Manufacturing process of double-layer carbon source storage tank made of stainless steel reinforced glass fibers

Through the manufacturing process of stainless steel reinforced glass fiber double-layer carbon source storage tanks, combined with anti-corrosion leakage lining layer and structural reinforcement layer, the leakage and damage problems of traditional storage tanks under corrosive media and pressure are solved, and the further development of the new storage tanks is achieved. High corrosion resistance and mechanical strength extend the service life of the storage tank.

CN118991064APending Publication Date: 2024-11-22JIANGSU CHANGHONG GLASS FIBRE REINFORCED PLASTIC CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411128557.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Traditional metal storage tanks are prone to leakage and damage under the action of corrosive media. Single-layer glass fiber storage tanks are corrosion and aging when facing strong corrosive media and external forces, causing leakage and damage. The existing reinforcement reinforcement support effect is limited and easy to support. Leave.

Method used

The manufacturing process of double-layer carbon source storage tanks made of stainless steel reinforced glass fiber is used. The outer layer uses stainless steel to enhance mechanical strength and compressive resistance. The inner layer of fiberglass adopts corrosion-resistant leakage inner lining layer, structural reinforcement layer and corrosion-resistant outer surface layer, combined with Polyester films enhance sealing, forming a double-layer structure to resist corrosion and pressure.

Benefits of technology

Significantly improve the corrosion resistance, leakage and pressure bearing performance of the storage tank, extend its service life, and facilitate maintenance and maintenance through split installation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004997171700000081
    Figure BDA0004997171700000081
  • Figure BDA0004997171700000091
    Figure BDA0004997171700000091
Patent Text Reader

Abstract

The invention relates to the technical field of chemical storage tanks, and discloses a manufacturing process for a double-layer carbon source storage tank made of stainless steel reinforced glass fibers. A manufacturing process of a double-layer carbon source storage tank made of stainless steel reinforced glass fibers comprises the following specific steps that a polyester film is wound on the outer surface of inner-layer glass fiber reinforced plastic in advance, then the polyester film serves as a hoisting fulcrum, a stainless steel layer is hoisted on the outer surface of the inner-layer glass fiber reinforced plastic, and outer-layer stainless steel is formed; the polyester film is attached to the outer-layer stainless steel, the opening of the inner-layer glass fiber reinforced plastic is located in the outer-layer stainless steel, the opening of the inner-layer glass fiber reinforced plastic is aligned with the opening of the outer-layer stainless steel to form a cylinder, the cylinder is sealed through a sealing head to form a tank body, and manufacturing of the double-layer carbon source storage tank is completed. According to the double-layer carbon source storage tank, the outer layer is the stainless steel layer, the inner layer is the glass fiber reinforced plastic layer compounded by multiple structures, the overall bearing pressure and sealing performance of the storage tank are improved, and leakage of chemical media is prevented.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of chemical storage tanks, and in particular to a manufacturing process for a double-layer carbon source storage tank made of stainless steel reinforced glass fiber. Background Art

[0002] In the fields of chemical industry, environmental protection, etc., corrosive chemical liquids are often required to be stored. Traditional metal storage tanks are prone to leakage and damage under the action of corrosive media for a long time, while single fiberglass storage tanks are prone to leakage and damage due to corrosion and aging of materials when facing multiple challenges such as strong corrosive media, overall pressure and unexpected external force collision.

[0003] At present, the domestic industry adopts the method of setting reinforcing ribs inside the tank body, but usually metal or composite material reinforcing ribs are used for large-degree support, and the supporting effect is limited. In addition, due to the invasion of storage medium and rust, the internal supporting ribs are easy to fall off and lose their supporting strength, causing the tank body to leak and collapse. Summary of the invention

[0004] In order to improve the corrosion resistance and bearing pressure of existing storage tanks, the present application provides a manufacturing process for a double-layer carbon source storage tank made of stainless steel reinforced glass fiber.

[0005] The present application provides a manufacturing process for a stainless steel reinforced glass fiber double-layer carbon source storage tank, which adopts the following technical solution: A manufacturing process of a stainless steel reinforced glass fiber double-layer carbon source storage tank comprises the following specific steps: A layer of polyester film is pre-wound on the outer surface of the inner layer of FRP, and then the polyester film is used as a lifting fulcrum to hoist a layer of stainless steel on the outer surface of the inner layer of FRP to form an outer layer of stainless steel, the side of the polyester film away from the inner layer of FRP is in contact with the outer layer of stainless steel, the opening of the inner layer of FRP is aligned with the opening of the outer layer of stainless steel, the opening of the inner layer of FRP is located inside the outer layer of stainless steel to form a cylinder, and the cylinder is sealed with a head to form a tank body, thus completing the manufacture of the double-layer carbon source storage tank; the inner layer of FRP includes an anti-corrosion and leakage inner lining layer, a structural reinforcement layer and a corrosion-resistant outer layer, and the structural reinforcement layer is located between the anti-corrosion and leakage inner lining layer and the corrosion-resistant outer layer.

[0006] By adopting the above technical solution, the outer layer of the storage tank uses a stainless steel layer, which can enhance the mechanical strength and pressure resistance of the storage tank, withstand greater external pressure and internal medium pressure, improve the overall bearing pressure of the storage tank, and extend the service life of the storage tank. The inner fiberglass layer is composited with an anti-corrosion and leakage lining layer, a structural reinforcement layer, and a corrosion-resistant outer layer. The fiberglass layer made of multiple layers of anti-corrosion and permeable reinforcement materials has a strong tolerance to corrosive chemical media, effectively resists the erosion of corrosive media such as acids and alkalis, and improves the corrosion resistance and anti-leakage performance of the storage tank. By wrapping a layer of polyester film on the outer surface of the inner fiberglass layer and then compounding it with the outer stainless steel layer, the sealing of the storage tank can be enhanced to prevent the leakage of stored chemical media, while reducing the impact of the external environment on the internal medium of the storage tank and extending the service life of the storage tank.

[0007] Preferably, the outer layer of stainless steel is divided into an upper part and a lower part, and the upper and lower parts of the stainless steel are hoisted by a crane until the upper and lower parts of the stainless steel are in contact with the polyester film wrapped around the surface of the fiberglass, the opening of the inner layer of fiberglass is aligned with the opening of the outer layer of stainless steel, and then the upper and lower parts of the stainless steel are connected by welding to form a cylinder, and the cylinder is sealed with a head to form a tank body, thereby completing the manufacture of the double-layer carbon source storage tank.

[0008] By adopting the above technical solution, the outer stainless steel is divided into two parts, the upper and lower parts, which can be easily installed and disassembled, facilitate the maintenance and inspection of the storage tank, and reduce the difficulty of installation and maintenance caused by the large size of the storage tank.

[0009] Preferably, the anti-corrosion and leakage lining layer is formed by spraying and bonding glass fiber surface felt with inner lining layer adhesive, the structural reinforcement layer is formed by spraying and bonding alkali-free untwisted glass fiber roving with structural layer adhesive, and the corrosion-resistant outer surface layer is formed by spraying resin slurry.

[0010] By adopting the above technical solution, the anti-corrosion penetration lining layer is formed by spraying the glass fiber surface felt and the inner lining rubber. The glass fiber surface felt has good corrosion resistance, fit and sealing properties, and can be combined with the rubber to form a dense protective layer to resist the erosion of chemical media, prevent the leakage of chemical media, and improve the corrosion resistance, leakage resistance and pressure bearing capacity of the storage tank. At the same time, the glass fiber surface felt also has good thermal insulation performance, reduces the temperature change of the medium inside the storage tank, and improves the stability of the storage medium. The structural reinforcement layer is sprayed by alkali-free untwisted glass fiber roving and rubber. The alkali-free untwisted glass fiber roving has not been twisted, can maintain the original shape of the fiber, has high strength and rigidity, can act as the reinforcing material used for the barrel, improve the pressure bearing capacity and strength of the storage tank, and extend the service life of the storage tank.

[0011] Preferably, the anti-corrosion and leakage lining layer has a rubber content of ≥95%, and the structural reinforcement layer has a rubber content of ≥40%.

[0012] Preferably, the inner lining rubber material comprises the following raw materials in parts by weight: 90-110 parts of vinyl resin, 20-30 parts of corrosion-resistant resin, 1-3 parts of initiator, and 0.1-0.2 parts of accelerator; the corrosion-resistant resin is one of phenolic resin and bisphenol A epoxy resin.

[0013] By adopting the above technical scheme, phenolic resin, bisphenol A epoxy resin and vinyl resin are compounded as the base resin of the inner lining rubber material, which has good corrosion resistance and heat resistance, and also has high bonding strength, thereby improving the corrosion resistance and sealing performance of the inner layer of fiberglass and reducing erosion and leakage of chemical media.

[0014] Preferably, the bisphenol A epoxy resin is modified by nano-titanium and a coupling agent; the modification method comprises the following specific steps: pre-mixing the solvent with the bisphenol A epoxy resin, then adding nano-titanium and a coupling agent and stirring to obtain nano-titanium modified epoxy resin.

[0015] By adopting the above technical solution, nano-titanium and coupling agent are grafted to modify the epoxy resin, which can improve the thermal stability, tensile strength and compressive strength of the epoxy resin, make the inner layer of fiberglass more durable, improve the impact resistance and thermal stability of the storage tank, and reduce the temperature change of the medium inside the storage tank.

[0016] Preferably, the structural layer rubber material comprises the following raw materials in parts by weight: 90-110 parts of unsaturated polyester resin, 1-3 parts of initiator, and 0.1-0.2 parts of accelerator.

[0017] By adopting the above technical scheme, unsaturated polyester resin is more suitable for injection molding, has higher tensile and compressive strength, can improve the compressive strength of the inner layer of fiberglass, enhance the bearing capacity of the storage tank, reduce the damage caused by external impact on the storage tank, and extend the service life of the storage tank.

[0018] Preferably, the resin slurry comprises the following raw materials in parts by weight: 90-110 parts of unsaturated polyester resin, 20-30 parts of flame retardant resin, 1-3 parts of initiator, and 0.1-0.2 parts of accelerator; the flame retardant resin is a vinyl phosphorus-containing resin.

[0019] By adopting the above technical solution, by combining unsaturated resin with flame retardant resin, the inner layer of FRP can maintain high corrosion resistance and flame retardancy, which can delay the spread of fire and improve the fire resistance of the storage tank. The use of vinyl phosphorus-containing resin and unsaturated polyester resin can improve the flame retardancy of the inner layer of FRP, which can delay combustion when the storage tank encounters the source of goods and improve the fire resistance of the storage tank. The use of flame retardant resin can reduce the addition of a large amount of solid flame retardants, promote the outer layer of resin slurry to be firmly bonded to the surface of the structural reinforcement layer, improve the density of the inner layer of FRP, and reduce the leakage of chemical media.

[0020] Preferably, the preparation method of the vinyl phosphorus-containing resin comprises the following specific steps: mixing a solvent with a phosphorus-containing phenolic resin and triethylamine, then adding a methacrylic chloride solution, wherein the mass ratio of the phosphorus-containing phenolic resin, triethylamine and methacrylic chloride is (3-4):(1-1.5):1, mixing evenly to form a reaction mixture, heating the reaction mixture to 40-50°C under the protection of nitrogen for reaction, and then washing and drying to obtain the vinyl phosphorus-containing resin.

[0021] Preferably, the head material is formed by injection molding using alkali-free gingham cloth and unsaturated polyester resin.

[0022] By adopting the above technical solution, the alkali-free woven fabric has better acid resistance and can ensure the bearing capacity of accessories such as heads. The alkali-free woven fabric is combined with resin as a reinforcing material, so that the prepared heads have better corrosion resistance and strength.

[0023] In summary, this application has the following beneficial effects: 1. Since the present application adopts a combination of an outer layer of stainless steel and an inner layer of fiberglass to form a double-layer carbon source storage tank, the mechanical strength and compressive resistance of stainless steel are utilized on the outside to improve the overall bearing capacity of the storage tank, and the fiberglass layer formed by the anti-corrosion and leakage lining layer, the structural reinforcement layer and the corrosion-resistant outer layer is utilized on the inside to resist the erosion of corrosive media such as acids and alkalis, prevent the leakage of stored chemical media, and improve the corrosion resistance and anti-leakage performance of the storage tank.

[0024] 2. In the present application, the anti-corrosion and penetration lining layer is formed by spraying the glass fiber surface felt with the inner lining rubber, and the structural reinforcement layer is formed by spraying the alkali-free and untwisted glass fiber roving and the rubber. The glass fibers with different properties are combined with the resin rubbers with different properties. This can make the anti-corrosion and penetration lining layer have better sealing and corrosion resistance, and make the structural reinforcement layer have higher strength and rigidity, thereby improving the pressure bearing capacity, corrosion resistance and leakage prevention performance of the storage tank. DETAILED DESCRIPTION

[0025] The present application is further described in detail below with reference to the embodiments.

[0026] All raw materials in the examples are commercially available.

[0027] The initiator is methyl ethyl ketone peroxide.

[0028] The accelerator is cobalt octoate.

[0029] The unsaturated polyester resin is a conventional unsaturated polyester resin, and this embodiment uses 196# unsaturated polyester resin produced by Changzhou Tianma Co., Ltd.

[0030] The vinyl resin is a conventional vinyl resin, and this embodiment uses SW901# produced by Shanghai Shangwei Fine Chemical Co., Ltd.

[0031] The phenolic resin selected was 415 phenolic resin from Orilon Chemical Co., Ltd.

[0032] The glass fiber surface felt was purchased from Changzhou Tianma Group Co., Ltd. The model is 30g / m 2 Surface felt.

[0033] The alkali-free untwisted glass fiber roving was purchased from Zhejiang Jushi Group Co., Ltd. 2400TEX glass fiber roving.

[0034] The polyester film was purchased from Nanjing Hengli Packaging Company.

[0035] Preparation example of inner lining rubber compound Preparation Example 1 The rubber material of the inner lining layer includes the following raw materials in parts by weight: 100 kg of vinyl resin, 25 kg of corrosion-resistant resin, 2 kg of initiator, and 0.15 kg of accelerator. The corrosion-resistant resin is phenolic resin.

[0036] The preparation method of the inner lining rubber material comprises the following specific steps: The vinyl resin, the corrosion-resistant resin, the initiator and the accelerator are mixed and stirred evenly to prepare the inner lining rubber material.

[0037] Preparation Example 2 The difference between Preparation Example 2 and Preparation Example 1 is that the amount of vinyl resin used in the inner lining rubber raw material is 90 kg, the amount of corrosion-resistant resin used is 20 kg, the amount of initiator used is 1 kg, and the amount of accelerator used is 0.1 kg.

[0038] Preparation Example 3 The difference between Preparation Example 3 and Preparation Example 1 is that the amount of vinyl resin used in the inner lining rubber raw material is 110 kg, the amount of corrosion-resistant resin used is 30 kg, the amount of initiator used is 3 kg, and the amount of accelerator used is 0.2 kg.

[0039] Preparation Example 4 The difference between Preparation Example 4 and Preparation Example 1 is that the corrosion-resistant resin in the rubber material of the inner lining layer is bisphenol A type epoxy resin. The bisphenol A type epoxy resin is EP-1441-310.

[0040] Preparation Example 5 The difference between Preparation Example 5 and Preparation Example 4 is that the raw material of the inner lining rubber material, bisphenol A epoxy resin, is modified by nano-titanium and a coupling agent. The coupling agent is KH-570. The particle size of the nano-titanium powder is 1000 mesh.

[0041] The preparation method of the inner lining rubber material comprises the following specific steps: S1: Mix xylene and bisphenol A epoxy resin in advance, stir at a speed of 500r / min for 5 minutes, and then add coupling agent and nano-titanium. The mass ratio of xylene, bisphenol A epoxy resin, coupling agent and nano-titanium is 1:1:0.5:0.3. Stir at a speed of 500r / min for 10 minutes to obtain nano-titanium modified epoxy resin.

[0042] S2: Mix vinyl resin, nano-titanium modified epoxy resin, initiator and accelerator, stir evenly, and prepare inner lining rubber material.

[0043] Preparation example of structural layer rubber compound Preparation Example 6 The structural layer rubber material includes the following raw materials in parts by weight: 100 kg of unsaturated polyester resin, 2 kg of initiator, and 0.15 kg of accelerator.

[0044] The method for preparing the structural layer rubber material comprises the following specific steps: Mix the unsaturated polyester resin, initiator and accelerator, stir evenly to form a structural layer rubber compound.

[0045] Preparation Example 7 The difference between Preparation Example 7 and Preparation Example 6 is that the amount of unsaturated polyester resin used in the structural layer rubber material is 90 kg, the amount of initiator used is 1 kg, and the amount of accelerator used is 0.1 kg.

[0046] Preparation Example 8 The difference between Preparation Example 8 and Preparation Example 6 is that the amount of unsaturated polyester resin used in the structural layer rubber raw material is 110 kg, the amount of initiator used is 3 kg, and the amount of accelerator used is 0.2 kg.

[0047] Preparation example of structural layer rubber compound Preparation Example 9 The resin slurry includes the following raw materials in parts by weight: 100 kg of unsaturated polyester resin, 25 kg of flame retardant resin, 2 kg of initiator, and 0.15 kg of accelerator. The flame retardant resin is a vinyl phosphorus-containing resin.

[0048] The method for preparing the resin slurry comprises the following specific steps: S1: Mix methacryloyl chloride and anhydrous toluene to form a methacryloyl chloride solution, the mass ratio of methacryloyl chloride to anhydrous toluene is 1:0.3; mix anhydrous toluene, phosphorus-containing phenolic resin and triethylamine, the mass ratio of anhydrous toluene, phosphorus-containing phenolic resin and triethylamine is 3:1:0.3, and then add methacryloyl chloride solution dropwise under the protection of nitrogen, the mass ratio of phosphorus-containing phenolic resin and methacryloyl chloride is 3.5:1, heat to 45°C and react for 5h, wash after the reaction to remove toluene, and vacuum dry to obtain vinyl phosphorus-containing resin.

[0049] S2: Mix unsaturated polyester resin, vinyl phosphorus-containing resin, initiator and accelerator, stir evenly to form resin slurry.

[0050] Preparation Example 10 The difference between Preparation Example 10 and Preparation Example 9 is that the amount of unsaturated polyester resin used in the resin slurry raw material is 90 kg, the amount of flame retardant resin used is 20 kg, the amount of initiator used is 1 kg, and the amount of accelerator used is 0.1 kg.

[0051] Preparation Example 11 The difference between Preparation Example 11 and Preparation Example 9 is that the amount of unsaturated polyester resin used in the resin slurry raw material is 110 kg, the amount of flame retardant resin used is 30 kg, the amount of initiator used is 3 kg, and the amount of accelerator used is 0.2 kg.

[0052] Preparation Example 12 The difference between Preparation Example 12 and Preparation Example 9 is that an equal amount of flame retardant is used in the resin slurry raw material instead of the flame retardant resin, and the flame retardant is aluminum hydroxide. Example

[0053] Example 1 This embodiment provides a manufacturing process for a stainless steel reinforced glass fiber double-layer carbon source storage tank, comprising the following specific steps: S1: Lay the glass fiber surface felt flat, pressurize the inner lining rubber and spray it on both sides of the glass fiber surface felt through a spray gun, the inner lining rubber comes from Preparation Example 1, so that the glass fiber surface felt and the rubber are penetrated and bonded, and after heating and curing at 100°C, an anti-corrosion and leakage lining layer is formed, and the anti-corrosion and leakage lining layer content reaches 95%; pressurize the structural layer rubber and spray it on the surface of the alkali-free untwisted glass fiber roving through a spray gun, the structural layer rubber comes from Preparation Example 6, and after spraying, it is compounded with the anti-corrosion and leakage lining layer, and hot-pressed and cured at 120°C using a hot press to obtain a structural reinforcement layer; then pressurize the resin slurry and spray it on the surface of the structural reinforcement layer through a spray gun, the resin slurry comes from Preparation Example 9, let it stand for 20 minutes after spraying, and then hot-pressed and cured at 140°C to form a corrosion-resistant outer layer, that is, the inner layer of glass fiber reinforced plastic is obtained.

[0054] S2: Wrap a layer of polyester film on the outer surface of the inner layer of FRP, the flat thickness of the polyester film is 30μm, divide the outer stainless steel into upper and lower parts, and then use the polyester film as a lifting fulcrum to lift the upper and lower parts of the stainless steel onto the outer surface of the inner layer of FRP through a crane. The upper and lower parts of the stainless steel surround the outer surface of the inner layer of FRP and are connected by welding. The inner side of the stainless steel is bonded to the inner lining FRP through the polyester film to form an outer layer of stainless steel. Align the opening of the inner layer of FRP with the opening of the outer layer of stainless steel. The opening of the inner layer of FRP is located inside the outer layer of stainless steel to form a cylinder.

[0055] S3: After the resin slurry is pressurized, it is sprayed on the surface of the alkali-free woven fabric through a spray gun. The thickness of the alkali-free woven fabric is 0.24mm and 180g / m 2 The resin slurry comes from Preparation Example 9. After spraying, it is allowed to stand for 20 minutes and then hot-pressed and cured at 120°C to form a head. The cylinder is then sealed with the head to complete the manufacture of a stainless steel reinforced glass fiber double-layer carbon source storage tank.

[0056] Example 2 The difference between Example 2 and Example 1 is that in the manufacturing process of the stainless steel reinforced glass fiber double-layer carbon source storage tank, the inner lining rubber material in the inner layer of glass fiber reinforced plastic comes from Preparation Example 2.

[0057] Example 3 The difference between Example 3 and Example 1 is that in the manufacturing process of the stainless steel reinforced glass fiber double-layer carbon source storage tank, the inner lining rubber material in the inner layer of glass fiber reinforced plastic comes from Preparation Example 3.

[0058] Example 4 The difference between Example 4 and Example 1 is that in the manufacturing process of the stainless steel reinforced glass fiber double-layer carbon source storage tank, the structural layer rubber material in the inner layer of glass fiber reinforced plastic comes from Preparation Example 7.

[0059] Example 5 The difference between Example 5 and Example 1 is that in the manufacturing process of the stainless steel reinforced glass fiber double-layer carbon source storage tank, the structural layer rubber material in the inner layer of glass fiber reinforced plastic comes from Preparation Example 8.

[0060] Example 6 The difference between Example 6 and Example 1 is that in the manufacturing process of the stainless steel reinforced glass fiber double-layer carbon source storage tank, the resin slurry in the inner layer of glass fiber reinforced plastic comes from Preparation Example 10.

[0061] Example 7 The difference between Example 7 and Example 1 is that in the manufacturing process of the stainless steel reinforced glass fiber double-layer carbon source storage tank, the resin slurry in the inner layer of glass fiber reinforced plastic comes from Preparation Example 11.

[0062] Example 8 The difference between Example 8 and Example 1 is that in the manufacturing process of the stainless steel reinforced glass fiber double-layer carbon source storage tank, the inner lining rubber material in the inner layer of glass fiber reinforced plastic comes from Preparation Example 4.

[0063] Example 9 The difference between Example 9 and Example 1 is that in the manufacturing process of the stainless steel reinforced glass fiber double-layer carbon source storage tank, the inner lining rubber material in the inner layer of glass fiber reinforced plastic comes from Preparation Example 5.

[0064] Example 10 The difference between Example 10 and Example 1 is that in the manufacturing process of the stainless steel reinforced glass fiber double-layer carbon source storage tank, the resin slurry in the inner layer of glass fiber reinforced plastic comes from Preparation Example 12.

[0065] Comparative Example Comparative Example 1 The difference between Comparative Example 1 and Example 1 is that in the manufacturing process of the stainless steel reinforced glass fiber double-layer carbon source storage tank, no structural reinforcement layer is used in the inner layer of glass fiber reinforced plastic.

[0066] Comparative Example 2 The difference between Comparative Example 2 and Example 1 is that in the manufacturing process of the stainless steel reinforced glass fiber double-layer carbon source storage tank, no corrosion-resistant leakage lining layer is used in the inner layer of glass fiber reinforced plastics.

[0067] Performance testing According to the stainless steel reinforced glass fiber double-layer carbon source storage tank provided in Examples 1-10 and Comparative Examples 1-2 of the present application, the following performance tests were performed, and the specific test results are shown in Table 1.

[0068] Detection Methods 1. Leakage test The stainless steel reinforced glass fiber double-layer carbon source storage tank prepared in the present application was filled with clean water, and after 48 hours of hydrostatic pressure, the storage tank was observed for leakage.

[0069] 2. Strength test The tensile elastic modulus of the stainless steel reinforced glass fiber double-layer carbon source storage tank prepared by the present application was tested with reference to the standard of GB / T1447-2005 "Test Method for Tensile Properties of Fiber Reinforced Plastics". The tensile strength of the inner layer of glass fiber reinforced plastic prepared by the present application was tested with reference to the standard of GB / T5349-2005 "Test Method for Axial Tensile Properties of Fiber Reinforced Thermosetting Plastic Pipes", and the bending strength of the inner layer of glass fiber reinforced plastic prepared by the present application was tested with reference to the standard of DIN 53452 "Plastic Testing. Bending Test and Impact Test for Force Measurement Test".

[0070] 3. Corrosion resistance The inner layer of FRP prepared in the present application was immersed in a sodium acetate solution as a medium for 72 hours, and the corrosion resistance was tested. The front and rear inner layers of FRP were weighed and the corrosion rate was calculated.

[0071] It can be seen from the performance test results that the stainless steel reinforced glass fiber double-layer carbon source storage tank prepared in the present application has good anti-leakage and corrosion resistance, and at the same time has high mechanical strength, which enables the storage tank to have good bearing pressure and service life.

[0072] By comparing Examples 8-9 with Example 1, it can be seen that Example 8 uses bisphenol A epoxy resin, and Example 9 uses titanium powder to modify the epoxy resin. From the performance test results, it can be seen that the strength and corrosion resistance of the prepared inner layer of fiberglass are improved.

[0073] By comparing Example 10 with Example 1, it can be seen that Example 10 uses conventional flame retardants instead of the flame retardant resin prepared in the present application. From the performance test results, it can be seen that the leakage resistance, corrosion resistance and strength of the inner layer of glass fiber reinforced plastics prepared in the present application will decrease. It is further shown that using a resin with flame retardant properties instead of traditional flame retardants can improve the sealing of the inner layer of glass fiber reinforced plastics and reduce the leakage of chemical media.

[0074] By comparing Comparative Examples 1-2 with Example 1, it can be seen that Comparative Example 1 does not use a structural reinforcement layer, and Comparative Example 2 does not use an anti-corrosion and leakage lining layer. From the performance test results, it can be seen that by changing the structure of the inner layer of fiberglass reinforced plastics in the present application, the anti-leakage and corrosion resistance of the prepared storage tanks are significantly reduced, and leakage has occurred.

[0075] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A manufacturing process for a stainless steel reinforced glass fiber double-layer carbon source storage tank, It is characterized in that The specific steps include: A layer of polyester film is pre-wound on the outer surface of the inner layer of glass fiber reinforced plastics, and then a layer of stainless steel is hoisted on the outer surface of the inner layer of glass fiber reinforced plastics with the polyester film as a lifting fulcrum to form an outer layer of stainless steel, the side of the polyester film away from the inner layer of glass fiber reinforced plastics is in contact with the outer layer of stainless steel, the opening of the inner layer of glass fiber reinforced plastics is aligned with the opening of the outer layer of stainless steel, and the opening of the inner layer of glass fiber reinforced plastics is located inside the outer layer of stainless steel to form a cylinder, and the cylinder is sealed with a head to form a tank body, thus completing the manufacture of a double-layer carbon source storage tank; The inner layer of glass fiber reinforced plastics comprises an anti-corrosion and leakage inner lining layer, a structural reinforcement layer and a corrosion-resistant outer surface layer, wherein the structural reinforcement layer is located between the anti-corrosion and leakage inner lining layer and the corrosion-resistant outer surface layer.

2. The manufacturing process of the stainless steel reinforced glass fiber double-layer carbon source storage tank according to claim 1, It is characterized in that The outer stainless steel layer is divided into an upper part and a lower part. The upper and lower parts of the stainless steel are hoisted by a crane until the upper and lower parts of the stainless steel are both in contact with the polyester film wrapped around the surface of the fiberglass reinforced plastic. The opening of the inner fiberglass reinforced plastic is aligned with the opening of the outer stainless steel layer. The upper and lower parts of the stainless steel are then connected by welding to form a cylinder. The cylinder is sealed with a head to form a tank body, thereby completing the manufacture of the double-layer carbon source storage tank.

3. The manufacturing process of the stainless steel reinforced glass fiber double-layer carbon source storage tank according to claim 1, It is characterized in that The anti-corrosion and leakage lining layer is formed by spraying and bonding glass fiber surface felt with inner lining layer adhesive, the structural reinforcement layer is formed by spraying and bonding alkali-free untwisted glass fiber roving with structural layer adhesive, and the corrosion-resistant outer surface is formed by spraying resin slurry.

4. The manufacturing process of the stainless steel reinforced glass fiber double-layer carbon source storage tank according to claim 3, It is characterized in that The rubber content of the anti-corrosion and leakage lining layer is ≥95%, and the rubber content of the structural reinforcement layer is ≥40%.

5. The manufacturing process of the stainless steel reinforced glass fiber double-layer carbon source storage tank according to claim 3, It is characterized in that The inner lining rubber material comprises the following raw materials in parts by weight: 90-110 parts of vinyl resin, 20-30 parts of corrosion-resistant resin, 1-3 parts of initiator, and 0.1-0.2 parts of accelerator; the corrosion-resistant resin is one of phenolic resin and bisphenol A epoxy resin.

6. The manufacturing process of the stainless steel reinforced glass fiber double-layer carbon source storage tank according to claim 5, It is characterized in that The bisphenol A epoxy resin is modified by nano-titanium and a coupling agent; the modification method comprises the following specific steps: pre-mixing a solvent with the bisphenol A epoxy resin, then adding nano-titanium and a coupling agent and stirring to obtain nano-titanium modified epoxy resin.

7. The manufacturing process of the stainless steel reinforced glass fiber double-layer carbon source storage tank according to claim 3, It is characterized in that The structural layer rubber material comprises the following raw materials in parts by weight: 90-110 parts of unsaturated polyester resin, 1-3 parts of initiator, and 0.1-0.2 parts of accelerator.

8. The manufacturing process of the stainless steel reinforced glass fiber double-layer carbon source storage tank according to claim 3, It is characterized in that The resin slurry comprises the following raw materials in parts by weight: 90-110 parts of unsaturated polyester resin, 20-30 parts of flame retardant resin, 1-3 parts of initiator, and 0.1-0.2 parts of accelerator; the flame retardant resin is vinyl phosphorus-containing resin.

9. The manufacturing process of the stainless steel reinforced glass fiber double-layer carbon source storage tank according to claim 8, It is characterized in that The preparation method of the vinyl phosphorus-containing resin comprises the following specific steps: mixing a solvent with a phosphorus-containing phenolic resin and triethylamine, then adding a methacrylic chloride solution, wherein the mass ratio of the phosphorus-containing phenolic resin to the methacrylic chloride is (3-4):1, mixing evenly to form a reaction mixture, heating the reaction mixture to 40-50°C under the protection of nitrogen for reaction, and then washing and drying to obtain the vinyl phosphorus-containing resin.

10. The manufacturing process of the stainless steel reinforced glass fiber double-layer carbon source storage tank according to claim 8, It is characterized in that The head material is formed by spraying alkali-free gingham cloth and resin slurry.