Doped and coated sodium electric precursor material as well as preparation method and application thereof
By doping zinc and copper into the sodium-electric precursor material and covering zinc and copper on the surface, the cycle performance problems caused by structural defects of the positive electrode material of sodium ion battery are solved, and the energy density and cycle performance of the battery are improved.
Patent Information
- Application Number
- CN202411111918.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-11-22
AI Technical Summary
The structural defects of the transition metal layered oxide positive electrode materials of existing sodium ion batteries affect the cycling performance and limit the application of sodium ion batteries in the energy storage field.
Doply zinc and/or copper in the body phase of the sodium-electric precursor material, and synchronously coat the zinc and/or copper on the surface, and cooperate in coordination to form a doped coated material to improve crystal structure stability and average filling Discharge voltage.
The crystal structure stability and capacity of sodium electropositive electrode materials are enhanced, and the energy density and cycling performance of the battery are improved.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of sodium ion batteries and relates to a doped and coated sodium battery precursor material and a preparation method and application thereof. Background Art
[0002] With the continuous development of the economy and society, the depletion of non-renewable resources and the rapid deterioration of the ecological environment have become increasingly prominent. Although clean and renewable energy such as wind energy, hydropower, and solar energy can be substituted to a certain extent, their low utilization rate and unsuitability for recycling have limited their development and application. In recent years, with the continuous development of the new energy industry, chemical batteries represented by lithium batteries have become the focus of attention due to their advantages such as high voltage, high energy density, fast charging and discharging, and long cycle life. However, due to the extremely small reserves and uneven distribution of lithium resources, coupled with the unstable price of lithium resources, relatively cheap sodium-ion batteries are becoming more and more popular. Sodium elements are abundant in reserves and sources on the earth, and the price of raw materials is low and fluctuates little. Transition metal layered oxides NaxMO2 (0<x≤1, M is a transition metal element) are one of the most widely used sodium positive electrode materials. Although layered oxide materials are currently widely used in the actual production of sodium-ion batteries, the structural defects of layered oxide materials will have a greater impact on the cycle performance of sodium-ion batteries, which to a certain extent limits the application of sodium-ion batteries in the field of energy storage.
[0003] Therefore, how to improve the stability of the crystal structure of transition metal layered oxide positive electrode materials for sodium ion batteries and increase the capacity and average charge and discharge voltage is a technical problem that needs to be solved urgently. Summary of the invention
[0004] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a doped and coated sodium battery precursor material and a preparation method and application thereof. The present invention dopes zinc and / or copper inside the bulk phase of the sodium battery precursor material, and simultaneously coats zinc and / or copper on the surface, and the coating element is at least one of the doping elements. The synergistic cooperation can not only make the crystal structure of the obtained sodium battery positive electrode material more stable, but also indirectly provide capacity for the material, and at the same time improve the average charge and discharge voltage of the material, thereby improving the energy density and cycle performance of the battery.
[0005] To achieve this object, the present invention adopts the following technical solutions:
[0006] In a first aspect, the present invention provides a doped and coated sodium electricity precursor material, wherein the doped and coated sodium electricity precursor material comprises a sodium electricity precursor matrix material and a coating layer;
[0007] The sodium electrode precursor matrix material is doped with element A, and the coating layer is a coating material containing at least one element of element A; the element A includes Zn and / or Cu.
[0008] The sodium battery precursor material provided by the present invention is doped with zinc and / or copper in the bulk phase, and is simultaneously coated with zinc and / or copper on the surface, which cooperates with each other, and the coating element is at least one of the doping elements. This not only makes the crystal structure of the obtained sodium battery positive electrode material more stable, but also indirectly provides capacity for the material, and at the same time increases the average charge and discharge voltage of the material, thereby improving the energy density and cycle performance of the battery.
[0009] The following are preferred technical solutions of the present invention, but are not intended to limit the technical solutions provided by the present invention. Through the following preferred technical solutions, the technical objectives and beneficial effects of the present invention can be better achieved and realized.
[0010] Preferably, the sodium electrode precursor matrix material D50 is 3.0-5.0 μm, for example, 3.0 μm, 3.5 μm, 4.0 μm, 4.5 μm or 5.0 μm, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0011] Preferably, the thickness of the coating layer is 0.1-1.0 μm, for example, 0.1 μm, 0.2 μm, 0.3 μm, 0.4 μm, 0.5 μm, 0.6 μm, 0.7 μm, 0.8 μm, 0.9 μm or 1.0 μm, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0012] Preferably, the sodium electrode precursor matrix material has a general chemical formula of Ni x Mn z A y M k (OH)2, wherein M comprises a transition metal element, 0.1≤x≤0.5, 0.01≤y≤0.20, 0.1≤z≤0.5, 0.1≤k≤0.5.
[0013] For example, the x may be 0.1, 0.2, 0.3, 0.4 or 0.5, the y may be 0.01, 0.03, 0.05, 0.08, 0.1, 0.13, 0.15, 0.18 or 0.2, the z may be 0.1, 0.2, 0.3, 0.4 or 0.5, and the k may be 0.1, 0.2, 0.3, 0.4 or 0.5, but are not limited to the listed values, and other values not listed within the numerical range are equally applicable.
[0014] In the present invention, if the stoichiometric ratio of the doping element A in the sodium electrode precursor matrix material is too large, the capacity of the positive electrode material will be reduced, while if the stoichiometric ratio is too small, the cycle performance of the positive electrode material will be affected.
[0015] Preferably, the M comprises Co and / or Fe, preferably Fe.
[0016] Preferably, the mass of element A in the coating layer in the doped coated sodium electrode precursor material is 4-8%, for example 4%, 5%, 6%, 7% or 8%, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0017] In a second aspect, the present invention provides a method for preparing the doped coated sodium electrode precursor material as described in the first aspect, the preparation method comprising the following steps:
[0018] A mixed salt solution of a main metal element and a doping element A, a first precipitant solution and a first complexing agent solvent are subjected to a first coprecipitation reaction to obtain a sodium electrode precursor matrix material;
[0019] After the first coprecipitation reaction is completed, a coating agent solution containing at least one element of the A element, a second precipitant solution, and a second complexing agent solution are continuously added to carry out a second coprecipitation reaction to obtain the doped and coated sodium electrode precursor material;
[0020] The element A includes Zn and / or Cu.
[0021] It should be noted that, in the present invention, the concentration and type of the first precipitant solution and the second precipitant solution may be the same or different, and the concentration and type of the first complexing agent solution and the second complexing agent solution may be the same or different, that is, after the first coprecipitation reaction is completed, the feed rate of the first precipitant solution and the first complexing agent solution may be directly adjusted as the second precipitant solution and the second complexing agent solution, or a new precipitant solution and a new complexing agent solution may be prepared for the reaction, and those skilled in the art may adapt and select.
[0022] The preparation method provided by the present invention first prepares a sodium battery precursor matrix material doped with element A in the bulk phase, and then performs coating precipitation of element A on the surface of the sodium battery precursor matrix material; a sodium battery precursor material with a stable crystal structure is obtained through a simple co-precipitation reaction; the preparation method is simple to operate and is suitable for mass production.
[0023] Preferably, the main metal elements include Ni, Mn and M, and the M includes Co and / or Fe, preferably Fe.
[0024] Preferably, the concentration of the mixed salt solution of the main metal element and the doping element A is 1 to 5 mol / L, for example, 1 mol / L, 1.5 mol / L, 2 mol / L, 2.5 mol / L, 3 mol / L, 3.5 mol / L, 4 mol / L, 4.5 mol / L or 5 mol / L, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0025] Preferably, the concentration of the first precipitant solution is 2 to 15 mol / L, for example, 2 mol / L, 3 mol / L, 4 mol / L, 5 mol / L, 6 mol / L, 7 mol / L, 8 mol / L, 9 mol / L, 10 mol / L, 11 mol / L, 12 mol / L, 13 mol / L, 14 mol / L or 15 mol / L, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0026] Preferably, the concentration of the first complexing agent solution is 4-12 mol / L, for example 4 mol / L, 5 mol / L, 6 mol / L, 7 mol / L, 8 mol / L, 9 mol / L, 10 mol / L, 11 mol / L or 12 mol / L, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0027] Preferably, the feed rate of the mixed salt solution of the main metal element and the doping element A is 4 to 50 L / h, for example, 4 L / h, 5 L / h, 10 L / h, 15 L / h, 20 L / h, 25 L / h, 30 L / h, 35 L / h, 40 L / h, 45 L / h or 50 L / h, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0028] Preferably, the feed rate of the first precipitant solution is 1 to 10 L / h, for example, 1 L / h, 2 L / h, 3 L / h, 4 L / h, 5 L / h, 6 L / h, 7 L / h, 8 L / h, 9 L / h or 10 L / h, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0029] Preferably, the feed rate of the first complexing agent solution is 0.5-10 L / h, for example 0.5 L / h, 1 L / h, 2 L / h, 3 L / h, 4 L / h, 5 L / h, 6 L / h, 7 L / h, 8 L / h, 9 L / h or 10 L / h, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0030] Preferably, the pH value of the first coprecipitation reaction is 8 to 12, for example 8, 8.3, 8.5, 8.8, 9, 9.3, 9.5, 9.8, 10, 10.3, 10.5, 10.8, 11, 11.3, 11.5, 11.8 or 12, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0031] Preferably, the concentration of the coating agent solution containing element A is 0.5-1.5 mol / L, for example, 0.5 mol / L, 0.6 mol / L, 0.7 mol / L, 0.8 mol / L, 0.9 mol / L, 1 mol / L, 1.1 mol / L, 1.2 mol / L, 1.3 mol / L, 1.4 mol / L or 1.5 mol / L, etc., but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0032] Preferably, the concentration of the second precipitant solution is 2 to 15 mol / L, for example, 2 mol / L, 3 mol / L, 4 mol / L, 5 mol / L, 6 mol / L, 7 mol / L, 8 mol / L, 9 mol / L, 10 mol / L, 11 mol / L, 12 mol / L, 13 mol / L, 14 mol / L or 15 mol / L, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0033] Preferably, the concentration of the second complexing agent solution is 4-12 mol / L, for example 4 mol / L, 5 mol / L, 6 mol / L, 7 mol / L, 8 mol / L, 9 mol / L, 10 mol / L, 11 mol / L or 12 mol / L, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0034] Preferably, the feed rate of the coating agent solution containing element A is 0 to 10 L / h and does not include 0 L / h, for example, 0.1 L / h, 0.5 L / h, 1 L / h, 2 L / h, 3 L / h, 4 L / h, 5 L / h, 6 L / h, 7 L / h, 8 L / h, 9 L / h or 10 L / h, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0035] In the present invention, by regulating the concentration of the coating agent solution containing element A and the feeding rate, the uniformity of the coating layer thickness is stabilized; if the feeding rate is too fast, the coating layer cannot be evenly distributed, thereby affecting the capacity and stability of the positive electrode material.
[0036] Preferably, the feed rate of the second precipitant solution is 0.1-2 L / h, for example 0.1 L / h, 0.3 L / h, 0.5 L / h, 0.8 L / h, 1 L / h, 1.3 L / h, 1.5 L / h, 1.8 L / h or 2 L / h, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0037] Preferably, the feed rate of the second complexing agent solution is 0.05-1 L / h, for example 0.05 L / h, 0.1 L / h, 0.2 L / h, 0.3 L / h, 0.4 L / h, 0.5 L / h, 0.6 L / h, 0.7 L / h, 0.8 L / h, 0.9 L / h or 1 L / h, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0038] Preferably, the pH value of the second coprecipitation reaction is 8 to 12, for example 8, 8.3, 8.5, 8.8, 9, 9.3, 9.5, 9.8, 10, 10.3, 10.5, 10.8, 11, 11.3, 11.5, 11.8 or 12, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0039] The preparation method provided by the present invention obtains a sodium electrode precursor material with stable structure and excellent performance through the coordinated cooperation of multiple preparation parameters.
[0040] As a preferred technical solution, the preparation method comprises the following steps:
[0041] A mixed salt solution of the main metal element and the doping element A is fed at a rate of 4 to 50 L / h, a first precipitant solution is fed at a rate of 1 to 10 L / h, and a first complexing agent solvent is fed at a rate of 0.5 to 10 L / h for a first coprecipitation reaction, wherein the pH value during the first coprecipitation reaction is 8 to 12, to obtain a sodium electrode precursor matrix material;
[0042] After the first coprecipitation reaction is completed, a coating agent solution containing at least one element of the A element at a feeding rate of 0 to 10 L / h and excluding 0 L / h, a second precipitant solution at a feeding rate of 0.1 to 2 L / h, and a second complexing agent solution at a feeding rate of 0.05 to 1 L / h are continuously added to carry out a second coprecipitation reaction, during which the pH value is 8 to 12 to obtain the doped and coated sodium electric precursor material;
[0043] The element A includes Zn and / or Cu.
[0044] It should also be noted that, except for the characteristic limitations provided above, the rest of the preparation process, material type selection and parameters are all conventional technical selections;
[0045] Specifically:
[0046] The first precipitant and the second precipitant include but are not limited to liquid alkali; the first complexing agent and the second complexing agent include but are not limited to ammonia water; the types of substances that can be used as precipitants and complexing agents are all applicable to the present invention;
[0047] The first coprecipitation reaction and the second coprecipitation reaction can be carried out in a base liquid, the base liquid can be pure water, or a mixed solution of pure water and a complexing agent, and the concentration of the complexing agent in the base liquid is 0-2 mol / L;
[0048] The reaction temperature of the first coprecipitation reaction and the second coprecipitation reaction are independently 30 to 90° C., the stirring speed is independently 150 to 400 rpm, and the stirring time can be adaptively adjusted according to the particle size and the thickness of the coating layer.
[0049] In a second aspect, the present invention provides a doped coated sodium battery positive electrode material, wherein the doped coated sodium battery positive electrode material is obtained by mixing and sintering the doped coated sodium battery precursor material as described in the first aspect with a sodium source.
[0050] Preferably, the ratio of the total molar amount of metal elements in the doped and coated sodium electric precursor material to the molar amount of sodium in the sodium source is 1:(0.9-1.2), for example 1:0.9, 1:1, 1:1.1 or 1:1.2, etc., but is not limited to the listed values, and other unlisted values within this numerical range are also applicable.
[0051] Preferably, the sintering atmosphere is an oxygen-containing atmosphere.
[0052] Preferably, during the sintering process, the flow rate of the oxygen-containing gas is 3 to 8 L / min, for example, 3 L / min, 4 L / min, 5 L / min, 6 L / min, 7 L / min or 8 L / min, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0053] Preferably, the sintering temperature is 700-1300°C, for example 700°C, 750°C, 800°C, 850°C, 900°C, 950°C, 1000°C, 1050°C, 1100°C, 1200°C, 1250°C or 1300°C, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0054] Preferably, the sintering time is 8 to 20 hours, for example 8 hours, 9 hours, 10 hours, 11 hours, 12 hours, 13 hours, 14 hours, 15 hours, 16 hours, 17 hours, 18 hours, 19 hours or 20 hours, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0055] In a fourth aspect, the present invention further provides a sodium ion battery, comprising the doped and coated sodium positive electrode material as described in the third aspect.
[0056] Compared with the prior art, the present invention has the following beneficial effects:
[0057] The sodium battery precursor material provided by the present invention is doped with zinc and / or copper in the bulk phase, and is simultaneously coated with zinc and / or copper on the surface, which cooperates with each other, and the coating element is at least one of the doping elements. This not only makes the crystal structure of the obtained sodium battery positive electrode material more stable, but also indirectly provides capacity for the material, and at the same time increases the average charge and discharge voltage of the material, thereby improving the energy density and cycle performance of the battery. DETAILED DESCRIPTION
[0058] The technical scheme of the present invention is further illustrated by specific examples below. Those skilled in the art should understand that the examples are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0059] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by technicians in the technical field to which this application belongs; the terms used herein are only for the purpose of describing specific embodiments and are not intended to limit this application; the terms "including" and "having" and any variations thereof in this application are intended to cover non-exclusive inclusions.
[0060] In the description of this application, technical terms such as "first" and "second" are only used to distinguish different objects and cannot be understood as indicating or implying relative importance or implicitly indicating the quantity, specific order or primary and secondary relationship of the indicated technical features.
[0061] Example 1
[0062] This embodiment provides a sodium electric precursor material that is simultaneously zinc-doped and zinc-coated. The zinc-doped and zinc-coated sodium electric precursor material comprises a sodium electric precursor base material (D50 is 3.5 μm) and a coating layer (thickness is 0.5 μm); the chemical formula of the sodium electric precursor base material is Ni 0.35 Fe 0.30 Mn 0.30 Zn 0.05 (OH)2, and the coating layer is Zn(OH)2.
[0063] The preparation method of the sodium electric precursor material is as follows:
[0064] (1) Mix manganese sulfate, nickel sulfate, ferrous sulfate solution and zinc sulfate solution to obtain a mixed metal salt solution with a total metal ion concentration of 2 mol / L and a molar ratio of nickel, iron, manganese and zinc of 0.35:0.30:0.30:0.05; feed the mixed metal salt solution at a feed rate of 10 L / h, and add 10 mol / L sodium hydroxide solution and 5 mol / L ammonia solution to the bottom liquid in parallel to perform a first coprecipitation reaction. By fine-tuning the feed flow rate of the sodium hydroxide solution and the ammonia solution, the pH value of the system is controlled to be maintained at 9.8 during the first coprecipitation reaction, and the stirring speed is 400 r / min, to obtain a sodium electric precursor matrix material with a D50 of 3.5 μm;
[0065] (2) Then stop adding the nickel-iron-manganese-zinc mixed salt solution, and add 1 mol / L zinc sulfate solution, 10 mol / L sodium hydroxide solution and 5 mol / L ammonia water to the bottom liquid in parallel to carry out a second coprecipitation reaction. By fine-tuning the feed flow rate of the sodium hydroxide solution and the ammonia solution, the pH value of the system is controlled to be maintained at 10 and the stirring speed is 300 r / min during the second coprecipitation reaction, and a sodium electric precursor matrix material with a coating layer thickness of 0.2 μm is obtained; stop the reaction, and after the reaction is completed, centrifuge and wash, and dry at 150° C., so as to obtain the sodium electric precursor material that is simultaneously zinc-doped and zinc-coated.
[0066] Example 2
[0067] This embodiment provides a sodium electric precursor material that is simultaneously zinc-doped and zinc-coated. The zinc-doped and zinc-coated sodium electric precursor material comprises a sodium electric precursor base material (D50 is 3 μm) and a coating layer (thickness is 0.1 μm); the chemical formula of the sodium electric precursor base material is Ni 0.35 Fe 0.30 Mn 0.15 Zn 0.2 (OH)2, and the coating layer is Zn(OH)2.
[0068] The preparation method of the sodium electric precursor material is as follows:
[0069] (1) Mix manganese sulfate, nickel sulfate, ferrous sulfate solution and zinc sulfate solution to obtain a mixed metal salt solution with a total metal ion concentration of 2 mol / L and a molar ratio of nickel, iron, manganese and zinc of 0.35:0.30:0.15:0.2; feed the mixed metal salt solution at a feed rate of 20 L / h, and add 10 mol / L sodium hydroxide solution and 5 mol / L ammonia solution to the bottom liquid in parallel to perform a first coprecipitation reaction. By fine-tuning the feed flow rate of sodium hydroxide solution and ammonia solution, the system pH value is controlled to be maintained at 10.5 during the first coprecipitation reaction, and the stirring speed is 350 r / min, to obtain a sodium electric precursor matrix material with a D50 of 3.0 μm;
[0070] (2) Then stop adding the nickel-iron-manganese-zinc mixed salt solution, and add 1 mol / L zinc sulfate solution, 10 mol / L sodium hydroxide solution and 5 mol / L ammonia water to the bottom liquid in parallel to carry out a second coprecipitation reaction. By fine-tuning the feed flow rate of the sodium hydroxide solution and the ammonia solution, the pH value of the system is controlled to be maintained at 9.5 and the stirring speed is 350 r / min during the second coprecipitation reaction, and a sodium electric precursor matrix material with a coating layer thickness of 0.1 μm is obtained; stop the reaction, and after the reaction is completed, centrifuge and wash, and dry at 150° C., so as to obtain the sodium electric precursor material that is simultaneously zinc-doped and zinc-coated.
[0071] Example 3
[0072] This embodiment provides a sodium battery precursor material that is simultaneously zinc-doped and zinc-coated. The zinc-doped and zinc-coated sodium battery precursor material comprises a sodium battery precursor base material (D50 is 5 μm) and a coating layer (thickness is 1 μm); the chemical formula of the sodium battery precursor base material is Ni 0.35 Fe 0.30 Mn 0.34 Zn 0.01 (OH)2, and the coating layer is Zn(OH)2.
[0073] The preparation method of the sodium electric precursor material is as follows:
[0074] (1) Mix manganese sulfate, nickel sulfate, ferrous sulfate solution and zinc sulfate solution to obtain a mixed metal salt solution with a total metal ion concentration of 3 mol / L and a molar ratio of nickel, iron, manganese and zinc of 0.35:0.30:0.34:0.01; feed the mixed metal salt solution at a feed rate of 10 L / h, and add 8 mol / L sodium hydroxide solution and 4 mol / L ammonia solution to the bottom liquid in parallel to perform a first coprecipitation reaction. By fine-tuning the feed flow rate of sodium hydroxide solution and ammonia solution, the system pH value is controlled to be maintained at 11.2 during the first coprecipitation reaction, and the stirring speed is 350 r / min, to obtain a sodium electric precursor matrix material with a D50 of 5 μm;
[0075] (2) Then stop adding the nickel-iron-manganese-zinc mixed salt solution, and add 1 mol / L zinc sulfate solution, 8 mol / L sodium hydroxide solution and 4 mol / L ammonia water to the bottom liquid in parallel to carry out a second coprecipitation reaction. By fine-tuning the feed flow rate of the sodium hydroxide solution and the ammonia solution, the pH value of the system is controlled to be maintained at 11.3 and the stirring speed is 320 r / min during the second coprecipitation reaction, and a sodium electric precursor matrix material with a coating layer thickness of 1 μm is obtained; stop the reaction, and after the reaction is completed, centrifuge and wash, and dry at 150° C., so as to obtain the sodium electric precursor material that is simultaneously zinc-doped and zinc-coated.
[0076] Example 4
[0077] The difference between this embodiment and embodiment 1 is that the sodium electrode precursor material in this embodiment is copper-doped and copper-coated.
[0078] In the preparation method, zinc sulfate is replaced by copper sulfate.
[0079] The rest of the preparation methods and parameters were the same as those in Example 1.
[0080] Example 5
[0081] This embodiment provides a copper-zinc doped and zinc-coated sodium-electric precursor material, wherein the sodium-electric precursor material comprises a sodium-electric precursor base material and a coating layer; the chemical formula of the sodium-electric precursor base material is Ni 0.35 Fe 0.30 Mn 0.30 Zn 0.02 Cu 0.03 (OH)2, the coating layer is Zn(OH)2;
[0082] In the preparation method, the molar ratio of nickel, iron, manganese, zinc and copper in the mixed metal salt solution of step (1) is 0.35:0.30:0.30:0.02:0.03.
[0083] The rest of the preparation methods and parameters were the same as those in Example 1.
[0084] Example 6
[0085] This embodiment provides a copper-zinc doped and zinc-coated sodium-electric precursor material, wherein the sodium-electric precursor material comprises a sodium-electric precursor base material and a coating layer; the chemical formula of the sodium-electric precursor base material is Ni 0.35 Fe 0.30 Mn 0.30 Zn 0.03 Cu 0.02 (OH)2, the coating layer is Zn(OH)2;
[0086] In the preparation method, in the mixed salt solution of step (1), the molar ratio of nickel, iron, manganese, zinc and copper is 0.35:0.30:0.30:0.03:0.02.
[0087] The rest of the preparation methods and parameters were the same as those in Example 1.
[0088] Example 7
[0089] The difference between this embodiment and embodiment 1 is that the chemical formula of the sodium electrode precursor matrix material in this embodiment is Ni 0.35 Fe 0.30 Mn 0.345 Zn 0.005 (OH)2;
[0090] In the preparation method, the molar ratio of nickel, iron, manganese and zinc is adaptively adjusted.
[0091] The rest of the preparation methods and parameters were the same as those in Example 1.
[0092] Example 8
[0093] The difference between this embodiment and embodiment 1 is that the chemical formula of the sodium electrode precursor matrix material in this embodiment is Ni 0.35 Fe 0.30 Mn 0.1 Zn 0.25 (OH)2;
[0094] In the preparation method, the molar ratio of nickel, iron, manganese and zinc is adaptively adjusted.
[0095] The rest of the preparation methods and parameters were the same as those in Example 1.
[0096] Example 9
[0097] The difference between this embodiment and embodiment 1 is that the thickness of the coating layer in this embodiment is 0.05 μm;
[0098] In the preparation method, the reaction is stopped after the thickness of the coating layer is adjusted to 0.05 μm in step (2).
[0099] The rest of the preparation methods and parameters were the same as those in Example 1.
[0100] Example 10
[0101] The difference between this embodiment and embodiment 1 is that the thickness of the coating layer in this embodiment is 1.1 μm;
[0102] In the preparation method, the reaction is stopped after the thickness of the coating layer is adjusted to 1.1 μm in step (2).
[0103] The rest of the preparation methods and parameters were the same as those in Example 1.
[0104] Comparative Example 1
[0105] The difference between this comparative example and Example 1 is that the sodium electrode precursor material in this comparative example does not contain a coating layer;
[0106] In the preparation method, the coating process of step (2) is not carried out, and the reaction in step (1) is stopped after the particle size D50 reaches 3.5 μm. After the reaction is completed, the mixture is centrifuged and washed, and dried at 150° C. to obtain the sodium electrode precursor material.
[0107] The rest of the preparation methods and parameters were the same as those in Example 1.
[0108] Comparative Example 2
[0109] The difference between this comparative example and Example 1 is that the sodium electricity precursor matrix material in the sodium electricity precursor material in this comparative example is not doped with zinc.
[0110] In the preparation method, the mixed salt solution in step (1) does not contain zinc, wherein the molar ratio of nickel, iron and manganese in the mixed metal ion solution used in step (1) is 0.35:0.30:0.35.
[0111] The rest of the preparation methods and parameters were the same as those in Example 1.
[0112] Comparative Example 3
[0113] The difference between this comparative example and Example 1 is that neither zinc doping nor zinc coating is performed in this comparative example.
[0114] In the preparation method, the mixed salt solution in step (1) does not contain zinc, wherein the molar ratio of nickel, iron and manganese in the mixed metal ion solution used in step (1) is 0.35:0.30:0.35; the reaction is carried out until the average particle size is 3.5 μm, and the coating process (second coprecipitation reaction process) of step (2) is not carried out. After the first coprecipitation reaction is completed, centrifugal washing is performed and drying is performed at 150° C. to obtain the sodium electric precursor material.
[0115] The rest of the preparation methods and parameters were the same as those in Example 1.
[0116] The sodium battery precursor materials provided in Examples 1-10 and Comparative Examples 1-3 were uniformly mixed with sodium carbonate at a molar ratio of 1:1.06, calcined at 1100° C. for 10 hours in an air atmosphere, and then ground and sieved to obtain a sodium battery positive electrode material.
[0117] The prepared positive electrode material, acetylene black and polyvinylidene fluoride are mixed in a mass ratio of 8:1:1, added to N-methyl-2-pyrrolidone to obtain a positive electrode slurry, and the positive electrode slurry is evenly spread on an aluminum foil, dried and punched into a thin sheet to obtain a positive electrode plate; the positive electrode plate, a single sodium plate, a glass fiber separator, an electrolyte (the sodium salt is NaClO4), a gasket, a shrapnel and a battery shell are assembled into a button battery in an Ar gas glove box.
[0118] The sodium ion batteries provided in Examples 1-10 and Comparative Examples 1-3 were subjected to performance tests. The test conditions were as follows: electrochemical performance tests were performed in a voltage range of 1.5-4.1 V and a discharge current density of 20 mA / g. The test results of the capacity retention rate after 4000 cycles are shown in Table 1.
[0119] Table 1
[0120] Capacity retention after 4000 cycles (%) Example 1 86.6 Example 2 87.5 Example 3 86.1 Example 4 85.9 Example 5 86.4 Example 6 87.2 Example 7 79.7 Example 8 78.8 Example 9 81.1 Example 10 80.5 Comparative Example 1 72.5 Comparative Example 2 73.7 Comparative Example 3 69.4
[0121] From Table 1, we can get:
[0122] From the data results of Examples 1-6, it can be seen that the sodium battery precursor material provided by the present invention is doped with zinc and / or copper in the bulk phase, and is simultaneously coated on the surface with a coating material having at least one element identical to the doping element, which synergistically greatly improves the cycle performance of the sodium battery positive electrode material.
[0123] It can be seen from the data results of Example 1 and Examples 7 and 8 that too much or too little doping of element A will affect the improvement of the cycle performance of the positive electrode material.
[0124] It can be seen from the data results of Example 1 and Examples 9 and 10 that if the thickness of the coating layer is too thin or too thick, it will affect the improvement of the cycle performance of the positive electrode material.
[0125] From the data results of Example 1 and Comparative Examples 1-3, it can be seen that in the sodium-electric precursor material provided by the present invention, zinc and / or copper must be doped inside the bulk phase, and zinc and / or copper must be coated on the surface simultaneously, and they must cooperate synergistically, and at least one of the doping and coating elements must be consistent, so that the cycle performance of the positive electrode material can be significantly improved. In summary, the bulk phase of the sodium-electric precursor material provided by the present invention is doped with zinc and / or copper, and zinc and / or copper are simultaneously coated on the surface, and they cooperate synergistically, and the coating element is at least one of the doping elements, which can not only make the crystal structure of the obtained sodium-electric positive electrode material more stable, but also indirectly provide capacity for the material, and at the same time increase the average charge and discharge voltage of the material, thereby improving the energy density and cycle performance of the battery.
[0126] The specific embodiments described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A doped and coated sodium electrode precursor material, characterized in that: The doped and coated sodium electricity precursor material comprises a sodium electricity precursor matrix material and a coating layer; The sodium electrode precursor matrix material is doped with element A, and the coating layer is a coating material containing at least one element of element A; the element A includes Zn and / or Cu.
2. The doped and coated sodium electrode precursor material according to claim 1, characterized in that: The sodium electrode precursor matrix material D50 is 3.0 to 5.0 μm; Preferably, the coating layer has a thickness of 0.1 to 1.0 μm.
3. The doped and coated sodium electrode precursor material according to claim 1 or 2, characterized in that: The chemical formula of the sodium battery precursor matrix material is Ni x Mn z A y M k (OH)2, wherein M comprises a transition metal element, 0.1≤x≤0.5, 0.01≤y≤0.20, 0.1≤z≤0.5, 0.1≤k≤0.5; Preferably, the M comprises Co and / or Fe, preferably Fe; Preferably, the mass of the element A in the coating layer in the doped and coated sodium electrode precursor material is 4-8%.
4. A method for preparing a doped and coated sodium electrode precursor material according to any one of claims 1 to 3, characterized in that: The preparation method comprises the following steps: A mixed salt solution of a main metal element and a doping element A, a first precipitant solution and a first complexing agent solvent are subjected to a first coprecipitation reaction to obtain a sodium electrode precursor matrix material; After the first coprecipitation reaction is completed, a coating agent solution containing at least one element of the A element, a second precipitant solution, and a second complexing agent solution are continuously added to carry out a second coprecipitation reaction to obtain the doped and coated sodium electrode precursor material; The element A includes Zn and / or Cu.
5. The preparation method according to claim 4, characterized in that: The main metal elements include Ni, Mn and M, and the M includes Co and / or Fe, preferably Fe; Preferably, the concentration of the mixed salt solution of the main metal element and the doping element A is 1 to 5 mol / L; Preferably, the concentration of the first precipitant solution is 2 to 15 mol / L; Preferably, the concentration of the first complexing agent solution is 4 to 12 mol / L; Preferably, the feed rate of the mixed salt solution of the main metal element and the doping element A is 4 to 50 L / h; Preferably, the feed rate of the first precipitant solution is 1 to 10 L / h; Preferably, the feed rate of the first complexing agent solution is 0.5 to 10 L / h; Preferably, the pH value of the first coprecipitation reaction is 8-12.
6. The preparation method according to claim 4 or 5, characterized in that: The concentration of the coating agent solution containing element A is 0.5-1.5 mol / L; Preferably, the concentration of the second precipitant solution is 2 to 15 mol / L; Preferably, the concentration of the second complexing agent solution is 4 to 12 mol / L; Preferably, the feeding rate of the coating agent solution containing element A is 0 to 10 L / h and does not include 0 L / h; Preferably, the feed rate of the second precipitant solution is 0.1 to 2 L / h; Preferably, the feed rate of the second complexing agent solution is 0.05 to 1 L / h; Preferably, the pH value of the second coprecipitation reaction is 8-12.
7. The preparation method according to any one of claims 4 to 6, characterized in that: The preparation method comprises the following steps: A mixed salt solution of the main metal element and the doping element A is fed at a rate of 4 to 50 L / h, a first precipitant solution is fed at a rate of 1 to 10 L / h, and a first complexing agent solvent is fed at a rate of 0.5 to 10 L / h for a first coprecipitation reaction, wherein the pH value during the first coprecipitation reaction is 8 to 12, to obtain a sodium electrode precursor matrix material; After the first coprecipitation reaction is completed, a coating agent solution containing at least one element of the A element at a feeding rate of 0 to 10 L / h and excluding 0 L / h, a second precipitant solution at a feeding rate of 0.1 to 2 L / h, and a second complexing agent solution at a feeding rate of 0.05 to 1 L / h are continuously added to carry out a second coprecipitation reaction, during which the pH value is 8 to 12 to obtain the doped and coated sodium electric precursor material; The element A includes Zn and / or Cu.
8. A doped and coated sodium positive electrode material, characterized in that: The doped and coated sodium battery positive electrode material is obtained by mixing and sintering the doped and coated sodium battery precursor material according to any one of claims 1 to 3 with a sodium source.
9. The doped coated sodium positive electrode material according to claim 8, characterized in that: The ratio of the total molar amount of metal elements in the doped and coated sodium electric precursor material to the molar amount of sodium in the sodium source is 1:(0.9-1.2); Preferably, the sintering atmosphere is an oxygen-containing atmosphere; Preferably, during the sintering process, the flow rate of the oxygen-containing gas is 3 to 8 L / min; Preferably, the sintering temperature is 700-1300° C., and the sintering time is 8-20 hours.
10. A sodium ion battery, characterized in that: The sodium ion battery comprises the doped and coated sodium positive electrode material as described in claim 8 or 9.
Citation Information
Cited By
Active-inactive element co-coated sodium electric precursor as well as preparation method and application thereof
CN119706974A