Catalyst for preparing p-xylene through CO2 hydrogenation as well as preparation method and application of catalyst

Through a tandem catalytic system composed of hollow tubular HZSM-5 zeolite and ZnZrOx solid solution, the problem of low selectivity of the catalyst for xylene hydrogenation in the prior art is solved, high selectivity and stability are achieved, and sheet-like and chain-like The advantages of HZSM-5 zeolite prevent the isomerization of xylene.

CN118988389APending Publication Date: 2024-11-22NORTHWEST NORMAL UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411078642.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The existing CO2 hydrogenation catalyst is uncontrollable in thermodynamics and reaction kinetics, resulting in low selectivity, and the selectivity of paraxylene on the existing HZSM-5 zeolite is low, and the selectivity of aromatics is high, making it difficult to achieve Highly efficient CO2 conversion to xylene.

Method used

The hollow tubular HZSM-5 zeolite and ZnZrOx solid solution are used to form a tandem catalytic system. The silicon-aluminum ratio and water volume of zeolite are regulated through reasonable preparation methods to form a hollow tubular HZSM-5 zeolite with a special morphology, and combined with the metal oxide ZnZrOx, to form CO2 addition Hydrogen-made paraxylene catalyst.

Benefits of technology

Under the reaction conditions of 320°C, 3.0MPa, 2400 mL·g-1·h-1, the CO2 conversion rate was 16.3%, the aromatic selectivity was 71.3%, the para-selectivity of xylene reached 76.2%, and the 100-h There was no obvious inactivation in the stability test, achieving high selectivity and stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118988389A_ABST
    Figure CN118988389A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of catalysts, particularly relates to a catalyst for preparing p-xylene through CO2 hydrogenation and a preparation method and application thereof, and reports that the morphology of HZSM-5 zeolite is regulated and controlled through a reasonable means to enable the HZSM-5 zeolite to have a hollow tubular structure, and due to the special forming process of the hollow tubular morphology, the outer surface of the HZSM-5 zeolite does not contain aluminum, so that the content of the p-xylene is reduced. Therefore, the acidity of the outer surface of the zeolite is passivated, so that the zeolite has higher aromatic hydrocarbon selectivity than sheet-shaped HZSM-5 zeolite and higher paraxylene selectivity than chain-shaped HZSM-5 zeolite. The hollow tubular HZSM-5 zeolite and the ZnZrOx metal oxide form a series catalyst. Under the reaction conditions of 320 DEG C, 3.0 MPa, 2400 mL.g <-1 >. H <-1 > and H2 / CO2 = 3 / 1, the para-selectivity of p-xylene reaches 76.2%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of catalysts, and specifically relates to a CO2 hydrogenation catalyst for preparing p-xylene, and a preparation method and application thereof. Background Art

[0002] With the rapid development of the polyester industry, the domestic demand for polyethylene terephthalate (PET) is in short supply. Among them, paraxylene (PX) has attracted widespread attention as an important intermediate in the production of PET. The production of traditional PX mainly relies on the catalytic reforming process of naphtha in the petroleum route. This process not only leads to the increasing depletion of petroleum resources, but also aggravates the emission of greenhouse gases. Therefore, it is necessary to find an efficient, economical and environmentally friendly method for synthesizing PX. In recent years, CO2 hydrogenation reaction has become one of the focuses of one-carbon chemistry researchers as a sustainable development method. By converting waste CO2 resources into high-value-added chemicals, it can not only effectively reduce CO2 emissions, but also realize the recycling of carbon resources, which has important environmental and economic significance.

[0003] However, due to the uncontrollable thermodynamics and reaction kinetics, the high selectivity of CO2 hydrogenation to PX is still a great challenge. The tandem catalytic system composed of metal oxides and zeolites (Ox-Zeo) has the characteristics of effectively separating the two active centers of reactant activation (CO2 activation) and product generation (CC coupling), and is considered to be a potential strategy to achieve this goal. Studies have shown that the tandem catalytic reaction of the composite catalytic system that uses methanol and methoxy species as a bridge to connect CO2 hydrogenation to methanol and methanol to aromatics (MeOH-mediated route) is not a simple addition, but a coupling reaction. The aromatics generation reaction can drive CO2 hydrogenation to methanol. Binary metal oxides ZnZrO in solid solution x It is an active catalyst for the conversion of CO2 to methanol with high selectivity and stability. It has abundant oxygen vacancies and unique Zn-O-Zr asymmetric sites. Oxygen vacancies can provide more active sites for the activation of CO2, and the Zn-O-Zr asymmetric sites can promote the formation of formate during the reaction, and can promote the conversion of formate to methoxy species, thereby promoting the formation of methanol. The Zn site is responsible for the activation of H2, and the Zr site is conducive to the stability of the intermediate. The H2 cracking promoted by the Zn-O-Zr asymmetric site is to improve the ZnZrO x The key to the performance of the production of methanol, methoxy and other species on the catalyst.

[0004] As another component of the composite catalytic system, HZSM-5 zeolite has a unique three-dimensional pore structure. Its ten-membered ring pore structure (pore diameter of 0.51nm×0.55nm, 0.54nm×0.56nm) is comparable to the kinetic diameter of light aromatic molecules such as benzene, toluene, and xylene, and is an excellent catalyst for the methanol to aromatics (MTA) reaction. Its unique pore structure not only provides a spatial restriction for shape-selective catalysis, but also provides abundant access channels for reactants and products, and also provides a crystal structure basis for the preparation of highly selective, highly active, and highly resistant to carbon deposition and deactivation industrial catalysts. The catalytic activity of HZSM-5 zeolite is closely related to a certain crystal face or axis of the zeolite crystal. For example, the zigzag pore structure parallel to the a-axis in the crystal is conducive to the shape selectivity of the molecule, and the straight pore parallel to the b-axis is conducive to the transmission of the molecule, reducing the formation of carbon deposition in the pores and extending the life of the zeolite. It is reported that the flake-shaped HZSM-5 zeolite can significantly enhance the aromatization activity. Due to its shorter b-axis length, it is conducive to the transport and diffusion of substances, making it easier for guest molecules to enter the active sites and preventing the occurrence of side reactions. The smaller the aspect ratio of the b / a axis of the crystal, the more aromatic compounds are formed. The b-axis pore radius of the chain-shaped HZSM-5 zeolite is close to the molecular dynamic radius of p-xylene. Properly increasing the b-axis length is conducive to improving the selectivity of p-xylene. However, the selectivity of existing flake HZSM-5 zeolites for p-xylene is low, while the selectivity of chain-shaped HZSM-5 zeolites for aromatics is low. Summary of the invention

[0005] In view of the deficiencies of the above-mentioned prior art, the purpose of the present invention is to provide a CO2 hydrogenation catalyst for producing p-xylene, and a preparation method and application thereof, combining the advantages of flaky and chain HZSM-5 zeolites, constructing a hollow tubular HZSM-5 zeolite with a special morphology through reasonable means, and composite the hollow tubular HZSM-5 zeolite with a ZnZrOx solid solution to form a series catalytic system, thereby achieving the goal of improving the selectivity of p-xylene while maintaining high aromatics selectivity.

[0006] In order to solve the above technical problems, the present invention adopts the following technical solutions:

[0007] A method for preparing a catalyst for preparing p-xylene by hydrogenating CO2 comprises the following steps:

[0008] The seed gel is prepared by mixing tetraethyl orthosilicate and a template agent, tetrapropylammonium hydroxide;

[0009] adding sodium aluminate to the seed gel, stirring and then adding water to dilute it, impregnating quartz wool with the diluted seed gel, and then drying the quartz wool impregnated with the seed gel;

[0010] The dried quartz wool is subjected to steam-assisted crystallization, and then cooled, dried, and calcined to remove the template agent, thereby obtaining a hollow tubular sodium-type ZSM-5 zeolite;

[0011] Adding NH4Cl solution to the hollow tubular sodium-type ZSM-5 zeolite for ion exchange, followed by drying and calcining to obtain a hollow tubular HZSM-5 zeolite;

[0012] Hollow tubular HZSM-5 zeolite and metal oxide ZnZrO x The mixture is mixed to obtain a catalyst for preparing p-xylene by hydrogenating CO2.

[0013] In a preferred embodiment of the present invention, the molar ratio of tetraethyl orthosilicate to sodium aluminate is 100-150:1.

[0014] In a preferred embodiment of the present invention, the molar ratio of ethyl orthosilicate to tetrapropylammonium hydroxide is 100-150:0.2.

[0015] In a preferred embodiment of the present invention, the ratio of the added water to tetraethyl silicate is 18 mL: 100-150 mol.

[0016] In a preferred embodiment of the present invention, the hollow tubular HZSM-5 zeolite and the metal oxide ZnZrO x The mass ratio is 1~2:1~2.

[0017] In a preferred embodiment of the present invention, the steam-assisted crystallization temperature is 160-220° C., and the crystallization time is 30-50 h.

[0018] Another object of the present invention is to provide a catalyst for producing p-xylene by hydrogenating CO2 obtained by any of the preparation methods described above.

[0019] In a preferred embodiment of the present invention, the catalyst is composed of hollow tubular HZSM-5 zeolite and ZnZrO x The hollow tubular HZSM-5 zeolite and the metal oxide ZnZrO x The mass ratio is 1~2:1~2.

[0020] The third object of the present invention is to provide an application of the above-mentioned catalyst in the preparation of p-xylene by hydrogenation of CO2, characterized in that the reaction conditions are: the ratio of H2 / CO2 of the reaction raw gas is 3:1, the reaction temperature is 320°C, the reaction pressure is 3.0MPa, and the reaction gas space velocity is 2400mL·g -1 ·h -1 .

[0021] Compared with the prior art, the present invention has the following beneficial effects:

[0022] 1. The present invention adopts reasonable means to prepare Z5 zeolite with a hollow tubular morphology. The morphology of HZSM-5 zeolite is regulated by adjusting the silicon-aluminum ratio of the zeolite and the amount of water used to adjust the morphology of the zeolite so that it has a hollow tubular structure. Due to the special formation process of the hollow tubular morphology, the outer surface of the HZSM-5 zeolite does not contain aluminum, and the acidity of the outer surface of the zeolite is passivated, so that it has the advantages of high aromatics selectivity of flaky HZSM-5 zeolite and high para-xylene selectivity of chain HZSM-5 zeolite.

[0023] 2. The present invention combines hollow tubular HZSM-5 zeolite with ZnZrO x Metal oxide series catalyst, at 320℃, 3.0MPa, 2400mL·g -1 ·h -1 Under the reaction conditions of H2 / CO2=3 / 1, the CO2 conversion rate was 16.3%, the aromatics selectivity was 71.3%, and the para-selectivity of xylene reached 76.2%. The results show that the high para-xylene selectivity is attributed to the pore structure of the hollow tubular HZSM-5 zeolite, which is conducive to the formation of para-xylene, and the acidity of the passivated zeolite surface prevents the isomerization of para-xylene. In addition, in the 100h stability test, the catalyst did not show obvious deactivation, which provides an effective strategy for the design of catalysts for the selective preparation of specific aromatics by CO2 hydrogenation. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 XRD patterns of different samples prepared in the present invention; (a) Z5-HT with different Si / Al ratios; (b) Z5-HT with different H2O addition amounts; (c) XRD patterns of ZZO, Z5-HT and ZZO / Z5-HT;

[0025] Figure 2 The present invention shows (a) Z5-HT with different Si / Al ratios, (b) NH3-TPD spectra of ZZO, Z5-HT and ZZO / Z5-HT, and (c, d) Py-IR spectra of Z5-HT with different Si / Al ratios;

[0026] Figure 3 (a) The formation mechanism of the hollow tubular Z5 of the present invention; SEM images of Z5-HT, Si / Al ratio is (b) 30, (c) 60, (d) 100, (e) 150; water content is (f) 0mL, (g) 9mL, (h) 18mL, (i) 27mL, (m)-(p) SEM-EDS element mapping diagram;

[0027] Figure 4The effects of (a) ZZO and Z5 with different morphologies, (b) ZZO and Z5 with different Si / Al ratios, and (c) ZZO and Z5 with different H2O contents on the tandem catalysts for CO2 hydrogenation to aromatics of the present invention;

[0028] Figure 5 (a) para-xylene selectivity of the present invention; (b) stability evaluation of the ZZO / Z5-HT tandem catalyst in CO2 hydrogenation reaction. DETAILED DESCRIPTION

[0029] The following is a detailed description of the technical solutions in the embodiments of the present invention in combination with the preferred embodiments and the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0030] It should be noted that all professional terms used in the present invention are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention. Unless otherwise specifically stated, various raw materials, reagents, instruments and equipment used in the following embodiments of the present invention can be purchased from the market or prepared by existing methods.

[0031] Example 1

[0032] A method for preparing a catalyst for preparing p-xylene by hydrogenating CO2 comprises the following steps:

[0033] (1) Synthesis of hollow tubular HZSM-5

[0034] The raw material dosage ratio of the synthesis system is 100 mol SiO2: 0.2 mol TPAOH: 1.0 mol Al2O3: 18 mL H2O. 10.0 g of tetraethyl orthosilicate (TEOS) and 7.8 g of tetrapropylammonium hydroxide (TPAOH) were mixed and stirred at room temperature for 6 h to obtain a clear mixed liquid. Then it was treated in a rotary oven at 130 ° C for 12 h and a seed gel was obtained after cooling. Then sodium aluminate was added to the above 3.2 g seed gel, and after ultrasonic treatment for a period of time, it was stirred at room temperature for 2 h, and then 18 mL of deionized water was added to the above seed gel and continued to stir for 30 min. 1.0 g of quartz wool was impregnated with the diluted seed gel, and after standing for 60 min, it was transferred to a 60 ° C oven for drying for 12 h. Finally, the dried quartz wool was placed on a raised polytetrafluoroethylene support frame in a polytetrafluoroethylene liner, and the support frame was placed in a stainless steel autoclave. Add 5.0 mL of deionized water to the bottom of the inner liner, and perform steam-assisted crystallization at a high temperature of 180°C for 40 hours. After cooling to room temperature, the product was recovered and dried at 110°C for 12 hours. Finally, it was calcined at 550°C for 6 hours with a heating rate of 1°C / min. A hollow tubular sodium-type ZSM-5 zeolite was obtained. Then, ion exchange was performed with 1M NH4Cl solution (solid-liquid ratio of 1:30) at 90°C with stirring and reflux for 2.5 hours. The obtained sample was dried at 110°C for 12 hours, and then calcined at 550°C for 3 hours to obtain a hollow tubular HZSM-5 zeolite. The obtained sample was named Z5 100 (18)-HT.

[0035] (2) Synthesis of ZnZrOx solid solution

[0036] 1.2 g Zn(NO3)2·6H2O and 11.6 g Zr(NO3)4·5H2O were dissolved in a round-bottom flask filled with 200.0 mL deionized water. Then 200.0 mL precipitant containing 6.12 g (NH4)2CO3 was added to the previous solution using a separatory funnel at a rate of 3 mL / min. The mixture was stirred vigorously at 70 °C to form a precipitate. The mixture was stirred for 2 h, cooled to room temperature, washed with deionized water by centrifugation for 6 times, dried at 110 °C for 6 h, and calcined at 500 °C in a muffle furnace for 3 h to obtain ZnZrO x Solid solution, named ZZO.

[0037] (3) The hollow tubular HZSM-5 zeolite and ZnZrO x The metal oxides form a tandem catalyst.

[0038] Example 2

[0039] A method for preparing a catalyst for preparing p-xylene by hydrogenating CO2 comprises the following steps:

[0040] (1) Synthesis of hollow tubular HZSM-5

[0041] The raw material dosage ratio of the synthesis system is 150mol SiO2: 0.2mol TPAOH: 1.0molAl2O3: 18mL H2O. A certain amount of tetraethyl orthosilicate (TEOS) and tetrapropylammonium hydroxide (TPAOH) are mixed and stirred at room temperature for 6 hours to obtain a clear mixed liquid. Then it is treated in a rotary oven at 130℃ for 12 hours and a seed gel is obtained after cooling. Then sodium aluminate is added to the above 3.2g seed gel, and after ultrasonic treatment for a period of time, it is stirred at room temperature for 2 hours. After that, 18mL deionized water is added to the above seed gel and continued to stir for 30min. 1.0g quartz wool is impregnated with the diluted seed gel, and after standing for 60min, it is transferred to a 60℃ oven for drying for 12h. Finally, the dried quartz wool is placed on a raised polytetrafluoroethylene support frame in a polytetrafluoroethylene liner, and the support frame is placed in a stainless steel autoclave. 5.0mL deionized water is added to the bottom of the liner frame, and steam-assisted crystallization is carried out at a high temperature of 180℃ for 40h. After cooling to room temperature, the product was recovered and dried at 110°C for 12 hours. Finally, it was calcined at 550°C for 6 hours with a heating rate of 1°C / min. A hollow tubular sodium-type ZSM-5 zeolite was obtained. Then, ion exchange was performed with 1M NH4Cl solution (solid-liquid ratio of 1:30) at 90°C with stirring and reflux for 2.5 hours. The obtained sample was dried at 110°C for 12 hours and then calcined at 550°C for 3 hours to obtain a hollow tubular HZSM-5 zeolite. The obtained sample was named Z5 150 (18)-HT.

[0042] (2) Synthesis of ZnZrOx solid solution

[0043] 1.2 g Zn(NO3)2·6H2O and 11.6 g Zr(NO3)4·5H2O were dissolved in a round-bottom flask filled with 200.0 mL deionized water. Then 200.0 mL precipitant containing 6.12 g (NH4)2CO3 was added to the previous solution using a separatory funnel at a rate of 3 mL / min. The mixture was stirred vigorously at 70 °C to form a precipitate. The mixture was stirred for 2 h, cooled to room temperature, washed with deionized water by centrifugation for 6 times, dried at 110 °C for 6 h, and calcined at 500 °C in a muffle furnace for 3 h to obtain ZnZrO x Solid solution, named ZZO.

[0044] (3) The hollow tubular HZSM-5 zeolite and ZnZrO x The metal oxides form a tandem catalyst.

[0045] Example 3

[0046] A method for preparing a catalyst for preparing p-xylene by hydrogenating CO2 comprises the following steps:

[0047] (1) Synthesis of hollow tubular HZSM-5

[0048] The raw material dosage ratio of the synthesis system is 100 mol SiO2: 0.2 mol TPAOH: 1.0 mol Al2O3: 9 mL H2O. A certain amount of tetraethyl orthosilicate (TEOS) and tetrapropylammonium hydroxide (TPAOH) were mixed and stirred at room temperature for 6 hours to obtain a clear mixed liquid. Then it was treated in a rotary oven at 130 ° C for 12 hours and a seed gel was obtained after cooling. Then sodium aluminate was added to the above 3.2 g seed gel, and it was stirred at room temperature for 2 hours after ultrasonic treatment for a period of time. After that, 9 mL of deionized water was added to the above seed gel and continued to stir for 30 minutes. 1.0 g of quartz wool was impregnated with the diluted seed gel, and after standing for 60 minutes, it was transferred to a 60 ° C oven for drying for 12 hours. Finally, the dried quartz wool was placed on a raised polytetrafluoroethylene support frame in the polytetrafluoroethylene liner, and the support frame was placed in a stainless steel autoclave. 5.0 mL of deionized water was added to the bottom of the liner frame, and steam-assisted crystallization was carried out at a high temperature of 180 ° C for 40 hours. After cooling to room temperature, the product was recovered and dried at 110°C for 12 hours. Finally, it was calcined at 550°C for 6 hours with a heating rate of 1°C / min. A hollow tubular sodium-type ZSM-5 zeolite was obtained. Then, ion exchange was performed with 1M NH4Cl solution (solid-liquid ratio of 1:30) at 90°C with stirring and reflux for 2.5 hours. The obtained sample was dried at 110°C for 12 hours and then calcined at 550°C for 3 hours to obtain a hollow tubular HZSM-5 zeolite. The obtained sample was named Z5 100 (9)-HT.

[0049] (2) Synthesis of ZnZrOx solid solution

[0050] 1.2 g Zn(NO3)2·6H2O and 11.6 g Zr(NO3)4·5H2O were dissolved in a round-bottom flask filled with 200.0 mL deionized water. Then 200.0 mL precipitant containing 6.12 g (NH4)2CO3 was added to the previous solution using a separatory funnel at a rate of 3 mL / min. The mixture was stirred vigorously at 70 °C to form a precipitate. The mixture was stirred for 2 h, cooled to room temperature, washed with deionized water by centrifugation for 6 times, dried at 110 °C for 6 h, and calcined at 500 °C in a muffle furnace for 3 h to obtain ZnZrO x Solid solution, named ZZO.

[0051] (3) The hollow tubular HZSM-5 zeolite and ZnZrO x The metal oxides form a tandem catalyst.

[0052] Comparative Example 1

[0053] A method for preparing a catalyst for preparing p-xylene by hydrogenating CO2 comprises the following steps:

[0054] (1) Synthesis of flake HZSM-5:

[0055] First, 39.04 g of TPAOH was dissolved in 75.60 g of distilled water and reacted under magnetic stirring for 1-2 h. Then, 25.00 g of TEOS was added dropwise to the mixed solution and stirred at room temperature for about 12 h to replenish the volatile water. Then, 0.82 g of C9H 21 AlO3 and 0.16g NaOH, stirred for 12h, then added 9.36g urea (Urea). The molar composition of the above gel system is SiO2: Al2O3: TPAOH: Na2O: H2O: urea = 1: 1 / 60: 0.4: 1 / 60: 35: 1.5. The obtained gel was transferred to a stainless steel autoclave lined with polytetrafluoroethylene, crystallized at 170℃ in an oven for 24h, cooled to room temperature, centrifuged and washed with deionized water until neutral, and dried at 110℃ overnight. It was calcined at 550℃ in air for 6h to remove the organic template to obtain Na-type ZSM-5 (NaZSM-5), with a heating rate of 5℃ / min. Then it was ion exchanged twice at 80℃ with 1MNH4Cl solution (solid-liquid ratio of 1:30), each time for 3h, dried at 100℃ overnight, and calcined in a muffle furnace at 550℃ for 6h. Finally, the obtained sheet sample was recorded as Z5-S.

[0056] (2) The flaky Z5-S and ZnZrO x The metal oxides form a tandem catalyst.

[0057] Comparative Example 2

[0058] A method for preparing a catalyst for preparing p-xylene by hydrogenating CO2 comprises the following steps:

[0059] (1) Synthesis of chain HZSM-5

[0060] First, 39.04 g of TPAOH was added to 75.60 g of deionized water and stirred to mix evenly. Then, 25.00 g of TEOS was added dropwise to the mixture and stirred vigorously for 2 h. The obtained gel was transferred to a high-pressure closed reactor and crystallized in an oven at 100 ° C for 2 to 3 h. After cooling, 4.29 g of starch was added. After stirring for 12 h, 0.82 g of C9H 21AlO3 and 0.16gNaOH, after stirring overnight, the material molar composition of the gel system was SiO2:Al2O3:TPAOH:Na2O:H2O:starch=1:1 / 60:0.4:1 / 60:35:0.00072. The mixed solution was transferred to a high-pressure closed reactor lined with polytetrafluoroethylene and crystallized in an oven at 180℃ for 120h. Cooled to room temperature, then washed to neutrality, dried at 110℃ for 12h, and calcined at 550℃ for 6h to remove the organic template to obtain Na-type ZSM-5 (Na-ZSM-5). Finally, the obtained sample was ion exchanged with 1M NH4Cl aqueous solution, dried at 110℃ overnight, and calcined at 550℃ for 6h. Finally, the chain-like sample obtained was named Z5-C.

[0061] (2) The flaky Z5-C and ZnZrO x The metal oxides form a tandem catalyst.

[0062] Comparative Example 3

[0063] A method for preparing a catalyst for preparing p-xylene by hydrogenating CO2 comprises the following steps:

[0064] (1) Synthesis of hollow tubular HZSM-5

[0065] The raw material dosage ratio of the synthesis system is 30mol SiO2: 0.2mol TPAOH: 1.0molAl2O3: 18mL H2O. A certain amount of tetraethyl orthosilicate (TEOS) and tetrapropylammonium hydroxide (TPAOH) were mixed and stirred at room temperature for 6 hours to obtain a clear mixed liquid. Then it was treated in a rotary oven at 130℃ for 12 hours and a seed gel was obtained after cooling. Then sodium aluminate was added to the above 3.2g seed gel, and it was stirred at room temperature for 2 hours after ultrasonic treatment for a period of time. Then 18mL deionized water was added to the above seed gel and continued to stir for 30min. 1.0g quartz wool was impregnated with the diluted seed gel, and after standing for 60min, it was transferred to a 60℃ oven for drying for 12h. Finally, the dried quartz wool was placed on a raised polytetrafluoroethylene support frame in a polytetrafluoroethylene liner, and the support frame was placed in a stainless steel autoclave. 5.0mL deionized water was added to the bottom of the liner frame, and steam-assisted crystallization was carried out at a high temperature of 180℃ for 40h. After cooling to room temperature, the product was recovered and dried at 110°C for 12 hours. Finally, it was calcined at 550°C for 6 hours with a heating rate of 1°C / min. A hollow tubular sodium-type ZSM-5 zeolite was obtained. Then, ion exchange was performed with 1M NH4Cl solution (solid-liquid ratio of 1:30) at 90°C with stirring and reflux for 2.5 hours. The obtained sample was dried at 110°C for 12 hours and then calcined at 550°C for 3 hours to obtain a hollow tubular HZSM-5 zeolite. The obtained sample was named Z5 30(18)-HT.

[0066] (2) The hollow tubular HZSM-5 zeolite and ZnZrO x The metal oxides form a tandem catalyst.

[0067] Comparative Example 4

[0068] A method for preparing a catalyst for preparing p-xylene by hydrogenating CO2 comprises the following steps:

[0069] (1) Synthesis of hollow tubular HZSM-5

[0070] The raw material dosage ratio of the synthesis system is 60mol SiO2: 0.2mol TPAOH: 1.0molAl2O3: 18mL H2O. A certain amount of tetraethyl orthosilicate (TEOS) and tetrapropylammonium hydroxide (TPAOH) are mixed and stirred at room temperature for 6 hours to obtain a clear mixed liquid. Then it is treated in a rotary oven at 130℃ for 12 hours and a seed gel is obtained after cooling. Then sodium aluminate is added to the above 3.2g seed gel, and after ultrasonication for a period of time, it is stirred at room temperature for 2 hours. After that, 18mL deionized water is added to the above seed gel and continued to stir for 30min. 1.0g quartz wool is impregnated with the diluted seed gel, and after standing for 60min, it is transferred to a 60℃ oven for drying for 12h. Finally, the dried quartz wool is placed on a raised polytetrafluoroethylene support frame in a polytetrafluoroethylene liner, and the support frame is placed in a stainless steel autoclave. 5.0mL deionized water is added to the bottom of the liner frame, and steam-assisted crystallization is carried out at a high temperature of 180℃ for 40h. After cooling to room temperature, the product was recovered and dried at 110°C for 12 hours. Finally, it was calcined at 550°C for 6 hours with a heating rate of 1°C / min. A hollow tubular sodium-type ZSM-5 zeolite was obtained. Then, ion exchange was performed with 1M NH4Cl solution (solid-liquid ratio of 1:30) at 90°C with stirring and reflux for 2.5 hours. The obtained sample was dried at 110°C for 12 hours and then calcined at 550°C for 3 hours to obtain a hollow tubular HZSM-5 zeolite. The obtained sample was named Z5 60 (18)-HT.

[0071] (2) The hollow tubular HZSM-5 zeolite and ZnZrO x The metal oxides form a tandem catalyst.

[0072] Comparative Example 5

[0073] A method for preparing a catalyst for preparing p-xylene by hydrogenating CO2 comprises the following steps:

[0074] (1) Synthesis of hollow tubular HZSM-5

[0075] The raw material dosage ratio of the synthesis system is 100 mol SiO2: 0.2 mol TPAOH: 1.0 mol Al2O3: 27 mL H2O. A certain amount of tetraethyl orthosilicate (TEOS) and tetrapropylammonium hydroxide (TPAOH) were mixed and stirred at room temperature for 6 hours to obtain a clear mixed liquid. Then it was treated in a rotary oven at 130 ° C for 12 hours and a seed gel was obtained after cooling. Then sodium aluminate was added to the above 3.2 g seed gel, and after ultrasonic treatment for a period of time, it was stirred at room temperature for 2 hours. After that, 27 mL of deionized water was added to the above seed gel and continued to stir for 30 minutes. 1.0 g of quartz wool was impregnated with the diluted seed gel, and after standing for 60 minutes, it was transferred to a 60 ° C oven for drying for 12 hours. Finally, the dried quartz wool was placed on a raised polytetrafluoroethylene support frame in the polytetrafluoroethylene liner, and the support frame was placed in a stainless steel autoclave. 5.0 mL of deionized water was added to the bottom of the liner frame, and steam-assisted crystallization was carried out at a high temperature of 180 ° C for 40 hours. After cooling to room temperature, the product was recovered and dried at 110°C for 12 hours. Finally, it was calcined at 550°C for 6 hours with a heating rate of 1°C / min. A hollow tubular sodium-type ZSM-5 zeolite was obtained. Then, ion exchange was performed with 1M NH4Cl solution (solid-liquid ratio of 1:30) at 90°C with stirring and reflux for 2.5 hours. The obtained sample was dried at 110°C for 12 hours and then calcined at 550°C for 3 hours to obtain a hollow tubular HZSM-5 zeolite. The obtained sample was named Z5 100 (27)-HT.

[0076] (2) The hollow tubular HZSM-5 zeolite and ZnZrO x The metal oxides form a tandem catalyst.

[0077] Comparative Example 6

[0078] A method for preparing a catalyst for preparing p-xylene by hydrogenating CO2 comprises the following steps:

[0079] (1) Synthesis of hollow tubular HZSM-5

[0080] The raw material dosage ratio of the synthesis system is 100 mol SiO2: 0.2 mol TPAOH: 1.0 mol Al2O3. A certain amount of tetraethyl orthosilicate (TEOS) and tetrapropylammonium hydroxide (TPAOH) are mixed and stirred at room temperature for 6 hours to obtain a clear mixed liquid. Then it is treated in a rotary oven at 130°C for 12 hours and a seed gel is obtained after cooling. Then sodium aluminate is added to the above 3.2g seed gel, and after ultrasonication for a period of time, it is stirred at room temperature for 2 hours. After that, 1.0g quartz wool is impregnated with the seed gel, and after standing for 60 minutes, it is transferred to a 60°C oven for drying for 12 hours. Finally, the dried quartz wool is placed on a raised polytetrafluoroethylene support frame in a polytetrafluoroethylene liner, and the support frame is placed in a stainless steel autoclave. 5.0mL of deionized water is added to the bottom of the liner frame, and steam-assisted crystallization is carried out at a high temperature of 180°C for 40 hours. After cooling to room temperature, the product is recovered and dried at 110°C for 12 hours. Finally, the sample was calcined at 550°C for 6 hours with a heating rate of 1°C / min to obtain a hollow tubular sodium ZSM-5 zeolite. Then, 1M NH4Cl solution (solid-liquid ratio of 1:30) was stirred and refluxed at 90°C for 2.5 hours for ion exchange. The obtained sample was dried at 110°C for 12 hours and then calcined at 550°C for 3 hours to obtain a hollow tubular HZSM-5 zeolite. The obtained sample was named Z5 100 (0)-HT.

[0081] (2) The hollow tubular HZSM-5 zeolite and ZnZrO x The metal oxides form a tandem catalyst.

[0082] Results Analysis

[0083] 1. Catalyst characterization

[0084] X-ray diffraction testing can be used to characterize the crystal structure information in the sample. Figure 1(a) to (c) are XRD spectra of different samples. It can be seen that all Z5 zeolites have obvious characteristic diffraction peaks at 2θ = 7.9°, 8.8°, 23.3°, 23.9°, and 24.4°, which correspond to (101), (200), (051), (303), and (133) crystal planes respectively compared with standard card #44-0003, indicating that the prepared zeolite samples all present the typical MFI topological structure of ZSM-5 zeolite, and the relative crystallinity of different zeolites is different. It can be seen from the Z5-HT zeolites with different silicon-aluminum ratios that the Z5-HT zeolite with a high silicon-aluminum ratio (above 100) has a higher crystallinity, which is attributed to the increase in Al content in the zeolite framework, which leads to a decrease in crystal size. When the Al content is high, it tends to produce charged and repulsive gel subunits, inhibiting the phase change process of gel particles through charge matching with TPA+, resulting in small-sized crystals during secondary nucleation of zeolite, thereby reducing the crystallinity. In addition, the Al species in the zeolite framework is +3 valence. In order to ensure that the aluminum-oxygen tetrahedron is electrically neutral, cations or protons are required to stabilize the framework. Therefore, a high aluminum content will lead to unstable framework and affect crystallinity. As the silicon-aluminum ratio increases from 30 to 150, the characteristic diffraction peak intensity shows an obvious trend of first increasing and then slightly decreasing, especially at 7.9° and 8.8°. This corresponds to the same trend of the (101) and (200) crystal face crystal phase content with the increase of the silicon-aluminum ratio. It has been reported that the zigzag pores parallel to the a-axis (i.e., the pores perpendicular to the (101) and (200) crystal faces) are conducive to achieving molecular selectivity. In the reaction, only light hydrocarbons, benzene, toluene and PX are easy to diffuse through the zigzag pores, while OX, MX and heavier aromatics are difficult to diffuse out of the zigzag pores. Therefore, properly exposing the (101)(200) crystal face is conducive to improving the selectivity of the target product. At the same time, adjusting the amount of water added during the preparation of Z5-HT zeolite can also change the crystallinity of the crystal (e.g. Figure 1 As shown in (b)). When the amount of water increased from 0mL to 18mL, the intensity of the characteristic diffraction peak of Z5-HT zeolite gradually increased, indicating that increasing the amount of water within a certain range is beneficial to improving the crystallinity of Z5-HT zeolite. ZZO metal oxide was prepared by deposition precipitation method, with obvious characteristic diffraction peaks at 2θ=30.4°, 35.2°, 50.6°, and 60.2°, which are related to the (011), (110), (020), and (202) crystal planes. Compared with the t-ZrO2 standard card #50-1089, there is a tendency to shift to a higher angle at the peak position of 2θ=30.3°, corresponding to the shift of the (011) crystal plane. This is due to the Zn 2+ The ionic radius Less than Zr 4+ The ionic radius When Zn 2+When Zn is added to the ZrO2 lattice, the interplanar spacing will decrease. According to the Labbougue equation 2dsinθ=λ, as the interplanar spacing d decreases, the diffraction angle θ will increase. These results further prove that Zn enters the ZrO2 lattice matrix and forms a ZZO solid solution. Figure 1 c It can be seen that the ZZO / Z5-HT tandem catalyst prepared by physical mixing method retains the characteristic diffraction peaks of ZZO and Z5-HT respectively, and has no obvious influence on each other.

[0085] The acid properties of different catalysts were characterized by NH3-TPD. The desorption curves are shown in Figure 2 As shown in (a) to (b). The NH3-TPD spectrum was fitted into NH3 desorption peaks at three different temperature positions using the Gaussian fitting method, where the desorption peak near 180°C belongs to the weak acid site adsorption, the desorption peak near 250°C belongs to the medium-strong acid site adsorption, and the desorption peak near 350°C belongs to the strong acid site adsorption. By comparing Z5-HT zeolites with different silicon-aluminum ratios, it can be seen that with the increase of aluminum content in the zeolite, the peak areas of the desorption peaks of weak acid, medium-strong acid and strong acid of the zeolite sample all show an increasing trend, indicating that the aluminum content in the zeolite directly affects the acid density of the zeolite. Figure 2 It can be seen that the acid density of ZZO is very low, and its acid density is negligible compared with that of Z5-HT. After ZZO and Z5-HT are connected in series, the peak areas of medium-strong acid sites and strong acid sites are reduced, while the peak area of ​​weak acid sites increases accordingly.

[0086] In order to further understand the effect of silicon-aluminum ratio on the acid properties of Z5-HT zeolite, pyridine adsorption infrared test was carried out on Z5-HT zeolites with different silicon-aluminum ratios using pyridine as a probe molecule. Figure 2 As shown in (c) to (d), in the Py-IR spectrum at 1545 cm -1 and 1445cm -1 The absorption peaks near Chemical adsorption on acid sites and Lewis acid sites at 1490 cm -1 The absorption peak near is due to the interaction of pyridine with and Lewis acid sites. Acid sites refer to the tetracoordinated skeleton Al 3+ The Lewis acid site refers to the unsaturated Al on or outside the skeleton. 3+ Species, aluminum content directly affects and the number of Lewis acid sites. It can be seen that the external acid sites of Z5-HT zeolite are mainly Lewis acid. The acid content is low, and as the amount of aluminum added decreases, The amount of Lewis acid is reduced. This is related to the special preparation method of Z5-HT zeolite. The acid sites are concentrated inside the pipe, and a small amount of free Al 3+ The species form non-framework Al, thus forming Lewis acid sites. The outside of the pipe is mainly composed of high-silicon or full-silicon zeolite, which can also be seen in EDS. The acid site does not have the ability to aromatize, but can promote the hydrogenation of unsaturated hydrocarbons to form alkanes, which is not conducive to the selectivity of aromatics.

[0087] like Figure 3 (a) to (p) show SEM images of Z5-HT. It can be seen that all zeolites have a hollow tubular morphology, indicating that the steam-assisted crystallization method has successfully prepared Z5 zeolite with a special morphology. Z5-HT zeolite is specifically characterized by a sheet-like morphology of zeolites arranged perpendicular to the hollow tube along the c-axis, and the stacking between sheets is similar to a chain, indicating that this morphology Z5 may have the characteristics of both sheet-like and chain-like Z5. Figure 3 (a) to (e) examine the effect of the silicon-aluminum ratio on the morphology of Z5-HT zeolite. It can be seen that the morphology of Z5-HT zeolite with a low silicon-aluminum ratio is irregular, which may be related to the crystallinity of the zeolite, which is consistent with the trend of the change of crystallinity with the silicon-aluminum ratio in the XRD spectrum. In addition, smaller spherical Z5 is attached to the surface of the low silicon-aluminum ratio Z5-HT zeolite. As the silicon-aluminum ratio increases, the number of spherical Z5 gradually decreases, and the number of spherical Z5 is the least when the silicon-aluminum ratio is above 100. Z5-HT with a high silicon-aluminum ratio (above 100) has a higher tube formation rate. At the same time, the effect of the amount of water added during the preparation process on the morphology of the zeolite was investigated, such as Figure 3 As shown in (f) to (i). It can be seen that when no water is added during the preparation process, serious seed gel agglomeration occurs on the surface of the zeolite. This is attributed to the fact that the silica-alumina seed gel has not been diluted with water, the seed concentration in the mother liquor is high, and the alkalinity is high, so that the quartz wool is directly dissolved in the high temperature environment and the hollow tubular morphology cannot be formed. When the water volume is increased to 9 mL, the hollow tubular morphology is initially formed, but there are a large number of spherical Z5 on the surface of the zeolite, resulting in its unstable morphology. This is attributed to the fact that water molecules can affect the crystal morphology and structure of ZSM-5 zeolite. High H2O / Si ratios promote crystal growth and lead to the formation of larger crystals. Low H2O / Si ratios may tend to form small crystal structures. When the water volume is increased to more than 18 mL, a regular hollow tubular morphology appears, but when the water volume is increased to 27 mL, the zeolite morphology is unstable due to excessive crystal growth.

[0088] At the same time, HRTEM characterization analysis of Z5-HT was carried out, such as Figure 3As shown in (j) to (l) in the figure. It can be seen that the HRTEM spectrum mainly shows flake and spherical Z5. Considering that the actual crystals on Z5-HT are mainly flake Z5, the present invention mainly examines the lattice planes exposed by flake Z5. The results show that the lattice spacing of the crystals on Z5-HT is 1.0nm ( Figure 3 Middle (l)), assigned to the (200) crystal plane of Z5 crystal. Figure 3 (j) shows that the crystals on Z5-HT exhibit a (101) lattice plane, which is consistent with the characterization results of XRD.

[0089] Figure 3 (m) to (p) are SEM-EDS element mapping images of Z5-HT. It can be observed that Si and O elements are evenly distributed on the surface of Z5-HT zeolite, while Al element is almost not observed on the surface of zeolite, which further confirms that the surface of Z5-HT zeolite is composed of high-silicon or full-silicon zeolite. In addition, the formation mechanism of hollow tubular Z5-HT was explored, such as Figure 3 As shown in (a). It can be seen that the formation of hollow tubular Z5-HT requires three stages. The first stage is the growth stage of consuming seed gel. The second stage is the growth stage of consuming quartz wool. The third stage is the formation stage of hollow tubular. In the early stage of the reaction, the seed gel attached to the surface of quartz wool consumes its own silicon source and aluminum source for the first growth. At this time, the growth direction of Z5 zeolite is to grow around the surface of quartz wool, and quartz wool acts as a pore expansion template. When the seed gel consumes its own silicon source, the quartz wool used as a pore expansion template is dissolved as silicon source to join the second growth. At this time, the growth direction of Z5 zeolite is perpendicular to the pipe. When all aluminum sources are consumed, quartz wool is not completely dissolved, and it is the third growth with only silicon source. When quartz wool is completely consumed, Z5 zeolite stops growing and a complete hollow tubular morphology appears, and the tube diameter is the diameter of quartz wool. Since the aluminum source is consumed first and the outside of the tube is high-silicon or full-silicon zeolite, the aluminum source is mainly concentrated inside the tube, thus achieving the purpose of reasonable regulation of aluminum distribution, which is consistent with the Py-IR and EDS test results.

[0090] 2. Catalytic performance test

[0091] The reaction performance of Z5 and ZZO metal oxides with different morphologies in series for catalytic CO2 hydrogenation to aromatics is shown in Figure 2. Figure 4 The specific product distribution is shown in Table 1. Under the reaction conditions of 320 °C, 3.0 MPa, 3600 mL·g -1 ·h -1Under the reaction conditions of H2 / CO2=3 / 1, the CO2 conversion rates of hollow tube, sheet and chain Z5 were 15.9%, 16.2% and 12.6% respectively, the aromatic selectivity was 67.9%, 62.0% and 46.3% respectively, and the BTX selectivity was 57.2%, 48.7% and 26.7% respectively. This shows that Z5-HT has the characteristics of high aromatic and high BTX selectivity compared with the other two morphologies of Z5, especially the selectivity of xylene, which reaches 50.2%. In addition, Z5-S has a higher aromatic selectivity (62.0%), but the C9+ product selectivity is 13.3%. This is attributed to the shorter b-axis straight channel of Z5-S, which makes it easier for reactants to diffuse to the outer surface through the zeolite channel. The outer surface of Z5-S without special treatment has more acidic sites. When the reactants diffuse from the zeolite channel to the acidic sites on the outer surface, reactions such as methylation hydrogen transfer will occur, resulting in a higher selectivity for C9+ products. Due to its special growth mode from inside to outside perpendicular to the pipe, Z5-HT consumes all aluminum sources in the seed crystal in the early stage of growth. In the subsequent steam-assisted crystallization, quartz wool is consumed as a silicon source to continue to grow, so that most of the acid sites are concentrated inside the pipe, and the outside is high silicon or full silicon zeolite, so as to achieve the purpose of adjusting the acidity and prevent further hydrogenation of the product. In addition, the morphology of Z5-HT is that the sheet Z5 is stacked along the c-axis orientation of the vertical pipe (as can be seen by SEM). The stacked sheet Z5 is similar to the morphology of the chain Z5, achieving the purpose of appropriately extending the b-axis channel, which further confirms that the hollow tubular Z5 has the characteristics of high aromatics selectivity of sheet Z5 and high PX selectivity of chain Z5 (see xylene para-selective activity test).

[0092] Table 1 Product distribution

[0093]

[0094] Reaction conditions: 320℃, 3.0MPa, 3600mL·g -1 ·h -1 ,H2 / CO2=3 / 1,B a =benzene,T b =toluene,X c =xylene,Aro d =B+T+X+C 9+ .

[0095] The silicon-aluminum ratio directly affects the acidity of zeolite, thereby affecting the catalytic performance of CO2 hydrogenation to aromatics. Figure 4(b) shows the effect of the Si / Al ratio of Z5-HT on product distribution. The results show that with the increase of Si / Al ratio, the CO2 conversion rate and CO selectivity both decrease, and the selectivity of aromatics and BTX shows a trend of first increasing and then decreasing. When the Si / Al ratio is 100, the selectivity of aromatics and BTX reaches the maximum. It can be seen that the CO2 conversion rate on the Z5-HT zeolite with low silicon-aluminum ratio is high, but the selectivity of aromatics and BTX is low. The reason for this phenomenon may be that the acid density of Z5-HT with low silicon-aluminum ratio is strong and there are more acid sites, which accelerates the reaction rate, causes a large number of side reactions, accelerates the carbon deposition of the catalyst, and causes a decrease in catalytic activity. Excessive acid density will also promote the formation of C9+ products, resulting in no obvious advantage in BTX selectivity. Appropriate acid density and acid site distribution are key factors affecting the catalytic activity and selectivity of zeolite.

[0096] At the same time, the effect of water addition during the synthesis of Z5-HT on the catalytic performance of CO2 hydrogenation to aromatics was investigated. Figure 4 It can be seen from (c) that the amount of water used not only affects the catalytic performance of Z5, but also plays a role in regulating the morphology of Z5 (see SEM). When the amount of water used increases from 0mL to 27mL, the selectivity of aromatics and BTX selectivity tends to increase first and then decrease. Studies have shown that the H2O / Si ratio of zeolite affects the pore structure, pore size, acid properties and crystal size of Z5 zeolite. A higher H2O / Si ratio may promote crystal growth, forming larger crystal size and mesoporous structure, and a low ratio is more likely to produce a small crystal size (which can be confirmed by SEM characterization) and a microporous structure. These factors directly affect the specific surface area and pore volume of Z5 zeolite. In addition, a high H2O / Si ratio usually leads to the formation of more acidic sites. Because water molecules can react with silicon sources to form silicon-oxygen bonds, thereby introducing more acidic sites, the Z5-HT zeolite of the present invention has the best catalytic performance when the water consumption is 18mL.

[0097] In order to understand the PX selectivity of ZZO / Z5-HT in CO2 hydrogenation reaction, the present invention conducted a test on its p-xylene selectivity activity and compared it with ZZO / Z5-S and ZZO / Z5-C. The results are as follows Figure 5As shown in (a), the PX selectivity of ZZO / Z5-HT is as high as 76.2%, which is higher than that of ZZO / Z5-S and ZZO / Z5-C. The PX selectivity of ZZO / Z5-C is 46.7%, which is higher than that of ZZO / Z5-S. This is attributed to the appropriate extension of the length of the b-axis, which can expose more zigzag pore structures, which is beneficial to improve the selectivity of PX. And it can be seen that the OX selectivities of ZZO / Z5-S and ZZO / Z5-C are 56.3% and 50.6%, respectively, indicating that PX is isomerized to OX by the acid sites on the outer surfaces of Z5-S and Z5-C zeolites. The OX selectivity of ZZO / Z5-HT is 21.9%, which is attributed to the fewer acid sites on the outer surface of Z5-HT, which prevents PX from further reacting. The above results show that the prepared Z5-HT not only combines the advantages of flake and chain Z5 in morphology to achieve molecular selectivity, but also passivates the acid sites on the outer surface of the zeolite to prevent the isomerization of the target product. In addition, the stability of ZZO / Z5-HT in CO2 hydrogenation reaction was also evaluated. Figure 5 As shown in (b). Each product component has a large fluctuation in the initial stage of the reaction. After a period of reaction, it basically remains within a certain range. No obvious deactivation phenomenon was found in the 100h test. The CO2 conversion rate remained at about 15-16%, and the aromatics selectivity remained at about 65-70%, indicating that the ZZO / Z5-HT catalyst has good stability. This is consistent with our original intention of designing the ZZO / Z5-HT catalyst. It is well known that the main reason for catalyst deactivation is concentrated on the carbon deposition of the zeolite component, and Z5-HT has a rich pore structure, which can effectively help the carbon deposits diffuse and prevent accumulation in the pores, thereby affecting the reaction activity.

[0098] Z5 zeolite with hollow tube morphology was prepared by a reasonable method. The results show that when the Si / Al ratio is greater than 100 and the water dosage is 18 mL, the tube formation rate of Z5-HT is higher and the hollow tube morphology is regular. Z5-HT and ZZO form a tandem catalyst, and the activity of ZZO / Z5-HT tandem catalyst in CO2 hydrogenation reaction is investigated. -1 ·h -1 Under the reaction conditions of 1 / 4 zeolite and 1 / 2 zeolite, the selectivity of xylene to aromatics reached 71.3% and the selectivity to PX reached 76.2%, both higher than those of ZZO / Z5-S and ZZO / Z5-C catalysts. This is because Z5-HT combines the advantages of sheet zeolite and chain zeolite in morphology, that is, it has selectivity for molecules (PX). In addition, the special preparation method passivates the acid sites on the outer surface of the zeolite, preventing the isomerization of PX to OX and MX.

[0099] In summary, the present invention adopts reasonable means to prepare Z5 zeolite with hollow tubular morphology. The purpose of controlling the morphology is achieved by adjusting the silicon-aluminum ratio and water consumption of the zeolite. The results show that when the silicon-aluminum ratio is above 100 and the water consumption is 18mL, Z5-HT has a higher tube formation rate and a regular hollow tubular morphology. Z5-HT and ZZO are combined into a series catalyst, and the activity of the ZZO / Z5-HT series catalyst in the CO2 hydrogenation reaction is investigated. Under the reaction conditions of 320℃, 3.0MPa, 2400mL·g -1 ·h -1 , under H2 / CO2=3 / 1, the selectivity of aromatics reached 71.3%, and the para-selectivity of para-xylene reached 76.2%, which is higher than that of ZZO / Z5-S and ZZO / Z5-C catalysts. This is attributed to the fact that Z5-HT has the advantages of both flake and chain zeolites in morphology, that is, it has the selectivity for molecules (PX). And its special preparation method passivates the acid sites on the outer surface of the zeolite, preventing PX from isomerizing to OX and MX.

[0100] It should be noted that when the present invention involves a numerical range, it should be understood that the two endpoints of each numerical range and any value between the two endpoints can be selected. Since the steps and methods used are the same as those in the embodiments, in order to avoid redundancy, the present invention describes a preferred embodiment. Although the preferred embodiments of the present invention have been described, those skilled in the art may make additional changes and modifications to these embodiments once they know the basic creative concept. Therefore, the attached claims are intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of the present invention.

[0101] Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.

Claims

1. A method for preparing a catalyst for preparing p-xylene by hydrogenation of CO2, characterized in that: The following steps are involved: The seed gel is prepared by mixing tetraethyl orthosilicate and a template agent, tetrapropylammonium hydroxide; adding sodium aluminate to the seed gel, stirring and then adding water to dilute it, impregnating quartz wool with the diluted seed gel, and then drying the quartz wool impregnated with the seed gel; The dried quartz wool is subjected to steam-assisted crystallization, and then cooled, dried, and calcined to remove the template agent, thereby obtaining a hollow tubular sodium-type ZSM-5 zeolite; Adding NH4Cl solution to the hollow tubular sodium ZSM-5 zeolite for ion exchange, followed by drying and calcining to obtain a hollow tubular HZSM-5 zeolite; Hollow tubular HZSM-5 zeolite and metal oxide ZnZrO x The mixture is mixed to obtain a catalyst for preparing p-xylene by hydrogenating CO2.

2. The method for preparing a catalyst for preparing p-xylene by hydrogenation of CO2 according to claim 1, characterized in that: The molar ratio of ethyl orthosilicate to sodium aluminate is 100-150:

1.

3. The method for preparing a catalyst for preparing p-xylene by hydrogenation of CO2 according to claim 1, characterized in that: The molar ratio of ethyl orthosilicate to tetrapropylammonium hydroxide is 100-150:0.

2.

4. The method for preparing a catalyst for preparing p-xylene by hydrogenation of CO2 according to claim 1, characterized in that: The ratio of added water to ethyl orthosilicate is 18mL:100-150mol.

5. The method for preparing a catalyst for preparing p-xylene by hydrogenation of CO2 according to claim 1, characterized in that: Hollow Tubular HZSM-5 Zeolite and Metal Oxide ZnZrO x The mass ratio is 1~2:1~2.

6. The method for preparing a catalyst for preparing p-xylene by hydrogenation of CO2 according to claim 1, characterized in that: The steam-assisted crystallization temperature is 160-220°C, and the crystallization time is 30-50h.

7. A catalyst for preparing p-xylene by hydrogenation of CO2 obtained by the preparation method according to any one of claims 1 to 6.

8. The catalyst for preparing p-xylene by hydrogenation of CO2 according to claim 7, characterized in that: The catalyst is composed of hollow tubular HZSM-5 zeolite and ZnZrO x The hollow tubular HZSM-5 zeolite and the metal oxide ZnZrO x The mass ratio is 1~2:1~2.

9. Use of the catalyst according to claim 7 in the preparation of p-xylene by hydrogenation of CO2, characterized in that: The reaction conditions are as follows: the volume ratio of the raw gas H2 to CO2 is 3:1, the reaction temperature is 320°C, the reaction pressure is 3.0 MPa, and the reaction gas space velocity is 2400 mL·g -1 ·h -1 .