stability of palladium-carbon catalysts in dechlorination reactions was solved, achieving efficient synthesis of 5-pyrimidinecarboxaldehyde and 2,3-dichloropyridine.
Patent Information
- Application Number
- CN202411081369.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-08
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2044-08-08
AI Technical Summary
Existing palladium-on-carbon catalysts suffer from difficulties in balancing activity and selectivity in dechlorination reactions, and their insufficient stability affects the synthesis efficiency of 5-pyrimidinecarboxaldehyde and 2,3-dichloropyridine.
A carbon-based noble metal palladium catalyst was prepared by adsorption and reduction using a mixed modified activated carbon and carbon-based materials as supports and a palladium nitrate solution containing dimethylaminoethanol as the palladium source solution. The process included sol-gel, acid treatment and organic amine modification to form a core-shell structure support, thereby improving the catalyst's reactivity and stability.
The prepared catalyst exhibits high reactivity and stability in the dechlorination reaction, and can effectively synthesize 5-pyrimidinecarboxaldehyde and 2,3-dichloropyridine. Furthermore, the support structure design avoids metal loss and catalyst poisoning, and enables multiple reuses.
Smart Images

Figure CN118988295B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of catalysis technology, specifically relating to the preparation method of dechlorination catalysts and carbon-based supported noble metal palladium catalysts. Background Technology
[0002] 5-Pyrimidinecarboxaldehyde is a commonly used basic raw material in organic synthesis and an intermediate in the synthesis of pharmaceutical molecules, with wide applications in organic synthesis. This substance is frequently used to synthesize other pyrimidine derivatives. Pyrimidines are important aromatic compounds, widely distributed in organisms, especially in the structure of nucleic acids (such as DNA and RNA). Pyrimidines and their derivatives play a crucial role in biology, being important components in constructing genetic information and regulating biological processes. 5-Pyrimidinecarboxaldehyde, as a derivative of pyrimidines, can be used to synthesize more complex pyrimidine compounds. 2,3-Dichloropyridine is an important chemical intermediate, widely used in pesticides and pharmaceuticals, and is a key substance in the synthesis of the novel insecticide chlorantraniliprole (20%). Currently, the synthesis of 5-pyrimidinecarboxaldehyde and 2,3-dichloropyridine typically employs a palladium-on-carbon catalyst to catalyze the dechlorination reaction of the organic compound 4,6-dichloro-5-pyrimidinecarboxaldehyde and 2,3,4,5-tetrachloropyridine (or 2,3,6-trichloropyridine).
[0003] Palladium-on-carbon catalysts are characterized by small feed amounts, high activity, stable performance, environmental friendliness, and easy recycling. They are widely used in pharmaceutical, petrochemical, dye and fragrance, electronics, and other fine chemical reaction processes. When one or more side reactions occur in the catalytic reaction, it is often necessary to balance the relationship between selectivity, activity, and catalyst stability. Therefore, selecting a suitable and efficient catalyst is particularly important.
[0004] Organic hydrogenation reactions involve complex raw materials and processes, and a wide variety of palladium-on-carbon catalysts are available. Furthermore, dechlorination reactions place high demands on catalyst performance, requiring stable reactivity as well as good selectivity and stability. Therefore, designing and preparing a catalyst that balances high activity, selectivity, and stability for dechlorination reactions is of paramount importance. Summary of the Invention
[0005] The technical problem to be solved by this invention is to address the shortcomings of the prior art by providing a method for preparing a dechlorination catalyst and a carbon-based material-supported palladium catalyst. The preparation method of this invention includes using a mixed-modified activated carbon and a carbon-based material as a support, and a palladium nitrate solution containing dimethylaminoethanol as a palladium source solution, to prepare a palladium catalyst via adsorption and reduction. This catalyst exhibits high reactivity and stability in the dechlorination reaction.
[0006] To solve the above-mentioned technical problems, the technical solution adopted by the present invention is as follows:
[0007] A method for preparing a carbon-based material supported noble metal palladium catalyst, characterized by comprising:
[0008] Step 1: Provide a carbon-based material carrier, specifically including:
[0009] Step 101: Mix the salt solution, organic ligand and alcohol in a mass ratio of (2-15):(10-50):(35-88) and stir at 60-100℃ for 8-15 hours to obtain a sol;
[0010] Step 102: Dry the sol at 90-150°C to obtain a gel. Crush the obtained gel and pass it through a 300-500 mesh sieve. Calcinate the sieved material at 600-900°C for 6-12 hours under N2 atmosphere to obtain carbon-based material precursor A.
[0011] Step 103: Mix activated carbon and carbon-based material precursor A in a mass ratio of (1-9):(9-1), cook in nitric acid solution at 90℃-100℃ for 1-2 hours, cool, filter, and wash to obtain acid-treated carrier;
[0012] Step 104: Place the acid-treated carrier in an ethanol solution of triethylamine, cook at 90℃~100℃ for 1h~2h, cool and filter to complete the modification, and obtain a carbon-based material carrier.
[0013] Step 2: According to the preset palladium mass percentage in the Pd / C catalyst, place the carbon-based material support described in Step 1 in a palladium nitrate solution containing dimethylaminoethanol, stir at room temperature for 1-3 hours to allow adsorption, filter, and obtain the catalyst precursor.
[0014] Step 3: Place the catalyst precursor in a reducing agent solution and stir to reduce it, thereby obtaining a carbon-based material supported on a noble metal palladium catalyst.
[0015] The above-mentioned method for preparing a carbon-based supported palladium catalyst is characterized in that the carbon-based supported palladium catalyst is a Pd / C catalyst with a Pd mass percentage of 1% to 5%.
[0016] The above-mentioned method for preparing a carbon-based material supported palladium catalyst is characterized in that, in step 101, the salt solution is a metal-soluble salt solution, the organic ligand is one or more of dicyandiamide, thiourea, pyridazine, melamine, cyanuric acid and urea, and the alcohol is methanol or anhydrous ethanol.
[0017] The method for preparing the carbon-based material supported palladium catalyst described above is characterized in that the soluble metal salt is one or more of ferric nitrate, copper nitrate, and nickel nitrate.
[0018] The method for preparing the above-mentioned carbon-based material supported palladium catalyst is characterized in that, in step 103, the mass percentage concentration of the nitric acid solution is 5% to 10%, and the mass of the nitric acid solution is 8 to 10 times the total mass of the activated carbon and the carbon-based material precursor A.
[0019] The above-mentioned method for preparing a carbon-based material supported palladium catalyst is characterized in that, in step 104, the mass percentage concentration of the triethylamine ethanol solution is 3%, and the mass of the triethylamine ethanol solution is 8 to 10 times the mass of the acid-treated support.
[0020] The method for preparing the carbon-based material supported palladium catalyst described above is characterized in that, in step two, the palladium nitrate solution containing dimethylaminoethanol has a palladium nitrate concentration of 0.1 g / ml to 0.5 g / ml and a dimethylaminoethanol mass percentage concentration of 0.1% to 0.3%.
[0021] The above-mentioned method for preparing a carbon-based material-supported palladium catalyst is characterized in that, in step three, the reducing agent solution is a sodium formate solution or a sodium borohydride solution with a mass percentage concentration of 10% to 20%, the stirring and reduction temperature is 80℃ to 90℃, the stirring and reduction time is 1h to 2h, and the mass of the reducing agent solution is 8 to 10 times the mass of the catalyst precursor.
[0022] The above-mentioned method for preparing a carbon-based material-supported palladium catalyst is characterized in that, in step two, the pH of the system is controlled to be 8.5 during the adsorption process.
[0023] In addition, the present invention provides a dechlorination catalyst, characterized in that the dechlorination catalyst is prepared by the above-described method for preparing a carbon-based material-supported noble metal palladium catalyst.
[0024] The reaction equation for the catalytic synthesis of 5-pyrimidinecarboxaldehyde is as follows:
[0025]
[0026] The reaction equation for the catalytic synthesis of 2,3-dichloropyridine is as follows:
[0027]
[0028] The reaction equation for the catalytic synthesis of biotin is as follows:
[0029]
[0030] Compared with the prior art, the present invention has the following advantages:
[0031] 1. This invention provides a method for preparing a palladium catalyst supported on a carbon-based material. The method includes using a mixed modified activated carbon and a carbon-based material as a support, and using a palladium nitrate solution containing dimethylaminoethanol as a palladium source solution to prepare a palladium catalyst by adsorption and reduction. The catalyst has high reactivity and stability in dechlorination reactions.
[0032] 2. The preparation method of the carbon-based material supported palladium catalyst of the present invention includes preparing a support obtained by mixing and modifying activated carbon and carbon-based material. The support uses a metal salt solution as a matrix. The performance of the carbon-based material and the support can be directionally adjusted by controlling the type and amount of metal. By mixing activated carbon and carbon-based material, the uncontrollable amount of metal and metal loss caused in the process of metal modification of activated carbon can be effectively avoided, and the advantages of activated carbon and carbon-based material can be fully combined.
[0033] 3. The preparation method of the carbon-based material supported noble metal palladium catalyst of the present invention includes using metal soluble salt, organic ligand and alcohol as the main raw materials, and preparing carbon-based material support through sol-gel, acid treatment and organic amine modification. The metal ions in the metal soluble salt are used as the core and the organic ligand is coated to form a carbon-based material support with a core-shell structure, which endows the support with higher physical properties, more uniform component distribution and richer pore structure, so as to realize the synergistic reaction of active components and improve the reaction activity and stability of the catalyst.
[0034] 4. The preparation method of the carbon-based material supported palladium catalyst of the present invention includes boiling activated carbon and the carbon-based material precursor with nitric acid. This can fully remove excess metal ions from the material and give the support a well-developed porous structure and abundant oxygen-containing functional groups on the support surface, so that the support surface exposes more metal sites. This can achieve both binding with the active component Pd and promoting the adsorption of easily poisoned catalyst components in the dechlorination reaction, thus avoiding catalyst poisoning.
[0035] 5. The method for preparing the carbon-based material supported palladium catalyst of the present invention includes modifying the acid-treated support with an alcoholic solution of triethylamine, which can effectively enrich the functional groups on the support surface and regulate the acid-base sites on the support surface, increase the number of nitrogen species on the surface, and improve the catalyst's resistance to poisoning and strong acids and bases.
[0036] 6. The preparation method of the carbon-based material supported noble metal palladium catalyst of the present invention includes using a palladium nitrate solution containing dimethylaminoethanol as a palladium source, which can make full use of the function of dimethylaminoethanol as a small molecule surfactant to regulate the dispersion rate and dispersion state of Pd on the support surface and promote its stable and uniform distribution on the support surface.
[0037] 7. The supported palladium catalyst prepared by the method of the present invention has a support particle size of about 400 mesh, which has the advantage of easy solid-liquid separation after reaction, and can be reused multiple times without the need for treatment of the catalyst after use.
[0038] 8. The dechlorination catalyst of the present invention comprises a mixed modified activated carbon and a carbon-based material as a support, and a palladium nitrate solution containing dimethylaminoethanol as a palladium source solution, which is prepared by adsorption and reduction. The catalyst has high reactivity and stability in the dechlorination reaction.
[0039] The technical solution of the present invention will be further described in detail below with reference to the accompanying drawings and embodiments. Attached Figure Description
[0040] Figure 1 This is a transmission electron microscope image of the carbon-based material carrier in Example 2. Detailed Implementation
[0041] Example 1
[0042] This embodiment provides a method for preparing a carbon-based material-supported palladium catalyst, wherein the carbon-based material-supported palladium catalyst is a Pd / C catalyst with a Pd mass percentage of 5%, and the preparation method includes:
[0043] Step 1: Provide a carbon-based material carrier, specifically including:
[0044] Step 101: Mix the salt solution, organic ligand, and alcohol in a mass ratio of 10:30:60, and stir the mixture at 80°C for 10 hours to obtain a sol; the salt solution is a copper nitrate solution with a mass percentage concentration of 0.5 g / ml, the organic ligand is dicyandiamide, and the alcohol is anhydrous ethanol.
[0045] Step 102: Dry the sol at 90°C to obtain a gel. Crush the obtained gel and pass it through a 300-mesh sieve. Calcinate the sieved material at 600°C for 12 hours under N2 atmosphere to obtain carbon-based material precursor A.
[0046] Step 103: Mix activated carbon and carbon-based material precursor A at a mass ratio of 7:3, cook in nitric acid solution at 90°C for 1 hour, cool and filter, wash with pure water until pH is 5, and obtain acid-treated carrier; the mass percentage concentration of the nitric acid solution is 5%, and the mass of the nitric acid solution is 10 times the total mass of activated carbon and carbon-based material precursor A;
[0047] Step 104: Place the acid-treated carrier in an ethanol solution of 3% triethylamine by mass, boil at 100°C for 2 hours, cool and filter to complete the modification, and obtain a carbon-based material carrier; the mass of the triethylamine ethanol solution is 10 times the mass of the carrier after acid treatment; the triethylamine ethanol solution is a triethylamine ethanol solution obtained by dissolving triethylamine in anhydrous ethanol.
[0048] Step 2: According to the preset palladium mass percentage in the Pd / C catalyst, 100g of the carbon-based material support described in Step 1 is placed in a palladium nitrate solution containing dimethylaminoethanol. The mixture is stirred at room temperature for 2 hours to allow adsorption. During stirring, the pH is controlled to 8.5 using NaOH solution. After adsorption is complete, the mixture is filtered to obtain the catalyst precursor. The palladium nitrate solution containing dimethylaminoethanol is obtained by dissolving dimethylaminoethanol in an aqueous palladium nitrate solution. The palladium nitrate concentration is 0.5g / ml, the dimethylaminoethanol mass percentage concentration is 0.3%, and the NaOH solution mass percentage concentration is 5%.
[0049] Step 3: The catalyst precursor is placed in a reducing agent solution and stirred for reduction to obtain a carbon-based material supported palladium catalyst; the reducing agent solution is a sodium borohydride solution with a mass percentage concentration of 20%, the stirring and reduction temperature is 80℃, and the stirring and reduction time is 2h; the mass of the reducing agent solution is 8 times the mass of the catalyst precursor.
[0050] Example 2
[0051] This embodiment provides a method for preparing a carbon-based material-supported palladium catalyst, wherein the carbon-based material-supported palladium catalyst is a Pd / C catalyst with a Pd mass percentage of 3%, and the preparation method includes:
[0052] Step 1: Provide a carbon-based material carrier, specifically including:
[0053] Step 101: Mix the salt solution, organic ligand, and alcohol in a mass ratio of 15:50:35 and stir at 100°C for 8 hours to obtain a sol; the salt solution is a ferric nitrate solution with a mass percentage concentration of 0.5 g / ml, the organic ligand is thiourea, and the alcohol is methanol;
[0054] Step 102: Dry the sol at 150°C to obtain a gel. Crush the obtained gel and pass it through a 350-mesh sieve. Calcinate the sieved material at 800°C for 8 hours under N2 atmosphere to obtain carbon-based material precursor A.
[0055] Step 103: Mix activated carbon and carbon-based material precursor A at a mass ratio of 7:3, cook in nitric acid solution at 90°C for 2 hours, cool and filter, wash with pure water until pH is 5, and obtain acid-treated carrier; the mass percentage concentration of the nitric acid solution is 5%, and the mass of the nitric acid solution is 10 times the total mass of activated carbon and carbon-based material precursor A;
[0056] Step 104: Place the acid-treated carrier in an ethanol solution with a mass percentage concentration of 3% triethylamine, cook at 90°C for 2 hours, cool and filter to complete the modification, and obtain a carbon-based material carrier; the mass of the triethylamine ethanol solution is 8 times the mass of the carrier after acid treatment;
[0057] Step 2: According to the preset palladium mass percentage in the Pd / C catalyst, 100g of the carbon-based material support described in Step 1 is placed in a palladium nitrate solution containing dimethylaminoethanol. The mixture is stirred at room temperature for 2 hours to allow adsorption. During stirring, the pH is controlled to 8.5 using NaOH solution. After adsorption is complete, the mixture is filtered to obtain the catalyst precursor. In the above palladium nitrate solution containing dimethylaminoethanol, the palladium nitrate concentration is 0.2g / ml, the dimethylaminoethanol mass percentage concentration is 0.2%, and the NaOH solution mass percentage concentration is 5%.
[0058] Step 3: The catalyst precursor is placed in a reducing agent solution and stirred for reduction to obtain a carbon-based material supported palladium catalyst; the reducing agent solution is a sodium formate solution with a mass percentage concentration of 20%, the stirring and reduction temperature is 90℃, and the stirring and reduction time is 1 hour; the mass of the reducing agent solution is 8 times the mass of the catalyst precursor.
[0059] The transmission electron microscope image of the carbon-based material obtained in step one of this embodiment is as follows: Figure 1 As shown in Table 1, the evaluation results of the structural properties of this material are presented.
[0060] Table 1 Evaluation results of structural properties of carbon-based materials
[0061]
[0062] The evaluation methods included: Experiment 1 involved immersing 100g of the carbon-based material from Example 2 in a hydrochloric acid solution, stirring at high speed for 12 hours, filtering, and then detecting the metal ions in the filtrate using ICP. Experiment 2 involved calcining 100g of the carbon-based material from Example 2 at 800°C for 6 hours in an oxygen atmosphere, dissolving the resulting ash in the aforementioned hydrochloric acid solution, filtering, and then detecting the metal ions in the filtrate using ICP.
[0063] As shown in Table 1, the metal content dissolved through complete carbonization and decomposition of carbon-based materials by calcination is far higher than that dissolved by strong acid and mechanical stirring. Because carbon-based materials possess an organic ligand shell structure, the internal metals do not leach into the filtrate. Figure 1 As can be seen from Table 1, the carbon-based material of the present invention has a core-shell structure with higher physical properties.
[0064] Example 3
[0065] This embodiment provides a method for preparing a carbon-based material-supported palladium catalyst, wherein the carbon-based material-supported palladium catalyst is a Pd / C catalyst with a Pd mass percentage of 2%, and the preparation method includes:
[0066] Step 1: Provide a carbon-based material carrier, specifically including:
[0067] Step 101: Mix the salt solution, organic ligand, and alcohol in a mass ratio of 5:40:55 and stir at 90°C for 15 hours to obtain a sol; the salt solution is a ferric nitrate solution with a mass percentage concentration of 0.5 g / ml, the organic ligand is pyridazine, and the alcohol is methanol;
[0068] Step 102: Dry the sol at 130°C to obtain a gel. Crush the obtained gel and pass it through a 400-mesh sieve. Calcinate the sieved material at 900°C for 6 hours under N2 atmosphere to obtain carbon-based material precursor A.
[0069] Step 103: Mix activated carbon and carbon-based material precursor A at a mass ratio of 5:5, cook in nitric acid solution at 90°C for 2 hours, cool and filter, wash with pure water until pH is 5, and obtain acid-treated carrier; the mass percentage concentration of the nitric acid solution is 8%, and the mass of the nitric acid solution is 8 times the total mass of activated carbon and carbon-based material precursor A;
[0070] Step 104: Place the acid-treated carrier in an ethanol solution of 3% triethylamine by mass, boil at 100°C for 2 hours, cool and filter to complete the modification, and obtain a carbon-based material carrier; the mass of the triethylamine ethanol solution is 9 times the mass of the carrier after acid treatment.
[0071] Step 2: According to the preset palladium mass percentage in the Pd / C catalyst, 100g of the carbon-based material support described in Step 1 is placed in a palladium nitrate solution containing dimethylaminoethanol and stirred at room temperature for 2 hours to allow adsorption. During stirring, the pH is controlled at 8.5 using NaOH solution. After adsorption is complete, the mixture is filtered to obtain the catalyst precursor. In the above palladium nitrate solution containing dimethylaminoethanol, the palladium nitrate concentration is 0.2g / ml, the dimethylaminoethanol mass percentage concentration is 0.1%, and the NaOH solution mass percentage concentration is 5%.
[0072] Step 3: The catalyst precursor is placed in a reducing agent solution and stirred for reduction to obtain a carbon-based material supported palladium catalyst; the reducing agent solution is a sodium formate solution with a mass percentage concentration of 10%, the stirring and reduction temperature is 80℃, and the stirring and reduction time is 1h; the mass of the reducing agent solution is 8 times the mass of the catalyst precursor.
[0073] Example 4
[0074] This embodiment provides a method for preparing a carbon-based material-supported palladium catalyst, wherein the carbon-based material-supported palladium catalyst is a Pd / C catalyst with a Pd mass percentage of 1%, and the preparation method includes:
[0075] Step 1: Provide a carbon-based material carrier, specifically including:
[0076] Step 101: Mix the salt solution, organic ligand, and alcohol in a mass ratio of 2:50:48 and stir at 60°C for 15 hours to obtain a sol; the salt solution is a ferric nitrate solution with a mass percentage concentration of 0.5 g / ml, the organic ligand is pyridazine, and the alcohol is anhydrous ethanol;
[0077] Step 102: Dry the sol at 90°C to obtain a gel. Crush the gel and pass it through a 500-mesh sieve. Calcinate the sieved material at 700°C for 12 hours under N2 atmosphere to obtain carbon-based material precursor A.
[0078] Step 103: Mix activated carbon and carbon-based material precursor A at a mass ratio of 5:5, cook in nitric acid solution at 90°C for 2 hours, cool and filter, wash with pure water until pH is 5, and obtain acid-treated carrier; the mass percentage concentration of the nitric acid solution is 8%, and the mass of the nitric acid solution is 8 times the total mass of activated carbon and carbon-based material precursor A;
[0079] Step 104: Place the acid-treated carrier in an ethanol solution with a mass percentage concentration of 3% triethylamine, boil at 100°C for 2 hours, cool and filter to complete the modification, and obtain a carbon-based material carrier; the mass of the triethylamine ethanol solution is 10 times the mass of the carrier after acid treatment.
[0080] Step 2: According to the preset palladium mass percentage in the Pd / C catalyst, 100g of the carbon-based material support described in Step 1 is placed in a palladium nitrate solution containing dimethylaminoethanol and stirred at room temperature for 2 hours to allow adsorption. During stirring, the pH is controlled at 8.5 using NaOH solution. After adsorption is complete, the mixture is filtered to obtain the catalyst precursor. In the above palladium nitrate solution containing dimethylaminoethanol, the palladium nitrate concentration is 0.2g / ml, the dimethylaminoethanol mass percentage concentration is 0.1%, and the NaOH solution mass percentage concentration is 5%.
[0081] Step 3: The catalyst precursor is placed in a reducing agent solution and stirred for reduction to obtain a carbon-based material supported palladium catalyst; the reducing agent solution is a sodium formate solution with a mass percentage concentration of 10%, the stirring and reduction temperature is 80℃, and the stirring and reduction time is 1h; the mass of the reducing agent solution is 8 times the mass of the catalyst precursor.
[0082] Example 5
[0083] This embodiment provides a method for preparing a carbon-based material-supported palladium catalyst, wherein the carbon-based material-supported palladium catalyst is a Pd / C catalyst with a Pd mass percentage of 1%, and the preparation method includes:
[0084] Step 1: Provide a carbon-based material carrier, specifically including:
[0085] Step 101: Mix the salt solution, organic ligand, and alcohol in a mass ratio of 2:10:88 and stir at 60°C for 15 hours to obtain a sol; the salt solution is a nickel nitrate solution with a mass percentage concentration of 0.5 g / ml, the organic ligand is melamine, and the alcohol is methanol;
[0086] Step 102: Dry the sol at 90°C to obtain a gel. Crush the gel and pass it through a 500-mesh sieve. Calcinate the sieved material at 700°C for 12 hours under N2 atmosphere to obtain carbon-based material precursor A.
[0087] Step 103: Mix activated carbon and carbon-based material precursor A at a mass ratio of 1:9, cook in nitric acid solution at 100°C for 2 hours, cool and filter, wash with pure water until pH is 5, and obtain acid-treated carrier; the mass percentage concentration of the nitric acid solution is 10%, and the mass of the nitric acid solution is 8 times the total mass of activated carbon and carbon-based material precursor A;
[0088] Step 104: Place the acid-treated carrier in an ethanol solution of 3% triethylamine by mass, boil at 100°C for 1 hour, cool and filter to complete the modification, and obtain a carbon-based material carrier; the mass of the triethylamine ethanol solution is 8 times the mass of the carrier after acid treatment.
[0089] Step 2: According to the preset palladium mass percentage in the Pd / C catalyst, 100g of the carbon-based material support described in Step 1 is placed in a palladium nitrate solution containing dimethylaminoethanol and stirred at room temperature for 1.5h to allow adsorption. During stirring, the pH is controlled at 8.5 using NaOH solution. After adsorption is complete, the mixture is filtered to obtain the catalyst precursor. In the above palladium nitrate solution containing dimethylaminoethanol, the palladium nitrate concentration is 0.1g / ml, the dimethylaminoethanol mass percentage concentration is 0.1%, and the NaOH solution mass percentage concentration is 5%.
[0090] Step 3: The catalyst precursor is placed in a reducing agent solution and stirred for reduction to obtain a carbon-based material supported palladium catalyst; the reducing agent solution is a sodium formate solution with a mass percentage concentration of 10%, the stirring and reduction temperature is 80℃, and the stirring and reduction time is 1h; the mass of the reducing agent solution is 8 times the mass of the catalyst precursor.
[0091] Example 6
[0092] This embodiment provides a method for preparing a carbon-based material-supported palladium catalyst, wherein the carbon-based material-supported palladium catalyst is a Pd / C catalyst with a Pd mass percentage of 5%, and the preparation method includes:
[0093] Step 1: Provide a carbon-based material carrier, specifically including:
[0094] Step 101: Mix the salt solution, organic ligand, and alcohol in a mass ratio of 2:10:88 and stir at 60°C for 15 hours to obtain a sol; the salt solution is a nickel nitrate solution with a mass percentage concentration of 0.5 g / ml, the organic ligand is cyanuric acid, and the alcohol is methanol;
[0095] Step 102: Dry the sol at 90°C to obtain a gel. Crush the gel and pass it through a 400-mesh sieve. Calcinate the sieved material at 700°C for 10 hours under N2 atmosphere to obtain carbon-based material precursor A.
[0096] Step 103: Mix activated carbon and carbon-based material precursor A at a mass ratio of 9:1, cook in nitric acid solution at 95°C for 2 hours, cool and filter, wash with pure water until pH is 5, and obtain acid-treated carrier; the mass percentage concentration of the nitric acid solution is 8%, and the mass of the nitric acid solution is 8 times the total mass of activated carbon and carbon-based material precursor A;
[0097] Step 104: Place the acid-treated carrier in an ethanol solution with a mass percentage concentration of 3% triethylamine, cook at 100°C for 1.5 hours, cool and filter to complete the modification, and obtain a carbon-based material carrier; the mass of the triethylamine ethanol solution is 10 times the mass of the carrier after acid treatment;
[0098] Step 2: According to the preset palladium mass percentage in the Pd / C catalyst, 100g of the carbon-based material support described in Step 1 is placed in a palladium nitrate solution containing dimethylaminoethanol and stirred at room temperature for 1 hour to allow adsorption. During stirring, the pH is controlled at 8.5 using NaOH solution. After adsorption is complete, the mixture is filtered to obtain the catalyst precursor. In the above palladium nitrate solution containing dimethylaminoethanol, the palladium nitrate concentration is 0.3g / ml, the dimethylaminoethanol mass percentage concentration is 0.1%, and the NaOH solution mass percentage concentration is 5%.
[0099] Step 3: The catalyst precursor is placed in a reducing agent solution and stirred for reduction to obtain a carbon-based material supported palladium catalyst; the reducing agent solution is a sodium formate solution with a mass percentage concentration of 10%, the stirring and reduction temperature is 80℃, and the stirring and reduction time is 1 hour; the mass of the reducing agent solution is 10 times the mass of the catalyst precursor.
[0100] Example 7
[0101] This embodiment provides a method for preparing a carbon-based material-supported palladium catalyst, wherein the carbon-based material-supported palladium catalyst is a Pd / C catalyst with a Pd mass percentage of 1%, and the preparation method includes:
[0102] Step 1: Provide a carbon-based material carrier, specifically including:
[0103] Step 101: Mix the salt solution, organic ligand, and alcohol in a mass ratio of 2:50:48 and stir at 60°C for 15 hours to obtain a sol; the salt solution is a ferric nitrate solution with a mass percentage concentration of 0.5 g / ml, the organic ligand is urea, and the alcohol is anhydrous ethanol.
[0104] Step 102: Dry the sol at 90°C to obtain a gel. Crush the gel and pass it through a 500-mesh sieve. Calcinate the sieved material at 700°C for 12 hours under N2 atmosphere to obtain carbon-based material precursor A.
[0105] Step 103: Mix activated carbon and carbon-based material precursor A at a mass ratio of 5:5, cook in nitric acid solution at 90°C for 2 hours, cool and filter, wash with pure water until pH is 5, and obtain acid-treated carrier; the mass percentage concentration of the nitric acid solution is 8%, and the mass of the nitric acid solution is 8 times the total mass of activated carbon and carbon-based material precursor A;
[0106] Step 104: Place the acid-treated carrier in an ethanol solution with a mass percentage concentration of 3% triethylamine, boil at 100°C for 2 hours, cool and filter to complete the modification, and obtain a carbon-based material carrier; the mass of the triethylamine ethanol solution is 10 times the mass of the carrier after acid treatment.
[0107] Step 2: According to the preset palladium mass percentage in the Pd / C catalyst, 100g of the carbon-based material support described in Step 1 is placed in a palladium nitrate solution containing dimethylaminoethanol and stirred at room temperature for 2 hours to allow adsorption. During stirring, the pH is controlled at 8.5 using NaOH solution. After adsorption is complete, the mixture is filtered to obtain the catalyst precursor. In the above palladium nitrate solution containing dimethylaminoethanol, the palladium nitrate concentration is 0.2g / ml, the dimethylaminoethanol mass percentage concentration is 0.1%, and the NaOH solution mass percentage concentration is 5%.
[0108] Step 3: The catalyst precursor is placed in a reducing agent solution and stirred for reduction to obtain a carbon-based material supported palladium catalyst; the reducing agent solution is a sodium borohydride solution with a mass percentage concentration of 10%, the stirring and reduction temperature is 80℃, and the stirring and reduction time is 2h; the mass of the reducing agent solution is 8 times the mass of the catalyst precursor.
[0109] Example 8
[0110] This embodiment provides a method for preparing a carbon-based material-supported palladium catalyst, wherein the carbon-based material-supported palladium catalyst is a Pd / C catalyst with a Pd mass percentage of 3%, and the preparation method includes:
[0111] Step 1: Provide a carbon-based material carrier, specifically including:
[0112] Step 101: Mix the salt solution, organic ligand, and alcohol in a mass ratio of 10:50:40 and stir at 100°C for 8 hours to obtain a sol; the salt solution is a solution containing ferric nitrate and copper nitrate, wherein the mass percentage concentration of copper nitrate solution and ferric nitrate solution in the solution containing ferric nitrate and copper nitrate is 0.5 g / ml; the organic ligand is thiourea and urea in a mass ratio of 1:1; and the alcohol is methanol.
[0113] Step 102: Dry the sol at 150°C to obtain a gel. Crush the obtained gel and pass it through a 350-mesh sieve. Calcinate the sieved material at 800°C for 8 hours under N2 atmosphere to obtain carbon-based material precursor A.
[0114] Step 103: Mix activated carbon and carbon-based material precursor A at a mass ratio of 7:3, cook in nitric acid solution at 90°C for 2 hours, cool and filter, wash with pure water until pH is 5, and obtain acid-treated carrier; the mass percentage concentration of the nitric acid solution is 5%, and the mass of the nitric acid solution is 10 times the total mass of activated carbon and carbon-based material precursor A;
[0115] Step 104: Place the acid-treated carrier in an ethanol solution with a mass percentage concentration of 3% triethylamine, cook at 90°C for 2 hours, cool and filter to complete the modification, and obtain a carbon-based material carrier; the mass of the triethylamine ethanol solution is 10 times the mass of the carrier after acid treatment.
[0116] Step 2: According to the preset palladium mass percentage in the Pd / C catalyst, 100g of the carbon-based material support described in Step 1 is placed in a palladium nitrate solution containing dimethylaminoethanol and stirred at room temperature for 3 hours to allow adsorption. During stirring, the pH is controlled at 8.5 using NaOH solution. After adsorption is complete, the mixture is filtered to obtain the catalyst precursor. In the above palladium nitrate solution containing dimethylaminoethanol, the palladium nitrate concentration is 0.2g / ml, the dimethylaminoethanol mass percentage concentration is 0.2%, and the NaOH solution mass percentage concentration is 5%.
[0117] Step 3: The catalyst precursor is placed in a reducing agent solution and stirred for reduction to obtain a carbon-based material supported palladium catalyst; the reducing agent solution is a sodium formate solution with a mass percentage concentration of 20%, the stirring and reduction temperature is 90℃, and the stirring and reduction time is 2h; the mass of the reducing agent solution is 10 times the mass of the catalyst precursor.
[0118] Example 9
[0119] This embodiment provides a method for preparing a carbon-based material-supported palladium catalyst, wherein the carbon-based material-supported palladium catalyst is a Pd / C catalyst with a Pd mass percentage of 5%, and the preparation method includes:
[0120] Step 1: Provide a carbon-based material carrier, specifically including:
[0121] Step 101: Mix the salt solution, organic ligand, and alcohol in a mass ratio of 10:50:40 and stir at 100°C for 8 hours to obtain a sol; the salt solution is a solution containing ferric nitrate and nickel nitrate, wherein the mass percentage concentration of copper nitrate solution and ferric nitrate solution in the solution containing ferric nitrate and nickel nitrate is 0.5 g / ml; the organic ligand is urea, melamine, and cyanuric acid in a mass ratio of 2:1:1; and the alcohol is methanol.
[0122] Step 102: Dry the sol at 150°C to obtain a gel. Crush the obtained gel and pass it through a 350-mesh sieve. Calcinate the sieved material at 800°C for 8 hours under N2 atmosphere to obtain carbon-based material precursor A.
[0123] Step 103: Mix activated carbon and carbon-based material precursor A at a mass ratio of 7:3, cook in nitric acid solution at 90°C for 2 hours, cool and filter, wash with pure water until pH is 5, and obtain acid-treated carrier; the mass percentage concentration of the nitric acid solution is 5%, and the mass of the nitric acid solution is 10 times the total mass of activated carbon and carbon-based material precursor A;
[0124] Step 104: Place the acid-treated carrier in an ethanol solution with a mass percentage concentration of 3% triethylamine, cook at 90°C for 2 hours, cool and filter to complete the modification, and obtain a carbon-based material carrier; the mass of the triethylamine ethanol solution is 8 times the mass of the carrier after acid treatment;
[0125] Step 2: According to the preset palladium mass percentage in the Pd / C catalyst, 100g of the carbon-based material support described in Step 1 is placed in a palladium nitrate solution containing dimethylaminoethanol and stirred at room temperature for 3 hours to allow adsorption. During stirring, the pH is controlled at 8.5 using NaOH solution. After adsorption is complete, the mixture is filtered to obtain the catalyst precursor. In the above palladium nitrate solution containing dimethylaminoethanol, the palladium nitrate concentration is 0.2g / ml, the dimethylaminoethanol mass percentage concentration is 0.2%, and the NaOH solution mass percentage concentration is 5%.
[0126] Step 3: The catalyst precursor is placed in a reducing agent solution and stirred for reduction to obtain a carbon-based material supported palladium catalyst; the reducing agent solution is a sodium formate solution with a mass percentage concentration of 20%, the stirring and reduction temperature is 90℃, and the stirring and reduction time is 1 hour; the mass of the reducing agent solution is 8 times the mass of the catalyst precursor.
[0127] Comparative Example 1
[0128] This comparative example provides a method for preparing a Pd / C catalyst, comprising: mixing palladium nitrate solution and activated carbon for 1 hour according to a preset Pd mass percentage of 5% in the Pd / C catalyst; introducing sodium formate into the mixed system; stirring and reducing for 1 hour; washing; and filtering to obtain the Pd / C catalyst.
[0129] Comparative Example 2
[0130] The preparation method of this comparative catalyst is based on Example 4 of patent CN117085700A.
[0131] Application Example 1.1
[0132] This application example provides a method for catalytically synthesizing 5-pyrimidinecarboxaldehyde using the catalysts of Examples 1-9, Comparative Examples 1 and 2 as dechlorination catalysts. The raw materials include 4,6-dichloro-5-pyrimidinecarboxaldehyde, methanol, a Pd / C catalyst, and sodium bicarbonate. Based on a Pd mass percentage of 5% in the Pd / C catalyst, the mass ratio of 4,6-dichloro-5-pyrimidinecarboxaldehyde, methanol, Pd / C catalyst, and sodium bicarbonate is 5:75:0.1:1. In the catalytic synthesis of 5-pyrimidinecarboxaldehyde, the hydrogen pressure is 1.5 MPa, the reaction temperature is 70°C, the reaction time is 6 h, and the reaction speed is 900 r / min. Samples are taken for chromatographic analysis to determine the purity of the product in the system after the reaction. The results are shown in Table 2.
[0133] Table 2 Results of the catalytic synthesis of 5-pyrimidine carboxaldehyde
[0134]
[0135] As shown in Table 2, the dechlorination catalyst prepared by the method of the present invention can achieve a product purity of up to 94.6% in the synthesis of 5-pyrimidine formaldehyde. The catalyst prepared by the method of the present invention is significantly better than the traditional catalyst (Comparative Example 1); and its performance is slightly better than the catalyst prepared according to Example 4 of patent CN117085700A (Comparative Example 2).
[0136] Application Example 1.2
[0137] This application example provides a method for catalytic synthesis of 5-pyrimidine formaldehyde using the catalysts of Example 2 and Comparative Example 2 under sulfur poisoning conditions. The raw materials include sodium sulfide in addition to those in Application Example 1.1. The mass ratio of sodium sulfide to catalyst is 1:330. The results are shown in Table 3.
[0138] Table 3 Catalytic synthesis of 5-pyrimidinecarboxaldehyde under sulfur poisoning conditions
[0139]
[0140]
[0141] As can be seen from Table 3, the catalyst of the present invention can avoid poisoning and maintain high reactivity.
[0142] Application Example 1.3
[0143] This application example provides a method for synthesizing 5-pyrimidine formaldehyde by using the catalysts of Example 2 and Comparative Example 2. The method of application is the same as in Application Example 1.1. Each time the catalyst is used, no treatment is performed on the catalyst after the previous use. The data are as follows.
[0144] Table 4 shows the catalyst-catalyzed synthesis of 5-pyrimidinecarboxaldehyde.
[0145]
[0146] As shown in Table 4, the catalyst of the present invention can maintain high product purity even after being reused twice in the synthesis of 5-pyrimidine carboxaldehyde. The reaction activity and stability of the catalyst are significantly better than those of the comparative example.
[0147] Application Example 2.1
[0148] This application example provides a method for catalytically synthesizing 2,3-dichloropyridine using the catalysts of Examples 1-9, Comparative Examples 1, and Comparative Example 2 as dechlorination catalysts. The raw materials include 2,3,4,5-tetrachloropyridine, methanol, triethylamine, and a Pd / C catalyst. Based on a Pd mass percentage of 3% in the Pd / C catalyst, the mass ratio of 2,3,4,5-tetrachloropyridine, methanol, triethylamine, and the Pd / C catalyst is 25:80:15:0.05. In the catalytic synthesis of 2,3-dichloropyridine, the hydrogen pressure is 1.0 MPa, the reaction temperature is 45°C, the reaction time is 6 h, and the reaction speed is 900 r / min. Samples were taken for chromatographic analysis to determine the purity of the products in the system after the reaction; the results are shown in Table 5.
[0149] Table 5 Results of the catalytic synthesis of 2,3-dichloropyridine
[0150]
[0151] As shown in Table 5, the dechlorination catalyst prepared by the method of the present invention can achieve a product purity of up to 65.8% in the catalytic synthesis of 2,3-dichloropyridine. The catalyst prepared by the method of the present invention is significantly higher than that of the comparative example.
[0152] Application Example 2.2
[0153] This application example provides a method for catalytic synthesis of 2,3-dichloropyridine using the catalysts of Example 2 and Comparative Example 2 under sulfur poisoning conditions. The raw materials include sodium sulfide in addition to those in Application Example 2.1, with a mass ratio of sodium sulfide to catalyst of 1:250. The results are shown in Table 6.
[0154] Table 6. Catalytic synthesis of 2,3-dichloropyridine under sulfur poisoning conditions.
[0155]
[0156]
[0157] As can be seen from Table 6, the catalyst of the present invention can avoid poisoning and maintain high reactivity.
[0158] Application Example 2.3
[0159] This application example provides a method for catalytic synthesis of 2,3-dichloropyridine using the catalysts of Example 2 and Comparative Example 2. The method of application is the same as in Application Example 2.1. Each time the catalyst is applied, no treatment is performed on the catalyst after the previous use. The data are as follows.
[0160] Table 7. Catalytic Synthesis of 2,3-Dichloropyridine Using Utilizing Different Catalysts
[0161]
[0162] As shown in Table 7, the catalyst of the present invention can maintain high product purity even after being reused four times in the synthesis of 2,3-dichloropyridine. The reaction activity and stability of the catalyst are significantly better than those of the comparative example.
[0163] As can be seen from Application Examples 1 and 2, the dechlorination reaction catalyst of the present invention exhibits superior catalytic ability in the catalytic dechlorination reaction, as demonstrated by the significant improvement in the purity of the super-product in the synthesis of 5-pyrimidinecarboxaldehyde and the synthesis of 2,3-dichloropyridine.
[0164] Application Example 3
[0165] This application example provides a method for catalytically synthesizing biotin using the catalysts of Examples 1-2 and Comparative Examples 1-2 as dechlorination catalysts. The raw materials include: D-biotin intermediate, methanol, and a Pd / C catalyst. Based on a Pd mass percentage of 5% in the Pd / C catalyst, the mass ratio of the D-biotin intermediate, methanol, and Pd / C catalyst is 5:13:0.05. In the catalytic synthesis of D-biotin, the hydrogen pressure is 4.5 MPa, the reaction temperature is 110 °C, the reaction time is 3 h, and the reaction speed is 600 r / min. Samples were taken for chromatographic analysis to determine the purity of the products in the system after the reaction; the results are shown in Table 8.
[0166] Table 8 Catalytic Synthesis of Biotin
[0167]
[0168] As shown in Table 8, the reaction substrate in the catalytic synthesis of biotin contains sulfur atoms, which has a certain poisoning effect on the catalyst. When biotin is synthesized using the catalyst of the present invention, the purity of the product still exceeds 93%, which is significantly higher than that of the comparative example. Combined with application examples 1 to 3, it can be seen that the catalyst of the present invention has excellent resistance to the poisoning effect of the raw materials themselves and the poisoning effect during the reaction process.
[0169] The above description is merely a preferred embodiment of the present invention and does not constitute any limitation on the present invention. Any simple modifications, alterations, or equivalent structural changes made to the above embodiments based on the technical essence of the invention shall still fall within the protection scope of the present invention.
Claims
1. A method for preparing a carbon-based material-supported noble metal palladium catalyst, characterized in that, include: Step 1: Provide a carbon-based material carrier, specifically including: Step 101: Mix the metal soluble salt solution, organic ligand, and alcohol in a mass ratio of (2-15):(10-50):(35-88), and stir the mixture at 60-100℃ for 8-15 hours to obtain a sol; the metal soluble salt is one or more of ferric nitrate, copper nitrate, and nickel nitrate; the organic ligand is one or more of dicyandiamide, thiourea, pyridazine, melamine, cyanuric acid, and urea. Step 102: Dry the sol at 90-150°C to obtain a gel. Crush the obtained gel and pass it through a 300-500 mesh sieve. Calcinate the sieved material at 600-900°C for 6-12 hours under N2 atmosphere to obtain carbon-based material precursor A. Step 103: Mix activated carbon and carbon-based material precursor A in a mass ratio of (1-9):(9-1), cook in nitric acid solution at 90℃-100℃ for 1-2 hours, cool, filter, and wash to obtain acid-treated carrier; Step 104: Place the acid-treated carrier in an ethanol solution of triethylamine, cook at 90℃~100℃ for 1h~2h, cool and filter to complete the modification, and obtain a carbon-based material carrier. Step 2: According to the preset palladium mass percentage in the Pd / C catalyst, place the carbon-based material support described in Step 1 in a palladium nitrate solution containing dimethylaminoethanol, stir at room temperature for 1-3 hours to allow adsorption, filter, and obtain the catalyst precursor. Step 3: Place the catalyst precursor in a reducing agent solution and stir to reduce it, thereby obtaining a carbon-based material supported on a noble metal palladium catalyst.
2. The method for preparing a carbon-based supported noble metal palladium catalyst according to claim 1, characterized in that, The carbon-based material supported palladium catalyst is a Pd / C catalyst with a Pd mass percentage of 1% to 5%.
3. The method for preparing a carbon-based material-supported noble metal palladium catalyst according to claim 1, characterized in that, In step 101, the alcohol is methanol or anhydrous ethanol.
4. The method for preparing a carbon-based supported noble metal palladium catalyst according to claim 1, characterized in that, In step 103, the mass percentage concentration of the nitric acid solution is 5% to 10%, and the mass of the nitric acid solution is 8 to 10 times the total mass of the activated carbon and the carbon-based material precursor A.
5. The method for preparing a carbon-based supported noble metal palladium catalyst according to claim 1, characterized in that, In step 104, the mass percentage concentration of the triethylamine ethanol solution is 3%, and the mass of the triethylamine ethanol solution is 8 to 10 times the mass of the acid-treated carrier.
6. The method for preparing a carbon-based supported noble metal palladium catalyst according to claim 1, characterized in that, In step two, the palladium nitrate solution containing dimethylaminoethanol has a palladium nitrate concentration of 0.1 g / ml to 0.5 g / ml and a dimethylaminoethanol mass percentage concentration of 0.1% to 0.3%.
7. The method for preparing a carbon-based supported noble metal palladium catalyst according to claim 1, characterized in that, In step three, the reducing agent solution is a sodium formate solution or a sodium borohydride solution with a mass percentage concentration of 10% to 20%, the stirring and reduction temperature is 80℃ to 90℃, the stirring and reduction time is 1h to 2h, and the mass of the reducing agent solution is 8 to 10 times the mass of the catalyst precursor.
8. The method for preparing a carbon-based material-supported noble metal palladium catalyst according to claim 1, characterized in that, Step two also includes controlling the pH of the system to 8.5 during the adsorption process.
9. A dechlorination catalyst, characterized in that, The dechlorination catalyst is prepared by the method described in claim 1 for preparing a carbon-based material supported on a noble metal palladium catalyst.
Citation Information
Patent Citations
Catalyst for selective hydrogenation reaction of aromatic nitrocompound and preparation method of catalyst
CN105032424A
Preparation method and application method of catalyst special for dechlorination
CN117085700A