Solid acid nanosheet catalyst for catalyzing CO2 absorption pregnant solution desorption and preparation method of solid acid nanosheet catalyst

By designing a nanosheet HZSM-5 zeolite catalyst with short b-axis thickness, the high energy consumption and diffusion limitation problems of the desorption process in CO2 capture technology are solved, the efficiency and energy efficiency of CO2 desorption are improved, and the cost of CO2 capture is reduced.

CN118988388AActive Publication Date: 2024-11-22TIANFU YONGXING LAB

Patent Information

Application Number
CN202411055027.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-02
Publication Date
2024-11-22
Estimated Expiration
2044-08-02

AI Technical Summary

Technical Problem

In the existing CO2 capture technology, the high energy consumption and diffusion limitation of the CO2 desorption process hinder the industrial application of the technology, especially the mass transfer limitation caused by long micropore channels in three-dimensional zeolite materials reduces the utilization efficiency of active volume and separation and transmission efficiency.

Method used

A short b-axis thickness nanosheet HZSM-5 zeolite catalyst was designed, and nanosheets were prepared by hydrothermal treatment and autoclave synthesis method to reduce the b-axis thickness of MFI zeolite to reduce diffusion limits and improve the CO2 desorption mass transfer rate.

Benefits of technology

By reducing the b-axis thickness of MFI zeolite, the diffusion limit of CO2 desorption is significantly reduced, the mass transfer rate of desorption is improved, the regeneration energy consumption of CO2 absorption and rich liquid is reduced, and the cost of capturing CO2 is reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118988388A_ABST
    Figure CN118988388A_ABST
Patent Text Reader

Abstract

The invention discloses a solid acid nanosheet catalyst for catalyzing CO2 absorption pregnant solution desorption and a preparation method of the solid acid nanosheet catalyst. As the straight channel of the MFI zeolite is parallel to the b-axis, a faster diffusion rate can be observed in this direction. When the size of the nanocrystal is lower than 50nm, the influence of diffusion limitation is remarkably relieved. Thus, reducing the b-axis thickness of the MFI zeolite is an effective strategy to reduce diffusion limitations. The nanosheet HZSM-5 zeolite with the short b-axis thickness smaller than 50 nm is designed and used for CO2 absorption pregnant solution desorption, so that the diffusion limitation of CO2 desorption is reduced, the desorption mass transfer rate is increased, the regeneration energy consumption of CO2 absorption pregnant solution is reduced, and the CO2 capture cost is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of CO2 capture, and in particular relates to a catalyst for catalyzing the desorption of CO2 absorbed rich liquid. Background Art

[0002] my country is the world's largest energy consumer. The increase in energy demand has led to the extensive use of fossil fuels in power plants, which in turn has led to increased carbon dioxide (CO2) emissions, greatly harming the atmospheric environment. CO2 absorption by monoethanolamine (MEA) aqueous solvent plays a key role in post-combustion CO2 capture. However, in traditional MEA technology, CO2 desorption often occurs at high temperatures (110-140°C) due to the endothermic reaction of carbamate decomposition. This desorption process accounts for more than 70% of the total heat loss of the CO2 capture device, and the high energy consumption hinders the large-scale industrial application of CO2 capture technology.

[0003] Zeolites are an important class of porous inorganic crystalline materials, mainly including silicates (germanates) (such as ZSM-5), phosphates (arsenates) (such as AIPO4-5), or silicophosphates (such as SAPO-34). Zeolite molecular sieves have been widely used in ion exchange, adsorption separation and catalysis since their synthesis due to their rich framework topology and elemental composition. In the past decade, although zeolites have made remarkable progress in CO2 catalytic desorption, the mass transfer limitation caused by the presence of long microporous channels in three-dimensional (3D) zeolite materials remains an unresolved problem, which not only leads to low utilization efficiency of zeolite active volume, but also limits the transfer efficiency in separation and catalytic processes. HZSM-5 zeolite (MFI-type framework) catalyst has high acidity, excellent Bronsted acid sites (BAS) and Lewis acid sites (LAS). Researchers use it to accelerate the proton transfer rate of CO2 rich solution desorption process and reduce the desorption reaction heat of carbamate (AmineCOO-), so as to reduce the energy demand of CO2 rich solution desorption process. Shi et al. (Int. J Greenh. Gas Con., 2014, 26: 39-50.) first proposed the use of solid acid catalyst HZSM-5 to promote CO2 desorption and reduce solvent regeneration energy consumption. Compared with no catalyst added, adding HZSM-5 can reduce energy consumption by 35%. Patent CN 111715274 discloses a preparation method and application of a multiphase catalyst for desorbing CO2 from a solution. The catalyst SO4 2- / Metal oxide-HZSM-5 is used for the desorption of CO₂-rich amine solution. Compared with the case without a catalyst, the desorption rate is increased by 35-45%, and it can be recycled more than 4 times. Although HZSM-5 zeolite has excellent catalytic performance, it has two intersecting 10-membered ring channels, and the micropore size is in the range of 0.5-0.6 nm. The existence of micropores limits the diffusion and mass transfer of CO₂. Therefore, the limitation brought by the existence of long micropore channels in three-dimensional (3D) zeolite materials remains an issue to be solved, which not only leads to low utilization efficiency of the active volume of zeolite, but also limits the transport efficiency in the molecular sieve. This negative impact is particularly prominent for diffusion-limited reactions. The quite long micropores of bulk zeolite seriously hinder the diffusion of molecules, resulting in pore blockage and catalyst deactivation. Currently, all reports on using solid acid to catalyze CO₂ desorption adopt bulk zeolite, which greatly affects the diffusion rate and desorption efficiency of CO₂ desorption. Summary of the Invention

[0004] Aiming at the deficiencies of the prior art, the purpose of the present invention is to provide a solid acid nanosheet catalyst for catalyzing the desorption of CO₂-rich absorption liquid and its preparation method. By designing HZSM-5 zeolite with a short b-axis thickness nanosheet for the desorption of CO₂-rich absorption liquid, the diffusion limitation of CO₂ desorption is reduced, the desorption mass transfer rate is increased, thereby reducing the regeneration energy consumption of CO₂-rich absorption liquid and the cost of capturing CO₂.

[0005] Since the straight channels of MFI zeolite are parallel to the b-axis, faster diffusion rates can be observed in this direction. When the nanocrystal size is below 50 nm, the influence of diffusion limitation is significantly alleviated. Therefore, reducing the b-axis thickness of MFI zeolite is an effective strategy to reduce diffusion limitation. The present invention designs and synthesizes MFI zeolite with a short diffusion length along the b-axis, which can reduce the influence of diffusion limitation in catalyzing CO₂ desorption and improve the desorption efficiency.

[0006] The solid acid nanosheet catalyst (HZSM-5 zeolite) for catalyzing the desorption of CO₂-rich absorption liquid provided by the present invention is a nanosheet of HZSM-5 zeolite (MFI zeolite), and its b-axis thickness < 150 nm, preferably 20 nm < b-axis thickness < 150 nm, more preferably 20 nm < b-axis thickness < 50 nm.

[0007] The preparation method of the solid acid nanosheet (HZSM-5 nanosheet) catalyst for catalyzing the desorption of CO₂-rich absorption liquid provided by the present invention includes the following steps:

[0008] (1) Synthesis of nanocrystal seed suspension

[0009] The nanocrystalline seed suspension is prepared under hydrothermal treatment. 10 to 60 parts by mass of tetraethyl orthosilicate (TEOS) and 50 to 80 parts by mass of tetrapropylammonium hydroxide are mixed and stirred at 20 to 40°C for 4 to 6 hours to obtain a hydrolyzed clear solution; the obtained solution is heated to 40 to 60°C to remove ethanol produced by TEOS hydrolysis; the solution is then transferred to a stainless steel autoclave lined with polytetrafluoroethylene, and hydrothermally treated at 50 to 90°C under static conditions for 24 to 72 hours to obtain a nanocrystalline seed suspension with a size of 20 nm.

[0010] (2) Synthesis of HZSM-5 nanosheets

[0011] A silicon source, an organic base, deionized water and a nanocrystal seed suspension are mixed to prepare a solution A; an aluminum source and NH4F are dissolved in deionized water to prepare solutions B and C respectively; after stirring solution A at 35°C for 4 to 6 hours, solutions B and C are added dropwise in sequence to obtain a mixed solution; the mixed solution is vigorously stirred for 1 to 2 hours to obtain a precursor gel; the obtained gel is transferred to a stainless steel autoclave lined with polytetrafluoroethylene, and after crystallization at 170°C for 1 day, the solid product is centrifuged 2 to 3 times, rinsed with deionized water to neutrality, dried at 80 to 100°C for 12 to 24 hours, and then calcined in air at 500 to 600°C for 4 to 6 hours to obtain HZSM-5 nanosheets.

[0012] The molar ratio of the silicon source, aluminum source, organic base, NH4F, and the total amount of deionized water used is 1:(0.001-0.1):(0.01-1.0):(0.1-1.0):(50-200) according to SiO2:Al2O3:organic base:NH4F:H2O, that is, the amount of the silicon source is calculated based on the amount of SiO2, the amount of the aluminum source is calculated based on the amount of aluminum oxide Al2O3, and the deionized water is the total amount of deionized water used in this step. The amount of the nanocrystalline seed suspension added accounts for 0.1-100% of the mass of SiO2 in the silicon source.

[0013] In the above method, further, the molar ratio of the silicon source, the aluminum source, the organic base, NH4F, and the total amount of deionized water used is preferably 1:0.04:0.14:0.8:160 according to SiO2:Al2O3:organic base:NH4F:H2O.

[0014] In the above method, further, the silicon source is at least one of tetraethylammonium hydroxide, tetrapropylammonium hydroxide, tetrabutylammonium hydroxide or tetrapropylammonium bromide; the aluminum source is at least one of aluminum nitrate, aluminum chloride and aluminum isopropoxide.

[0015] The present invention also provides the use of the solid acid nanosheets in desorption of CO2 absorption rich solution. The CO2 absorption rich solution refers to a solution obtained by absorbing CO2 through an alcohol amine chemical absorbent aqueous solution during CO2 capture.

[0016] Compared with the prior art, the present invention has the following beneficial effects:

[0017] The present invention designs nanosheet HZSM-5 zeolite with a short b-axis thickness for CO2 absorption and rich liquid desorption, reduces the diffusion limitation of CO2 desorption, improves the desorption mass transfer rate, and realizes low-energy catalytic desorption of CO2. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 SEM images of nanosheets with different b-axis thickness prepared in the examples (including b-axis thickness distribution diagram): (a) ZN-1 30nm; (b) ZN-2 40nm; (c) ZN-3 50nm; (d) ZN-4 85nm; (e) ZN-5 130nm; (f) is the SEM image of NK-Z5 of comparative example 2 (including b-axis thickness distribution diagram);

[0019] Figure 2 is the XRD pattern of nanosheet zeolite with different b-axis thickness;

[0020] Figure 3 N2 adsorption-desorption isotherms of nanosheet zeolites with different b-axis thicknesses prepared in Example;

[0021] Figure 4 NH3-TPD of nanosheet zeolites with different b-axis thickness prepared in Example;

[0022] Figure 5 Py-IR of nanosheet zeolites with different b-axis thicknesses prepared in Examples. DETAILED DESCRIPTION

[0023] The present invention is further described below by way of examples. It is necessary to point out that the following examples are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Those skilled in the art may make some non-essential improvements and adjustments to the present invention according to the above-mentioned invention content and implement the invention specifically, which still falls within the scope of protection of the invention.

[0024] In the following examples, the prepared HZSM-5 nanosheets are denoted as ZN-y (y is the number of different samples).

[0025] Example 1

[0026] (1) Synthesis of Nanocrystalline Seed Suspension:

[0027] The nanocrystalline seed suspension was prepared under hydrothermal treatment. 30 g of tetraethyl orthosilicate (TEOS) was mixed with 50 g of tetrapropylammonium hydroxide and stirred at 35°C for 4 hours to obtain a hydrolyzed clear solution; the solution was heated to 45°C to remove the ethanol produced by the hydrolysis of TEOS, and then transferred to a stainless steel autoclave lined with polytetrafluoroethylene and hydrothermally treated at 70°C under static conditions for 72 hours to obtain a nanocrystalline seed suspension.

[0028] (2) Synthesis of HZSM-5 nanosheets

[0029] Ethyl orthosilicate, tetraethylammonium hydroxide and nanocrystalline seed suspension were dissolved in a certain amount of deionized water to prepare solution A. Aluminum nitrate and NH4F were dissolved in deionized water to prepare solutions B and C. After stirring solution A at 35°C for 6 hours, solutions B and C were added dropwise in sequence to obtain a mixed solution. The mixed solution was stirred vigorously for 2 hours to obtain a precursor gel, which was then transferred to a stainless steel autoclave lined with polytetrafluoroethylene. After crystallization at 170°C for 1 day, the solid product was centrifuged 3 times, rinsed with deionized water to neutrality, and dried at 80°C for 12 hours. The dried solid was calcined in air at 550°C for 6 hours to obtain HZSM-5 nanosheets, marked as ZN-1. Among them, the molar ratio of each part is 1SiO2:0.04Al2O3:0.2organic base:0.8NH4F:150H2O; the amount of nanocrystalline seed suspension added accounts for 50% of the mass percentage of SiO2.

[0030] Experimental procedures

[0031] The performance of HZSM-5 nanosheets catalyzing CO2 desorption prepared in Example 1 was evaluated using a laboratory-made CO2 absorption-desorption integrated device. The absorption was performed using a mass flow meter to simulate the flue gas composition (15% CO2-85% N2); the desorbed CO2 was diluted with an additional N2 flow, and the concentration of the mixed flow was measured by an infrared gas analyzer.

[0032] 1. Absorption experiment

[0033] 500 ml of 30% ethanolamine aqueous solution was used to simulate low-concentration CO2 flue gas with N2 / CO2 mixed gas (85 Vol.% / 15 Vol.%), and the absorption rich liquid with a CO2 loading of 0.52 mol CO2 / mol MEA was obtained.

[0034] The CO2 absorption rate and CO2 loading of the organic alcohol amine solution were calculated according to equations (1) and (2).

[0035]

[0036] In the formula, υ CO2is the rate at which the solution absorbs CO2, ml / min; is the N2 inlet rate, 100 mL / min; a is the CO2 concentration percentage at the outlet; is the volume of CO2 absorbed by the solution during time t, mL; t is time, min.

[0037] 2. Desorption experiment

[0038] 0.52 mol CO2 / mol MEA absorption rich solution was added to the reaction bottle, and the catalysts described in the comparative example and the embodiment were added respectively; the blank was thermal desorption without adding catalyst, and the amount of catalyst added was 0.5-2%. The desorption temperature was 80-100°C, and the desorption time was 60 minutes.

[0039] The concentration of CO2 during the desorption process was measured using an infrared gas analyzer, and the rate and amount of CO2 desorption catalyzed by the catalyst were calculated using equations (3) and (4).

[0040]

[0041] In the formula, is the amount of CO2 desorbed from the solution within time t, mmol; V des is the CO2 desorption rate of the solution, mmol / s; χ is the CO2 concentration percentage at the desorption outlet.

[0042] 3. Calculation of energy consumption for CO2 desorption

[0043] The evaluation parameter of the catalyst's catalytic CO2 desorption performance is the desorption energy consumption per unit mole of CO2, H (kJ / mol), which is defined as the ratio of the energy input rate to the CO2 desorption rate and is calculated by the following formula (5):

[0044]

[0045] Here E refers to the amount of electricity consumed by CO2 desorption within a certain period of time as recorded by the energy meter. The unit is kW·h and it needs to be converted into kJ when used.

[0046] Since the CO2 desorption energy consumption calculated by this method is only a relative value, in order to better evaluate the catalytic CO2 desorption performance of the catalyst, this project proposed and defined the parameter of relative desorption energy consumption RH (%), taking the desorption energy consumption of blank alcohol amine solution regenerated for 90 minutes as the benchmark (H b , kJ / mol), and its RH is 100%, then the RH of the catalytic CO2 desorption process is the desorption energy consumption H for catalytic CO2 desorption for 90 min. i (kJ / mol) and H b The ratio is calculated by the following formula (6):

[0047]

[0048] Example 2

[0049] (1) The method for synthesizing the nanocrystalline seed suspension is the same as that in Example 1.

[0050] (2) Synthesis of HZSM-5 nanosheets:

[0051] TEOS, tetrapropylammonium hydroxide and nanocrystalline seed suspension were dissolved in a certain amount of deionized water to prepare solution A. Aluminum nitrate and NH4F were dissolved in deionized water to prepare solutions B and C. After stirring solution A at 35°C for 6 hours, solutions B and C were added dropwise in sequence to obtain a mixed solution. The mixed solution was stirred vigorously for 2 hours to obtain a precursor gel, which was then transferred to a stainless steel autoclave lined with polytetrafluoroethylene. After crystallization at 170°C for 1 day, the solid product was centrifuged 3 times, rinsed with deionized water to neutrality, and dried at 80°C for 12 hours. Then, the dried solid was calcined at 550°C in air for 6 hours to obtain HZSM-5 nanosheets, marked as ZN-2. Among them, the molar ratio of silicon source, aluminum source, organic base, NH4F and water was 1SiO2:0.04Al2O3:0.2organic base:0.8NH4F:150H2O; the amount of nanocrystalline seed suspension added accounted for 20% by mass of SiO2.

[0052] The absorption and desorption experimental conditions and the energy consumption calculation method are the same as those in Example 1.

[0053] Example 3

[0054] (1) The method for synthesizing the nanocrystalline seed suspension is the same as that in Example 1.

[0055] (2) Synthesis of HZSM-5 nanosheets:

[0056] Ethyl orthosilicate, tetrapropylammonium bromide and nanocrystalline seeds were dissolved in a certain amount of deionized water to prepare solution A. Aluminum nitrate and NH4F were dissolved in deionized water to prepare solutions B and C. After stirring solution A at 35°C for 6 hours, solutions B and C were added dropwise in sequence to obtain a mixed solution. The mixed solution was stirred vigorously for 2 hours to obtain a precursor gel, which was then transferred to a stainless steel autoclave lined with polytetrafluoroethylene. After crystallization at 170°C for 1 day, the solid product was centrifuged 3 times, rinsed with deionized water to neutrality, and dried at 80°C for 12 hours. Then, the dried solid was calcined at 550°C in air for 6 hours to obtain HZSM-5 nanosheets, marked as ZN-3. Among them, the molar ratio of each part is 1SiO2:0.04Al2O3:0.2organic base:0.8NH4F:150H2O; the amount of nanocrystalline seed suspension added to the mass percentage of SiO2 is 5%.

[0057] The absorption and desorption experimental conditions and the energy consumption calculation method are the same as those in Example 1.

[0058] Example 4

[0059] (1) The method for synthesizing the nanocrystalline seed suspension is the same as that in Example 1.

[0060] (2) Synthesis of HZSM-5 nanosheets:

[0061] Ethyl orthosilicate, tetrabutylammonium hydroxide and nanocrystalline seeds were dissolved in a certain amount of deionized water to prepare solution A. Aluminum nitrate and NH4F were dissolved in deionized water to prepare solutions B and C. After stirring solution A at 35°C for 6 hours, solutions B and C were added dropwise in sequence to obtain a mixed solution. The mixed solution was stirred vigorously for 2 hours to obtain a precursor gel, which was then transferred to a stainless steel autoclave lined with polytetrafluoroethylene. After crystallization at 170°C for 1 day, the solid product was centrifuged 3 times, rinsed with deionized water to neutrality, and dried at 80°C overnight. Then, the dried solid was calcined at 550°C in air for 6 hours to obtain HZSM-5 nanosheets, marked as ZN-4. Among them, the molar ratio of each part is 1SiO2:0.04Al2O3:0.2organic base:0.8NH4F:150H2O; the amount of nanocrystalline seed suspension added to the mass percentage of SiO2 is 1%.

[0062] The method for synthesizing the nanocrystal seed suspension is the same as that in Example 1.

[0063] The absorption and desorption experimental conditions and the energy consumption calculation method are the same as those in Example 1.

[0064] Example 5

[0065] (1) The method for synthesizing the nanocrystalline seed suspension is the same as that in Example 1.

[0066] (2) Synthesis of HZSM-5 nanosheets:

[0067] Ethyl orthosilicate, tetraethylammonium hydroxide and nanocrystalline seeds were dissolved in a certain amount of deionized water to prepare solution A. Aluminum nitrate and NH4F were dissolved in deionized water to prepare solutions B and C. After stirring solution A at 35°C for 6 hours, solutions B and C were added dropwise in sequence to obtain a mixed solution. The mixed solution was stirred vigorously for 2 hours to obtain a precursor gel, which was then transferred to a stainless steel autoclave lined with polytetrafluoroethylene. After crystallization at 170°C for 1 day, the solid product was centrifuged several times, rinsed with deionized water to neutrality, and dried at 80°C overnight. Then, the dried solid was calcined at 550°C in air for 6 hours to obtain HZSM-5 nanosheets, marked as ZN-5. Among them, the molar ratio of each part is 1SiO2:0.04Al2O3:0.2organic base:0.8NH4F:150H2O; the amount of nanocrystalline seed suspension added to the mass percentage of SiO2 is 0.1%.

[0068] The absorption and desorption experimental conditions and the energy consumption calculation method are the same as those in Example 1.

[0069] Comparative Example 1

[0070] The absorption and desorption experimental conditions and the energy consumption calculation method were the same as in Example 1, but without adding a catalyst, which was recorded as blank.

[0071] Comparative Example 2

[0072] The absorption and desorption experimental conditions and the energy consumption calculation method are the same as those in Example 1. A commercial HZSM-5 zeolite (conventional b-axis thickness 80-800 nm) from Nankai University was purchased for comparison and recorded as NK-Z5.

[0073] Nanosheet zeolites with different b-axis thicknesses were synthesized by adjusting the amount of nanocrystal seeds. SEM images ( Figure 1 ) confirmed the successful synthesis of nanosheets, with average b-axis thicknesses of (a) ZN-1 30nm; (b) ZN-2 40nm; (c) ZN-3 50nm; (d) ZN-4 90nm; (e) ZN-5 130nm. Figure 2 It can be seen that the synthesized nanosheet zeolite samples with different b-axis thicknesses all have diffraction peaks at 7.9°, 8.8°, 23.1°, 23.9° and 24.3°, showing the typical MFI topological structure of H-ZSM-5, indicating that adjusting the thickness of the nanosheet does not change its structural characteristics.

[0074] Figure 3 The N2 adsorption-desorption isotherms of nanosheet zeolites with different b-axis thickness are shown. At relative pressures (P / P0) of 0.01-0.9, obvious type I isotherms can be observed for all samples, indicating that all HZSM-5 nanosheets have a typical microporous structure. With the increase of nanocrystal seeds (Table 1), the specific surface area (420→482m2 g -1 ) and mesopore volume (0.057→0.229cm 3 g -1 ) increases significantly, and among the samples, the ZN-1 sample has the highest specific surface area and mesopore volume, which is due to the stacking between very thin nanosheets, which is beneficial to improving the accessibility to acidic sites and the carbon deposition capacity of the catalyst.

[0075] As shown in Table 2, the ZN-1 sample with a b-axis thickness of 30 nm has the best catalytic desorption performance. Compared with the traditional thermal desorption (blank), the desorption energy consumption is reduced by 35.4%. There are three main reasons for the reduction in desorption energy consumption. First, the ZN-1 sample has the smallest b-axis thickness (30 nm) among the five nanosheet zeolites. The straight channel of the MFI zeolite is parallel to the b-axis. The smaller the b-axis thickness, the faster the desorption diffusion rate. Second, by quantifying the NH3-TPD of the five nanosheet zeolites, it was found that as the b-axis thickness shortened, the total acid content of the zeolite gradually increased ( Figure 4 ), ZN-1 sample has the highest total acid content. Although the total acid content of NK-Z5 in comparative example 2 is higher than that of ZN-1 sample, due to its wider b-axis thickness (700nm, Figure 1 f) affects its desorption diffusion rate, and then affects the desorption rate; thirdly, the changes in the ratio of B acid and L acid of five nanosheet zeolites were further analyzed by pyridine infrared, and the results are shown in Table 1, Figure 5 It can be seen that the increase in acid content caused by the shortening of the b-axis thickness is mainly due to the increase in the B acid content, which can enhance the desorption of carbamate (Amine - COO - ) breaks, increasing the desorption rate.

[0076] Table 1 Structure and acid properties of nanosheet zeolites with different b-axis thickness

[0077]

[0078]

[0079] Note: The total acid content is calculated based on the NH3-TPD spectrum. B / L is the ratio of Bronsted acid to Lewis acid, obtained by pyridine infrared.

[0080] Table 2 Comparison of relative desorption energy consumption of catalysts in the examples

[0081] serial number catalyst Relative desorption energy consumption RH (%) Energy consumption reduction (%) b-axis thickness (nm) Comparative Example 1 blank 100 / / Comparative Example 2 NK-Z5 81.2 18.8 700 Example 1 ZN-1 64.6 35.4 30 Example 2 ZN-2 69.4 30.6 40 Example 3 ZN-3 70.7 29.3 50 Example 4 ZN-4 73.2 26.8 90 Example 5 ZN-5 74.5 25.5 130

[0082] Note: The b-axis thickness of zeolite is obtained from SEM images.

Claims

1. A catalytic CO 2 Absorbing the solid acid nanosheet catalyst for desorption of rich liquid, It is characterized in that the catalyst is HZSM-5 zeolite nanosheets with a b-axis thickness < 150 nm.

2. The catalytic CO according to claim 1 2 Absorbing the solid acid nanosheet catalyst for desorption of rich liquid, It is characterized in that its b-axis thickness is 20 nm < b-axis thickness < 50 nm.

3. A catalytic CO 2 Preparation method of solid acid nanosheet catalyst for absorbing and desorbing rich liquid, It is characterized in that It includes the following steps: (1) Synthesis of nanocrystal seed suspension The nanocrystal seed suspension is prepared under hydrothermal treatment. 10 - 60 parts by mass of tetraethyl orthosilicate (TEOS) is mixed with 50 - 80 parts by mass of tetrapropylammonium hydroxide and stirred at 20 - 40 °C for 4 - 6 hours to obtain a hydrolyzed clear solution; The obtained solution is heated to 40 - 60 °C to remove the ethanol produced by the hydrolysis of TEOS; Then the solution is transferred to a stainless-steel autoclave with a polytetrafluoroethylene lining and hydrothermally treated at 50 - 90 °C under static conditions for 24 - 72 hours to obtain a nanocrystal seed suspension with a size of 20 nm; (2) Synthesis of solid acid nanosheet HZSM-5 nanosheets The silicon source, organic base, deionized water and nanocrystal seed suspension were mixed to prepare solution A; the aluminum source and NH 4 F was dissolved in deionized water to prepare solutions B and C, respectively; After stirring solution A at 35 °C for 4 - 6 h, solution B and C are successively added dropwise to obtain a mixed solution; the mixed solution is vigorously stirred for 1 - 2 h to obtain a precursor gel; The obtained gel is transferred to a stainless-steel autoclave with a polytetrafluoroethylene lining, crystallized at 170 °C for 1 day, the solid product is centrifuged 2 - 3 times, rinsed with deionized water until neutral, dried at 80 - 100 °C for 12 - 24 hours, and then calcined in air at 500 - 600 °C for 4 - 6 hours to obtain HZSM-5 nanosheets. Among them, silicon source, aluminum source, organic base, NH 4 F. The molar ratio of the total amount of deionized water used is based on SiO 2 :Al 2 O 3 :Organic base:NH 4 F:H 2 O is 1:(0.001~0.1):(0.01~1.0):(0.1~1.0):(50~200), that is, the amount of silicon source is SiO 2 Participation ratio calculation, the amount of aluminum source is based on the aluminum oxide Al 2 O 3 Participate in the ratio calculation, and deionized water is the total amount of deionized water used in this step.

4. According to the method described in claim 3, It is characterized in that The amount of nanocrystalline seed suspension added accounts for 1.3% of SiO in the silicon source. 2 The mass percentage is 0.1% to 100%.

5. According to the method described in claim 3, It is characterized in that the silicon source is at least one of tetraethyl orthosilicate and silica sol.

6. According to the method described in claim 3, It is characterized in that the organic base is at least one of tetraethylammonium hydroxide, tetrapropylammonium hydroxide, tetrabutylammonium hydroxide, or tetrapropylammonium bromide.

7. According to the method described in claim 3, It is characterized in that the aluminum source is at least one of aluminum nitrate, aluminum trichloride, and aluminum isopropoxide.

8. The solid acid nanosheet according to claim 1 is reacted with CO 2 Application in desorption of absorption rich liquid.

9. According to the application described in claim 8, It is characterized in that The CO 2 Absorption rich liquid refers to the 2 During the capture process, CO is absorbed by an aqueous solution of an amine chemical absorbent. 2 The resulting solution. 10.b The MFI zeolite with short diffusion length in CO 2 In the application of desorption of absorption rich liquid, the b-axis thickness of the MFI zeolite is less than 50nm.

Citation Information

Patent Citations

  • Preparation method of novel ZSM-5 zeolite nanosheet and application of novel ZSM-5 zeolite nanosheet in catalytic reaction

    CN115010145A

  • Hollow zeolite catalyst for CO2 absorption pregnant solution desorption as well as preparation method and application of hollow zeolite catalyst

    CN117943104A

  • Nanosheet zeolite for CO2 adsorption as well as preparation method and application thereof

    CN118767868A

Cited By

  • Dry glue water heating method for synthesizing sheet type ZSM-5 zeolite

    CN120440910A