Raney nickel carbon nanotube composite catalyst and method for preparing amine compound by using Raney nickel carbon nanotube composite catalyst

Through the preparation of Rainey nickel carbon nanotube composite catalyst, the existing Rainey nickel catalyst has been solved, and the problem of poor stability and low selectivity in the adipiconet hydrogenation reaction is achieved, and high-efficiency hydrogenation reaction and high-selectivity amines are achieved. Preparation of compounds like this, suitable for large-scale production.

CN118988346APending Publication Date: 2024-11-22BEIJING RISUN TECH CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411072832.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The existing Rainey nickel catalysts have poor stability, fast activity attenuation, low selectivity, and large catalyst usage in the preparation of hexanediamine in the hydrogenation of adiponitrile, which is difficult to meet the demand for increased domestic production capacity.

Method used

Using Rainey nickel carbon nanotube composite catalyst, the Rainey nickel carbon carbon is formed by dispersing, drying and calculating the aqueous solution of metal soluble salt with the carbon nanotubes, and adding wet Rainey nickel catalyst under the protection of inert gas, ball milling and calculating to form Rainey nickel carbon. Nanotube composite catalyst for hydrogenation reaction under specific conditions.

Benefits of technology

The hydrogenation reaction rate and conversion rate are improved, the selectivity of the product is improved, and a high activity, high stability and low cost catalyst is formed, suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118988346A_ABST
    Figure CN118988346A_ABST
Patent Text Reader

Abstract

The invention relates to a Raney nickel carbon nanotube composite catalyst and a method for preparing an amine compound by using the Raney nickel carbon nanotube composite catalyst. The Raney nickel carbon nanotube composite catalyst is formed by compounding a metal modified carbon nanotube and a Raney nickel catalyst, and shows high hydrogenation conversion rate and product selectivity in a reaction for preparing an amine compound.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of amine compound synthesis, and in particular to a Raney nickel carbon nanotube composite catalyst and a method for preparing amine compounds using the same. Background Art

[0002] Raney nickel catalyst is a sieve-shaped catalyst with active nickel as the main component. It was first invented by Murray Raney in the 1920s and is widely used in hydrogenation reactions in organic synthesis. It is valued by chemical research and industrial production for its high efficiency and low cost. Compared with precious metal catalytic grade, Raney nickel catalyst has the advantages of higher activity and low cost, and is widely used in the industry of preparing hexamethylenediamine by hydrogenation of adiponitrile. However, the existing Raney nickel catalyst often has the disadvantages of poor stability, fast activity decay, low selectivity, and large catalyst dosage during use. Patent CN103977819A discloses a modified Raney nickel catalyst, which is prepared by mixing a soluble salt of a metal with NaOH to form a solution, mixing with Raney nickel powder under microwave conditions, and then drying, roasting, and reducing to obtain a modified Raney nickel catalyst, but this method is not conducive to amplification production; Patent CN104923240A discloses a nickel-based sepiolite supported catalyst modified and improved with potassium and lanthanum as auxiliary agents, but the catalyst still has the disadvantages of low activity and poor selectivity. As the domestic production capacity of hexamethylenediamine produced by hydrogenation of adiponitrile gradually increases, it is extremely important to develop a highly active, highly stable and low-cost hydrogenation catalyst.

[0003] Carbon nanotubes are nanoscale tubular carbon materials that are 2 It has good adsorption and hydrogen overflow-promoting properties and is a good hydrogenation catalyst carrier or promoter [Applied Catalysis A: General 468 (2013) 44-51].

[0004] Therefore, there is a need to develop an efficient catalyst for preparing amine compounds by hydrogenation and a method for preparing amine compounds using the catalyst. Summary of the invention

[0005] The present invention provides a method for preparing a Raney nickel-carbon nanotube composite catalyst, the method comprising the following steps:

[0006] 1) adding an aqueous solution of a soluble metal salt to carbon nanotubes, dispersing for 1 to 48 hours, drying, and calcining, wherein the metal is selected from one or more of V, Cr, Mn, Fe, Co, Ni, Mo, and Cu, preferably Ni;

[0007] 2) reducing the material obtained in step 1);

[0008] 3) adding a wet Raney nickel catalyst in a solvent to the material obtained in step 2) under the protection of an inert gas, ball milling, removing excess solvent under the protection of an inert gas, and drying;

[0009] 4) placing the material obtained in step 3) in an inert gas atmosphere, calcining it in a rotary kiln, and cooling it naturally under the protection of the inert gas to obtain a Raney nickel-carbon nanotube composite catalyst.

[0010] In a specific embodiment, in step 1), in the aqueous solution of the metal soluble salt, the concentration of the metal soluble salt is 0.01 mol / L to 5 mol / L.

[0011] In a specific embodiment, in step 1), the carbon nanotubes are multi-walled carbon nanotubes. Multi-walled carbon nanotubes are selected in the present application because they have good hydrogen adsorption capacity.

[0012] In a specific embodiment, in step 1), the mass ratio of the aqueous solution of the metal soluble salt to the carbon nanotubes is 0.2:1 to 20:1.

[0013] In a specific implementation, in step 1), the dispersion technique is selected from ultrasound, mechanical stirring, and ball milling.

[0014] In a specific implementation, in step 1), the drying temperature is 30°C to 150°C, the time is 1h to 48h, and the calcination temperature is 300°C to 600°C, and the time is 0.5h to 24h.

[0015] In a specific embodiment, in step 2), the reduction can be carried out by using one or both of hydrogen and carbon monoxide, with a reduction temperature of 200° C. to 550° C. and a time of 1 h to 48 h.

[0016] In a specific embodiment, in step 3), the inert gas may be one or more of nitrogen and argon.

[0017] In a specific embodiment, in step 3), the mass ratio of the wet-base Raney nickel catalyst to the multi-walled carbon nanotubes is 100:0.5 to 100:20.

[0018] In a specific embodiment, in step 3), the solvent is selected from water and ethanol, preferably water.

[0019] In a specific implementation manner, in step 3), the ball milling speed is 30 to 1000 r / min, and the ball milling time is 1 min to 48 h.

[0020] In a specific embodiment, in step 3), the drying temperature is 30° C. to 150° C., and the drying time is 1 h to 48 h.

[0021] In a specific implementation, in step 4), the inert gas is one of nitrogen and argon, the calcination temperature is 300° C. to 1000° C., and the calcination time is 1 h to 48 h.

[0022] In a specific embodiment, in step 4), the obtained composite catalyst can be sealed with one or more of water, methanol, ethanol, nitrogen and argon.

[0023] In another aspect, the present invention provides a Raney nickel-carbon nanotube composite catalyst prepared by the above method.

[0024] On the other hand, the present invention provides a method for preparing amine compounds, which comprises: adding the composite catalyst prepared above, nitrile compounds, solvents, and additives into a reactor, and introducing hydrogen gas, and performing a hydrogenation reaction at a certain temperature and pressure to obtain amine compounds.

[0025] In a specific embodiment, the reactor can be one of a fixed bed reactor, a fluidized bed reactor, a batch tank reactor, and a continuous tank hydrogenation reactor.

[0026] In a specific embodiment, the nitrile compound includes aliphatic / alicyclic nitrile, for example, a dinitrile compound or a mononitrile compound, for example, adiponitrile, glutaronitrile, 6-aminocapronitrile.

[0027] In a specific embodiment, the solvent is a saturated monohydric alcohol, for example, the solvent may be anhydrous ethanol.

[0028] In a specific embodiment, the auxiliary agent is an aqueous solution of an alkali metal or alkaline earth metal hydroxide or ammonia, for example, the auxiliary agent is an aqueous solution of sodium hydroxide.

[0029] In a specific embodiment, the mass ratio of nitrile compound: auxiliary agent: solvent is 100:(0.1-20):(10-1000); the mass of nitrile compound treated per kg catalyst per hour is between 0.1kg and 200kg, preferably between 0.5kg and 10kg.

[0030] In a specific embodiment, in the hydrogenation reaction, the reaction temperature is 40°C-150°C, the reaction pressure is 1MPa-12MPa, and the reaction time is 1s-10h.

[0031] Beneficial Effects

[0032] After the catalyst of the present application is modified by metal, the metal microcrystals loaded on the CNTs and the nickel microcrystals in the Raney nickel undergo Ostwald ripening at high temperature to form large alloy / nickel crystal particles, so that the CNTs with excellent hydrogen adsorption capacity and the nickel microcrystals at the hydrogenation active sites are combined at the atomic level, and the surface of the active sites reaches a state of local hydrogen enrichment, which accelerates the speed of hydrogen diffusion to the active sites, thereby increasing the hydrogenation reaction rate. On this basis, the composite catalyst of the present application also shows high hydrogenation conversion rate and product selectivity in the reaction of preparing amine compounds. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 The XRD spectrum of the Raney nickel-carbon nanotube composite catalyst prepared in Example 8 is shown. DETAILED DESCRIPTION

[0034] The technical solution of the present invention is further illustrated by the following examples.

[0035] Materials and reagents

[0036] Multi-walled carbon nanotubes were prepared according to the reference [Carbon 35 (1997) 1495–1501.], and the other chemicals used were purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.

[0037] method:

[0038] In the following examples, the composition of the hydrogenation product was analyzed by using an Agilent 7890B gas chromatograph, an HP-5 column, 60 meters in length, and an FID detector. The conversion of the feedstock and the selectivity of the product were calculated by the internal standard method.

[0039] Example 1

[0040] 1) Dissolve 5.8 g of nickel nitrate hexahydrate in 5 g of water, add to 5 g of multi-walled carbon nanotubes, let stand and disperse for 24 hours, dry at 100° C. for 4 hours, and calcine at 600° C. for 1 hour;

[0041] 2) The material obtained in step 1 was treated with H 2 Reduce at 350 °C for 2 h;

[0042] 3) Add 1000 g of wet Raney nickel catalyst (containing 25% water) to the material obtained in step 2 under nitrogen protection. Ball mill for 12 h at a speed of 300 r / min, remove excess water under nitrogen protection, and dry at 100° C. for 8 h;

[0043] 4) placing the material obtained in step 3 in a nitrogen atmosphere, calcining in a rotary kiln at 300° C. for 48 h, and naturally cooling to room temperature under nitrogen protection to obtain a Raney nickel-carbon nanotube composite catalyst, which is sealed in water for later use;

[0044] 5) Hydrogenation reaction: 10 g of the composite catalyst prepared in step 4, 250 g of adiponitrile, 300 g of anhydrous ethanol, and 0.025 g of a 30% sodium hydroxide solution were added to a batch reactor, and hydrogen was introduced. The system temperature was controlled at 90° C. and the pressure was 6.0 MPa. After reacting for 1 h, the product composition was analyzed. The data are listed in Table 1 below.

[0045] Example 2

[0046] 1) 8.7 g nickel nitrate hexahydrate was dissolved in 20 g water, added to 80 g multi-walled carbon nanotubes, mechanically stirred for 4 hours, dried at 30° C. for 48 hours, and calcined at 400° C. for 2 hours;

[0047] 2) The material obtained in step 1 was treated with H 2 Reduction at 400 °C for 8 h;

[0048] 3) Add 800 g of wet Raney nickel catalyst (containing 25% water) to the material obtained in step 2 under nitrogen protection, ball mill for 8 hours at a speed of 800 r / min, remove excess water under nitrogen protection, and dry at 110° C. for 4 hours;

[0049] 4) placing the material obtained in step 3 in a nitrogen atmosphere, calcining in a rotary kiln at 700° C. for 6 h, and naturally cooling to room temperature under nitrogen protection to obtain a Raney nickel-carbon nanotube composite catalyst, which is sealed in water for later use;

[0050] 5) Hydrogenation reaction: 15 g of the composite catalyst prepared in step 4, 220 g of glutaronitrile, 330 g of anhydrous ethanol, and 3 g of a 30% sodium hydroxide solution were added to a batch reactor, and hydrogen was introduced. The system temperature was controlled at 60° C. and the pressure was 12 MPa. After reacting for 2 h, the product composition was analyzed. The data are listed in Table 1 below.

[0051] Example 3

[0052] 1) Dissolve 11.6 g nickel nitrate hexahydrate in 100 g water, add to 30 g multi-walled carbon nanotubes, stir mechanically for 2 hours, dry at 120° C. for 6 hours, and calcine at 500° C. for 2 hours;

[0053] 2) The material obtained in step 1 was treated with H 2 Reduction at 500°C for 12h;

[0054] 3) Add 700 g of wet Raney nickel catalyst (containing 25% water) to the material obtained in step 2 under nitrogen protection, ball mill for 48 hours at a speed of 30 r / min, remove excess water under nitrogen protection, and dry at 130° C. for 4 hours;

[0055] 4) The material obtained in step 3 is placed in a nitrogen atmosphere, calcined at 700° C. for 12 h in a rotary kiln, and naturally cooled to room temperature under nitrogen protection to obtain a Raney nickel carbon nanotube composite catalyst, which is sealed in ethanol for later use.

[0056] 5) Hydrogenation reaction: 20 g of the composite catalyst prepared in step 4, 20 g of adiponitrile, 530 g of anhydrous ethanol, and 0.5 g of a 30% sodium hydroxide solution were added to a batch reactor, and hydrogen was introduced. The system temperature was controlled at 60° C. and the pressure was 3 MPa. After reacting for 2 min, the product composition was analyzed. The data are listed in Table 1 below.

[0057] Example 4

[0058] 1) Dissolve 5.82 g of cobalt nitrate hexahydrate in 60 g of water, add to 70 g of multi-walled carbon nanotubes, let stand and disperse for 24 hours, dry at 110° C. for 24 hours, and calcine at 350° C. for 4 hours;

[0059] 2) The material obtained in step 1 was treated with H 2 Reduce at 370 °C for 6 h;

[0060] 3) Add 800 g of wet Raney nickel catalyst (containing 25% water) to the material obtained in step 2 under nitrogen protection. Ball mill for 4 h at a speed of 500 r / min, remove excess water under nitrogen protection, and dry at 110° C. for 12 h;

[0061] 4) The material obtained in step 3 is placed in a nitrogen atmosphere, calcined in a rotary kiln at 800° C. for 8 h, and naturally cooled to room temperature under nitrogen protection to obtain a Raney nickel-carbon nanotube composite catalyst, which is sealed in methanol for later use.

[0062] 5) Hydrogenation reaction: 50 g of the composite catalyst prepared in step 4, 240 g of adiponitrile, 310 g of anhydrous ethanol, and 10 g of a 30% sodium hydroxide solution were added to a batch reactor, and hydrogen was introduced. The system temperature was controlled at 70° C. and the pressure was 1 MPa. After reacting for 5 h, the product composition was analyzed. The data are listed in Table 1 below.

[0063] Example 5

[0064] 1) Dissolve 11.6 g nickel nitrate hexahydrate in 40 g water, add to 50 g multi-walled carbon nanotubes, stir mechanically for 1 hour, dry at 100° C. for 24 hours, and calcine at 450° C. for 8 hours;

[0065] 2) The material obtained in step 1 was treated with H 2 Reduction at 200°C for 48h;

[0066] 3) Add 800 g of wet Raney nickel catalyst (containing 25% water) to the material obtained in step 2 under nitrogen protection. Ball mill for 12 h at a speed of 100 r / min, remove excess water under nitrogen protection, and dry at 100° C. for 24 h;

[0067] 4) The material obtained in step 3 is placed in a nitrogen atmosphere, calcined at 600° C. for 8 h in a rotary kiln, and naturally cooled to room temperature under nitrogen protection to obtain a Raney nickel-carbon nanotube composite catalyst, which is sealed in water for later use.

[0068] 5) Hydrogenation reaction: 12 g of the composite catalyst prepared in step 4 was added to a batch reactor, 250 g of 6-aminocapronitrile, 300 g of anhydrous ethanol, and 4 g of a 30% sodium hydroxide solution were added, hydrogen was introduced, the system temperature was controlled at 120° C., the pressure was 5 MPa, and the product composition was analyzed after reacting for 30 min. The data are listed in Table 1 below.

[0069] Example 6

[0070] 1) Dissolve 11.64 g of cobalt nitrate hexahydrate in 50 g of water, add to 80 g of multi-walled carbon nanotubes, let stand and disperse for 24 hours, dry at 110° C. for 8 hours, and calcine at 550° C. for 2 hours;

[0071] 2) The material obtained in step 1 was treated with H 2 Reduction at 400 °C for 8 h;

[0072] 3) Add 800 g of wet Raney nickel catalyst (containing 25% water) to the material obtained in step 2 under nitrogen protection, ball mill for 12 h at a speed of 350 r / min, remove excess water under nitrogen protection, and dry at 110° C. for 8 h;

[0073] 4) The material obtained in step 3 is placed in a nitrogen atmosphere, calcined in a rotary kiln at 700° C. for 6 h, and naturally cooled to room temperature under nitrogen protection to obtain a Raney nickel-carbon nanotube composite catalyst, which is sealed in water for later use.

[0074] 5) Hydrogenation reaction: 15 g of the composite catalyst prepared in step 4, 350 g of adiponitrile, 200 g of anhydrous ethanol, and 10 g of a 30% sodium hydroxide solution were added to a batch reactor, and hydrogen was introduced. The system temperature was controlled at 40° C. and the pressure was 8 MPa. After reacting for 10 h, the product composition was analyzed. The data are listed in Table 1 below.

[0075] Example 7

[0076] 1) Dissolve 20g of ferrous chloride tetrahydrate in 50g of water, add to 100g of multi-walled carbon nanotubes, let stand and disperse for 48 hours, dry at 150°C for 1h, and calcine at 400°C for 12h;

[0077] 2) The material obtained in step 1 was treated with H2 Reduction at 350 °C for 6 h;

[0078] 3) Add 700 g of wet Raney nickel catalyst (containing 25% water) to the material obtained in step 2 under nitrogen protection. Ball mill for 1 min at a speed of 1000 r / min, remove excess water under nitrogen protection, and dry at 110° C. for 8 h;

[0079] 4) The material obtained in step 3 is placed in a nitrogen atmosphere, calcined at 600° C. for 8 h in a rotary kiln, and naturally cooled to room temperature under nitrogen protection to obtain a Raney nickel-carbon nanotube composite catalyst, which is sealed in water for later use.

[0080] 5) Hydrogenation reaction: 25 g of the composite catalyst prepared in step 4, 260 g of glutaronitrile, 290 g of anhydrous ethanol, and 5 g of a 30% sodium hydroxide solution were added to a batch reactor, and hydrogen was introduced. The system temperature was controlled at 90° C. and the pressure was 10 MPa. After reacting for 1 h, the product composition was analyzed. The data are listed in Table 1 below.

[0081] Example 8

[0082] 1) Dissolve 23.2 g nickel nitrate hexahydrate in 40 g water, add to 90 g multi-walled carbon nanotubes, let stand for 24 hours, dry at 110° C. for 12 hours, and calcine at 500° C. for 12 hours;

[0083] 2) The material obtained in step 1 was treated with H 2 Reduction at 400 °C for 8 h;

[0084] 3) Add 450 g of wet Raney nickel catalyst (containing 25% water) to the material obtained in step 2 under nitrogen protection. Ball mill for 4 h at a speed of 300 r / min, remove excess water under nitrogen protection, and dry at 110° C. for 12 h;

[0085] 4) The material obtained in step 3 is placed in a nitrogen atmosphere, calcined in a rotary kiln at 900° C. for 6 h, and naturally cooled to room temperature under nitrogen protection to obtain a Raney nickel-carbon nanotube composite catalyst, which is sealed in water for later use.

[0086] In addition, XRD analysis of the composite catalyst powder prepared in this example was performed on an X'pert PRO X-ray diffractometer from PANalytical of the Netherlands. The instrument working conditions were: Cu target, working current 30 mA, working voltage 40 kV; graphite monochromator, Kα as radiation source; scanning speed 10 deg / min. XRD spectrum can be found at Figure 1 .

[0087] It can be seen from the figure that the Ni grains of the composite catalyst are still small, but there is no obvious grain enlargement.

[0088] 5) Hydrogenation reaction: 36 g of the composite catalyst prepared in step 4 was added to a batch reactor, 1 g of 6-aminocapronitrile, 545 g of anhydrous ethanol, and 0.1 g of a 30% sodium hydroxide solution were added, and hydrogen was introduced. The system temperature was controlled at 150° C. and the pressure was 3 MPa. After reacting for 1 second, the product composition was analyzed. The data are listed in Table 1 below.

[0089] Example 9

[0090] 1) Dissolve 25g of ferrous chloride tetrahydrate in 50g of water, add to 60g of multi-walled carbon nanotubes, let stand and disperse for 48 hours, dry at 120°C for 6h, and calcine at 300°C for 24h;

[0091] 2) The material obtained in step 1 was treated with H 2 Reduction at 450 °C for 4 h;

[0092] 3) Add 700 g of wet Raney nickel catalyst (containing 25% water) to the material obtained in step 2 under nitrogen protection, ball mill for 2 h at a speed of 1000 r / min, remove excess water under nitrogen protection, and dry at 120° C. for 6 h;

[0093] 4) The material obtained in step 3 is placed in a nitrogen atmosphere, calcined in a rotary kiln at 500° C. for 12 h, and naturally cooled to room temperature under nitrogen protection to obtain a Raney nickel-carbon nanotube composite catalyst, which is sealed in water for later use.

[0094] 5) Hydrogenation reaction: 10 g of the composite catalyst prepared in step 4, 270 g of adiponitrile, 280 g of anhydrous ethanol, and 8 g of a 30% sodium hydroxide solution were added to a batch reactor, and hydrogen was introduced. The system temperature was controlled at 60° C. and the pressure was 2.5 MPa. After reacting for 1 h, the product composition was analyzed. The data are listed in Table 1 below.

[0095] Example 10

[0096] 1) Dissolve 11.6 g nickel nitrate hexahydrate in 40 g water, add to 50 g multi-walled carbon nanotubes, let stand and disperse for 12 hours, dry at 110° C. for 8 hours, and calcine at 450° C. for 12 hours;

[0097] 2) The material obtained in step 1 was treated with H 2 Reduce at 550 °C for 2 h;

[0098] 3) Add 1000 g of wet Raney nickel catalyst (containing 25% water) to the material obtained in step 2 under nitrogen protection, ball mill for 8 h at a speed of 600 r / min, remove excess water under nitrogen protection, and dry at 110° C. for 8 h;

[0099] 4) The material obtained in step 3 is placed in a nitrogen atmosphere, calcined in a rotary kiln at 1000° C. for 1 h, and naturally cooled to room temperature under nitrogen protection to obtain a Raney nickel-carbon nanotube composite catalyst, which is sealed in water for later use.

[0100] 5) Hydrogenation reaction: 40 g of the composite catalyst prepared in step 4, 230 g of adiponitrile, 320 g of anhydrous ethanol, and 5 g of a 30% sodium hydroxide solution were added to a batch reactor, and hydrogen was introduced. The system temperature was controlled at 60° C. and the pressure was 2 MPa. After reacting for 1 h, the product composition was analyzed. The data are listed in Table 1 below.

[0101] Embodiment 11

[0102] 1) Dissolve 11.6 g nickel nitrate hexahydrate in 60 g water, add to 50 g multi-walled carbon nanotubes, let stand for 12 hours, dry at 120° C. for 24 hours, and calcine at 400° C. for 8 hours;

[0103] 2) The material obtained in step 1 was treated with H 2 Reduce at 350°C for 24h;

[0104] 3) Add 800 g of wet Raney nickel catalyst (containing 25% water) to the material obtained in step 2 under nitrogen protection. Ball mill for 12 h at a speed of 100 r / min, remove excess water under nitrogen protection, and dry at 100° C. for 24 h;

[0105] 4) The material obtained in step 3 was placed in a nitrogen atmosphere, calcined at 550° C. for 8 h in a rotary kiln, and naturally cooled to room temperature under nitrogen protection to obtain a Raney nickel-carbon nanotube composite catalyst, which was sealed in water for later use.

[0106] 5) Hydrogenation reaction: 50 g of the composite catalyst prepared in step 4, 156 g of terephthalonitrile, 394 g of anhydrous ethanol, and 4 g of a 30% sodium hydroxide solution were added to a batch reactor, and hydrogen was introduced. The temperature of the system was controlled at 120° C. and the pressure was 5 MPa. After reacting for 0.5 h, the product composition was analyzed. The data are listed in Table 1 below.

[0107] Example 12

[0108] 1) Dissolve 12g of chromium nitrate nonahydrate in 60g of water, add to 45g of multi-walled carbon nanotubes, let stand and disperse for 12 hours, dry at 120°C for 24h, and calcine at 400°C for 4h;

[0109] 2) The material obtained in step 1 was treated with H 2 Reduction at 450 °C for 4 h;

[0110] 3) Add 1000 g of wet Raney nickel catalyst (containing 25% water) to the material obtained in step 2 under nitrogen protection, ball mill for 8 h at a speed of 200 r / min, remove excess water under nitrogen protection, and dry at 110° C. for 8 h;

[0111] 4) The material obtained in step 3 is placed in a nitrogen atmosphere, calcined at 600° C. for 4 h in a rotary kiln, and naturally cooled to room temperature under nitrogen protection to obtain a Raney nickel-carbon nanotube composite catalyst, which is sealed in water for later use.

[0112] 5) Hydrogenation reaction: 40 g of the composite catalyst prepared in step 4, 250 g of adiponitrile, 300 g of anhydrous ethanol, and 2 g of a 30% sodium hydroxide solution were added to a batch reactor, and hydrogen was introduced. The system temperature was controlled at 80° C. and the pressure was 2.5 MPa. After reacting for 1 h, the product composition was analyzed. The data are listed in Table 1 below.

[0113] Example 13

[0114] 1) Dissolve 11.6 g nickel nitrate hexahydrate in 70 g water, add to 50 g multi-walled carbon nanotubes, let stand and disperse for 24 hours, dry at 120° C. for 6 hours, and calcine at 400° C. for 12 hours;

[0115] 2) The material obtained in step 1 was treated with H 2 Reduction at 350 °C for 8 h;

[0116] 3) Add 700 g of wet Raney nickel catalyst (containing 25% water) to the material obtained in step 2 under nitrogen protection, ball mill for 8 h at a speed of 500 r / min, remove excess water under nitrogen protection, and dry at 120° C. for 8 h;

[0117] 4) The material obtained in step 3 was placed in a nitrogen atmosphere, calcined at 650° C. for 12 h in a rotary kiln, and naturally cooled to room temperature under nitrogen protection to obtain a Raney nickel-carbon nanotube composite catalyst, which was sealed in water for later use.

[0118] 5) Hydrogenation reaction: 30 g of the composite catalyst prepared in step 4, 300 g of adiponitrile, 250 g of isopropanol, and 8 g of 30% sodium hydroxide solution were added to a batch reactor, and hydrogen was introduced. The system temperature was controlled at 60° C. and the pressure was 2.5 MPa. After reacting for 1 h, the product composition was analyzed. The data are listed in Table 1 below.

[0119] Embodiment 14

[0120] 1) Dissolve 11.6 g nickel nitrate hexahydrate in 50 g water, add to 50 g multi-walled carbon nanotubes, let stand and disperse for 12 hours, dry at 110° C. for 8 hours, and calcine at 450° C. for 6 hours;

[0121] 2) The material obtained in step 1 was treated with H2 Reduction at 400 °C for 8 h;

[0122] 3) Add 800 g of wet Raney nickel catalyst (containing 25% water) to the material obtained in step 2 under nitrogen protection. Ball mill for 12 h at a speed of 300 r / min, remove excess water under nitrogen protection, and dry at 110° C. for 8 h;

[0123] 4) The material obtained in step 3 is placed in a nitrogen atmosphere, calcined in a rotary kiln at 700° C. for 6 h, and naturally cooled to room temperature under nitrogen protection to obtain a Raney nickel-carbon nanotube composite catalyst, which is sealed in water for later use.

[0124] 5) Hydrogenation reaction: 30 g of the composite catalyst prepared in step 4, 350 g of adiponitrile, 250 g of anhydrous ethanol, and 4 g of a 30% potassium hydroxide solution were added to a batch reactor, and hydrogen was introduced. The system temperature was controlled at 70° C. and the pressure was 3 MPa. After reacting for 1 h, the product composition was analyzed. The data are listed in Table 1 below.

[0125] Comparative Example 1

[0126] In a batch reactor, 10 g of a commercially available quaternary alloy series Raney nickel catalyst (Shanghai Xunkai New Material Technology Co., Ltd., RaneCAT-1200) was added, 270 g of adiponitrile, 280 g of anhydrous ethanol, and 8 g of a 30% sodium hydroxide solution were added, hydrogen was introduced, the system temperature was controlled at 60°C, the pressure was 2.5 MPa, and the product composition was analyzed after reacting for 1 h. The data are listed in Table 1 below.

[0127] Comparative Example 2

[0128] 1) Add 50 g of water to 60 g of multi-walled carbon nanotubes, let stand and disperse for 48 hours, dry at 120° C. for 6 hours, and calcine at 300° C. for 24 hours;

[0129] 2) The material obtained in step 1 was treated with H 2 Reduction at 450 °C for 4 h;

[0130] 3) Add 700 g of wet Raney nickel catalyst (containing 25% water) to the material obtained in step 2 under nitrogen protection, ball mill for 2 h at a speed of 1000 r / min, remove excess water under nitrogen protection, and dry at 120° C. for 6 h;

[0131] 4) The material obtained in step 3 is placed in a nitrogen atmosphere, calcined in a rotary kiln at 500° C. for 12 h, and naturally cooled to room temperature under nitrogen protection to obtain a Raney nickel-carbon nanotube composite catalyst, which is sealed in water for later use.

[0132] 5) Hydrogenation reaction: 10 g of the composite catalyst prepared in step 4, 270 g of adiponitrile, 280 g of anhydrous ethanol, and 8 g of a 30% sodium hydroxide solution were added to a batch reactor, and hydrogen was introduced. The system temperature was controlled at 60° C. and the pressure was 2.5 MPa. After reacting for 1 h, the product composition was analyzed. The data are listed in Table 1 below.

[0133] Table 1 Hydrogenation conversion and selectivity in Examples 1-14 and Comparative Examples 1-2

[0134] serial number Hydrogenation conversion rate, % Selectivity of diamine in product, % Example 1 96.4 97.5 Example 2 98.5 98.1 Example 3 99.3 98.4 Example 4 99.2 97.9 Example 5 96.4 99.1 Example 6 99.8 97.3 Example 7 96.3 98.5 Example 8 99.9 99.3 Example 9 91.9 97.2 Example 10 96.3 98.4 Embodiment 11 95.4 99.0 Example 12 95.8 97.7 Embodiment 13 95.9 97.1 Embodiment 14 97.5 97.6 Comparative Example 1 82.6 95.2 Comparative Example 2 82.2 95.5

[0135] It should be noted that after metal-modified CNT, the modified metal will be combined with the nickel crystallites in Raney nickel through Ostwald ripening, grow into large grains, and CNT and active center nickel reach atomic-level dispersion and mixing, which combines the hydrogen storage of CNT with the hydrogenation of Raney nickel, and improves the conversion rate of the catalyst and the selectivity of hydrogenated products. However, since CNT without metal modification does not have the "anchoring" of metal, CNT cannot reach the atomic-level contact effect after combining with Raney nickel, but can reduce the catalyst activity (see the data of Comparative Examples 1 and 2), which can also be confirmed by the data in Table 1. Compared with the composite catalyst of commercially available Raney nickel and carbon nanotubes without metal modification, the catalyst provided by the present invention shows higher catalytic activity in the catalytic hydrogenation reaction to generate amine compounds, and the selectivity of the target product is improved, and the generation of by-products is reduced, so it has greater economic value.

Claims

1. A method for preparing a Raney nickel-carbon nanotube composite catalyst, the method comprising the following steps: 1) adding an aqueous solution of a metal soluble salt to carbon nanotubes, dispersing for 1 to 48 hours, drying, and calcining, wherein the metal of the metal soluble salt is selected from one or more of V, Cr, Mn, Fe, Co, Ni, Mo, and Cu, preferably Ni; 2) reducing the material obtained in step 1); 3) adding a wet Raney nickel catalyst in a solvent to the material obtained in step 2) under the protection of an inert gas, ball milling, removing excess solvent under the protection of an inert gas, and drying; 4) placing the material obtained in step 3) in an inert gas atmosphere, calcining it in a rotary kiln, and cooling it naturally under the protection of the inert gas to obtain a Raney nickel-carbon nanotube composite catalyst.

2. The method according to claim 1, wherein: In step 1), In the aqueous solution of the metal-soluble salt, the concentration of the metal-soluble salt is 0.01 mol / L to 5 mol / L; and / or The carbon nanotubes are multi-walled carbon nanotubes; and / or The weight ratio of the aqueous solution of the metal soluble salt to the carbon nanotubes is 0.2:1 to 20:1; and / or The dispersion technique is selected from ultrasound, mechanical stirring, and ball milling; and / or The drying temperature is 30-150°C, and the time is 1-48h; the calcination temperature is 300-600°C, and the time is 0.5h-24h.

3. The method according to claim 1, wherein: In step 2), the reduction is carried out by using one or both of hydrogen and carbon monoxide, the reduction temperature is 200° C. to 550° C., and the time is 1 h to 48 h.

4. The method according to claim 2, wherein: In step 3), The inert gas is one or more of nitrogen and argon; and / or The mass ratio of the wet-based Raney nickel catalyst to the multi-walled carbon nanotubes is 100:0.5 to 100:20; and / or The solvent is selected from water and ethanol, preferably water; and / or The ball milling speed is 30 to 1000 r / min, and the ball milling time is 1 min to 48 h; and / or The drying temperature is 30-150°C and the time is 1-48 hours.

5. The method according to claim 1, wherein: In step 4), The inert gas is one of nitrogen and argon, the calcination temperature is 300° C. to 1000° C., and the calcination time is 1 to 48 hours; and / or The obtained Raney nickel carbon nanotube composite catalyst is sealed with one or more of water, methanol, ethanol, nitrogen and argon.

6. A Raney nickel-carbon nanotube composite catalyst, prepared by the method according to any one of claims 1 to 5.

7. A method for preparing an amine compound, the method comprising the following steps: The composite catalyst as claimed in claim 6, nitrile compounds, solvents, and additives are added into a reactor, and hydrogen is introduced to carry out a hydrogenation reaction to obtain amine compounds.

8. The method according to claim 7, wherein: The reactor is one selected from a fixed bed reactor, a fluidized bed reactor, a batch reactor and a continuous reactor hydrogenation reactor.

9. The method according to claim 7, wherein: The nitrile compound includes aliphatic / alicyclic nitrile, for example, a dinitrile compound or a mononitrile compound, for example, adiponitrile, glutaronitrile, 6-aminocapronitrile; and / or The solvent is a saturated monohydric alcohol, such as anhydrous ethanol; and / or The auxiliary agent is an aqueous solution of an alkali metal or alkaline earth metal hydroxide or ammonia, preferably an aqueous solution of sodium hydroxide; and / or The mass ratio of nitrile compound: auxiliary agent: solvent is 100:(0.1-20):(10-1000); the mass of nitrile compound treated per kg catalyst per hour is between 0.1kg and 200kg, preferably between 0.5kg and 10kg.

10. The method according to claim 7, wherein: The reaction temperature of the hydrogenation reaction is 40-150° C., the reaction pressure is 1-12 MPa, and the reaction time is 1 s-10 h.

Citation Information

Patent Citations

  • Preparation method for carbon nanotube loaded quaternary amorphous nickel-based catalyst and application

    CN107486208A

  • Preparation method of 2-methylpentanediamine

    CN111377820A

  • Method for preparing hexamethylenediamine by hydrogenation of adiponitrile

    CN114436852A

  • Carbon-modified metal reduction catalyst and preparation method and application thereof

    CN115155631A