Composite positive electrode material and preparation method thereof

By mixing the positive electrode material that removes the residual alkali on the surface with water and adding phosphate to form a composite positive electrode material, the problems of energy density reduction and poor circulation performance caused by water washing are solved, and higher stability and electrochemical performance are achieved.

CN118993174APending Publication Date: 2024-11-22GEM WUXI ENERGY MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411213020.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The prior art reduces the residual alkali on the surface by washing the cathode material by water, but it leads to a decrease in energy density and poor circulation performance, which cannot effectively overcome these two major defects.

Method used

The positive electrode material that removes the residual alkali on the surface is mixed with water to form a slurry, and phosphate is added at a certain temperature, and the solid-liquid separation and oxygen atmosphere calcination is formed to form a composite positive electrode material. The surface of the positive electrode material is coated with phosphate to form a low chemical activity. Level, slows side effects and improves stability.

Benefits of technology

It effectively reduces the residual alkali on the surface of the positive electrode material, improves its stability and electrochemical properties, enhances the circulation performance and energy density, and avoids the defect of the energy density drop during the washing process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118993174A_ABST
    Figure CN118993174A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of positive electrode materials, in particular to a composite positive electrode material and a preparation method thereof. The preparation method of the composite positive electrode material provided by the invention comprises the following steps: S1, mixing a positive electrode material of which the surface residual alkali is removed with water to obtain slurry, adding phosphate into the slurry at a certain temperature, mixing, and carrying out solid-liquid separation to obtain an intermediate; and S2, calcining the intermediate in an oxygen atmosphere to obtain the composite positive electrode material. The positive electrode material after residual alkali removal is coated with phosphate through a wet method, on one hand, the phosphate is utilized to form a coating layer with low chemical activity on the surface of the positive electrode material, so that side reaction between the positive electrode material and electrolyte can be slowed down, the residual alkali on the surface of the positive electrode material can be further reduced, and the stability of the positive electrode material is improved; on the other hand, phosphate and the positive electrode material form a strong metal-oxygen covalent bond, so that the stability of the positive electrode material is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of positive electrode materials, and in particular to a composite positive electrode material and a preparation method thereof. Background Art

[0002] The safety, cycle life and energy density of positive electrode materials determine the performance of new energy batteries. At present, conventional positive electrode materials mainly include lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, lithium iron phosphate, etc. Among them, lithium nickel cobalt aluminum oxide occupies a dominant position in new energy batteries due to its high energy density, but high-nickel materials similar to lithium nickel cobalt aluminum oxide have a high nickel content, which reduces the sintering temperature and reduces the volatilization of lithium salts, resulting in excessive lithium salts remaining on the surface of the positive electrode material, causing more alkaline substances to remain on the surface of the positive electrode material, which not only affects the cycle performance of the positive electrode material, but also reduces its storage of electricity.

[0003] The prior art reduces the lithium salt on the surface of the positive electrode material and reduces the residual alkali on the surface of the positive electrode material by washing the positive electrode material with water. However, the washing process causes the energy density of the positive electrode material to decrease and the capacity of the positive electrode material to be low. Summary of the invention

[0004] Therefore, the technical problem to be solved by the present invention is to overcome the defect of reducing the capacity of the positive electrode material by washing the positive electrode material with water in the prior art, thereby providing a composite positive electrode material and a preparation method thereof.

[0005] Another technical problem to be solved by the present invention is to overcome the defect of water-washed positive electrode materials in the prior art that the cycle performance of the positive electrode materials is reduced, thereby providing a composite positive electrode material and a preparation method thereof.

[0006] To this end, the present invention provides a method for preparing a composite positive electrode material, comprising the following steps: S1, mixing the positive electrode material from which the residual alkali on the surface has been removed with water to obtain a slurry, adding phosphate to the slurry at a certain temperature, mixing, and separating the solid and liquid to obtain an intermediate; S2, calcining the intermediate in an oxygen atmosphere to obtain a composite positive electrode material.

[0007] In some of the embodiments, in step S1, the method for removing residual alkali on the surface comprises washing the positive electrode material by mixing water with the positive electrode material, wherein the mass ratio of the positive electrode material to water is 1:(0.6-1).

[0008] In some embodiments, in step S1, the material added to the slurry also includes a dispersant.

[0009] Preferably, the dispersant is at least one of carboxymethyl cellulose, polyacrylic acid, and D-650. Among them, D-650 is a ternary positive electrode dispersant, which is an additive specially used in the preparation process of positive electrode materials for lithium-ion batteries. Its main function is to improve the dispersion performance of components such as active substances, conductive agents and binders in the slurry, ensure the formation of a uniform coating during the coating process, and thus improve the electrochemical performance and consistency of the battery.

[0010] In some of the embodiments, the mass ratio of the dispersant to the positive electrode material after washing is (0.01-0.1):1.

[0011] In some of the embodiments, the mass ratio of the phosphate to the positive electrode material after washing is (0.001-0.005):1.

[0012] Preferably, the phosphate includes at least one of magnesium phosphate, nickel phosphate, cobalt phosphate and manganese phosphate.

[0013] In some of the embodiments, the mass ratio of the positive electrode material from which the residual alkali on the surface is removed to the water is 1:(0.6-1).

[0014] In some embodiments, the temperature in step S1 is provided by a water bath method, and the temperature is 60-100°C.

[0015] In some embodiments, the solid-liquid separation step is at least one of evaporation or drying.

[0016] In some embodiments, the calcination temperature in step S2 is 300-600° C., and the calcination time is 4-6 hours.

[0017] The preparation method of the positive electrode material comprises the following steps: in an oxygen atmosphere, calcining a nickel-cobalt precursor, a lithium source, an alloy element material, and a doping element material at a first temperature for a first time, and then calcining at a second temperature for a second time to obtain the positive electrode material.

[0018] Preferably, the lithium source is at least one of lithium carbonate and lithium hydroxide.

[0019] Preferably, the alloy element material is at least one of aluminum oxide, aluminum carbonate and aluminum sulfate.

[0020] Preferably, the doping element is at least one of zirconium oxide, titanium oxide or cerium oxide.

[0021] In some of the embodiments, the molar ratio of the lithium source, the nickel-cobalt precursor, the lithium source, the alloy element material and the doping element material is (1.01-1.06):1:(0.022-0.025):(0.002-0.005).

[0022] In some embodiments, the first temperature is 300-600° C., and the first time is 4-6 hours.

[0023] In some embodiments, the second temperature is 700-800° C., and the second time is 10-15 hours.

[0024] On the other hand, the present invention provides a composite positive electrode material, which is prepared by the above-mentioned method for preparing the composite positive electrode material.

[0025] The technical solution of the present invention has the following advantages:

[0026] 1. A preparation method of a composite positive electrode material provided by the present invention comprises the following steps: S1, mixing the positive electrode material from which the residual alkali on the surface has been removed with water to obtain a slurry, adding phosphate to the slurry at a certain temperature, and then separating the solid and liquid to obtain an intermediate; S2, calcining the intermediate under an oxygen atmosphere to obtain a composite positive electrode material. The present invention utilizes the positive electrode material from which the residual alkali on the surface has been removed to mix with water to form a slurry, and adds phosphate thereto, and coats the positive electrode material from which the residual alkali has been removed with phosphate by a wet method. On the one hand, the phosphate is used to form a coating layer with low chemical activity on the surface of the positive electrode material, which can not only slow down the side reaction between the positive electrode material and the electrolyte, but also can further reduce the residual alkali on the surface of the positive electrode material, thereby improving the stability of the positive electrode material. On the other hand, the phosphate is used to form a strong metal-oxygen covalent bond with the positive electrode material, thereby improving the stability of the positive electrode material.

[0027] 2. In a method for preparing a composite positive electrode material provided by the present invention, in step S1, the material added to the slurry also includes a dispersant. In the present invention, by adding a dispersant to the slurry during the water washing process, the distribution of phosphate on the surface of the positive electrode material can be improved, so that the coating of phosphate on the surface of the positive electrode material is more uniform, and the performance of the prepared positive electrode material is more stable. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0029] Figure 1 It is a process flow chart of the method for preparing the composite positive electrode material in Example 1 of the present invention. DETAILED DESCRIPTION

[0030] The following examples are provided for a better understanding of the present invention, but are not intended to limit the best mode of implementation, nor to limit the content and protection scope of the present invention. Any product identical or similar to the present invention obtained by anyone under the inspiration of the present invention or by combining the features of the present invention with other prior arts shall fall within the protection scope of the present invention.

[0031] If no specific experimental steps or conditions are specified in the examples, the conventional experimental steps or conditions described in the literature in the field can be used. If no manufacturer is specified for the reagents or instruments used, they are all conventional reagent products that can be obtained commercially.

[0032] Example 1

[0033] See also Figure 1 As shown, this embodiment provides a method for preparing a composite positive electrode material, and the specific steps and parameters are as follows:

[0034] (1) The nickel-cobalt precursor is uniformly mixed with Li2CO3, Al2O3, and ZrO2, and the mixture is kept at 500°C for 5 hours and then kept at 720°C for 10 hours in a pure oxygen atmosphere to obtain a ternary positive electrode material, wherein the molar ratio of lithium salt to the nickel-cobalt precursor, aluminum source, and ZrO2 is 1.05:1:0.023:0.0038, and the residual alkali on the surface of the material is characterized by a lithium hydroxide content of 0.55wt% and a lithium carbonate content of 0.42wt%;

[0035] (2) Pour the ternary positive electrode material obtained in step (1) and water into a water washing tank in a mass ratio of 1:0.6 to form a slurry, and then perform slurry washing. After washing, the slurry is filtered to obtain a washed material.

[0036] (3) mixing the washed material obtained in step (2) with water in a mass ratio of 1:0.6 to obtain a slurry, pouring the slurry into a washing beaker and heating it in a water bath at a temperature of 80° C., and simultaneously adding cobalt phosphate and dispersant polyacrylic acid (PAA) to the slurry, wherein the mass ratio of cobalt phosphate to the washed material is 0.003:1, and the mass ratio of the dispersant to the washed material is 0.05:1, and continuously stirring until the water is evaporated to dryness, and placing the evaporated mixture in a vacuum drying oven for drying to obtain an intermediate, wherein the surface residual alkali of the intermediate is characterized by a lithium hydroxide content of 0.40wt% and a lithium carbonate content of 0.1wt%;

[0037] (4) The intermediate obtained in step (3) is kept at 600° C. for 6 h in a pure oxygen atmosphere to obtain a composite positive electrode material.

[0038] Example 2

[0039] This embodiment provides a method for preparing a composite positive electrode material, and the specific steps and parameters are as follows:

[0040] (1) The nickel-cobalt precursor is uniformly mixed with LiOH, Al2O3, and ZrO2, and the mixture is kept at 600°C for 6 hours and then kept at 700°C for 10 hours in a pure oxygen atmosphere to obtain a ternary positive electrode material, wherein the molar ratio of lithium salt to the nickel-cobalt precursor, aluminum source, and ZrO2 is 1.06:1:0.025:0.002, and the residual alkali on the surface of the material is characterized by a lithium hydroxide content of 0.52wt% and a lithium carbonate content of 0.44wt%;

[0041] (2) Pour the ternary positive electrode material obtained in step (1) and water into a water washing tank in a mass ratio of 1:1 to form a slurry, and then perform slurry washing. After washing, the slurry is filtered to obtain a washed material.

[0042] (3) mixing the washed material obtained in step (2) with water in a mass ratio of 1:1 to obtain a slurry, pouring the slurry into a washing beaker and heating it in a water bath at a temperature of 80° C., and adding magnesium phosphate and dispersant carboxymethyl cellulose (CMC) to the slurry, wherein the mass ratio of magnesium phosphate to the washed material is 0.001:1, and the mass ratio of the dispersant to the washed material is 0.05:1, and stirring is continued until the water is evaporated, and the evaporated mixture is placed in a vacuum drying oven for drying to obtain an intermediate, wherein the surface residual alkali of the intermediate is characterized by a lithium hydroxide content of 0.42wt% and a lithium carbonate content of 0.11wt%;

[0043] (4) The intermediate obtained in step (3) is kept at 600° C. for 4 h in a pure oxygen atmosphere to obtain a composite positive electrode material.

[0044] Example 3

[0045] This embodiment provides a method for preparing a composite positive electrode material, and the specific steps and parameters are as follows:

[0046] (1) The nickel-cobalt precursor is uniformly mixed with Li2CO3, Al2CO3, and TiO2, and the mixture is kept at 300°C for 4 hours and then kept at 800°C for 15 hours in a pure oxygen atmosphere to obtain a ternary positive electrode material, wherein the molar ratio of lithium salt to the nickel-cobalt precursor, aluminum source, and TiO2 is 1.05:1:0.022:0.005, and the residual alkali on the surface of the material is characterized by a lithium hydroxide content of 0.50wt% and a lithium carbonate content of 0.46wt%;

[0047] (2) Pour the ternary positive electrode material obtained in step (1) and water into a water washing tank in a mass ratio of 1:0.6 to form a slurry, and then perform slurry washing. After washing, the slurry is filtered to obtain a washed material.

[0048] (3) mixing the washed material obtained in step (2) with water in a mass ratio of 1:0.6 to obtain a slurry, pouring the slurry into a washed beaker and heating it in a water bath at a temperature of 60° C., and simultaneously adding manganese phosphate and dispersant ternary positive electrode dispersant D-650 to the slurry, wherein the mass ratio of manganese phosphate to the washed material is 0.005:1, and the mass ratio of the dispersant to the washed material is 0.1:1, and continuously stirring until the water is evaporated, and placing the evaporated mixture in a vacuum drying oven for drying to obtain an intermediate, wherein the surface residual alkali of the intermediate is characterized by a lithium hydroxide content of 0.38wt% and a lithium carbonate content of 0.12wt%;

[0049] (4) The intermediate obtained in step (3) is kept at 600° C. for 4 h in a pure oxygen atmosphere to obtain a composite positive electrode material.

[0050] Example 4

[0051] This embodiment provides a method for preparing a composite positive electrode material, and the specific steps and parameters are as follows:

[0052] (1) The nickel-cobalt precursor is uniformly mixed with LiOH, Al2SO4, and CeO2, and the mixture is kept at 400°C for 5 hours and then kept at 800°C for 15 hours in a pure oxygen atmosphere to obtain a ternary positive electrode material, wherein the molar ratio of lithium salt to nickel-cobalt precursor, aluminum source, and CeO2 is 1.01:1:0.024:0.003, and the residual alkali on the surface of the material is characterized by a lithium hydroxide content of 0.55wt% and a lithium carbonate content of 0.43wt%;

[0053] (2) Pour the ternary positive electrode material obtained in step (1) and water into a water washing tank in a mass ratio of 1:0.6 to form a slurry, and then perform slurry washing. After washing, the slurry is filtered to obtain a washed material.

[0054] (3) mixing the washed material obtained in step (2) with water in a mass ratio of 1:0.6 to obtain a slurry, pouring the slurry into a washing beaker and heating it in a water bath at a temperature of 100° C., and adding nickel phosphate and dispersant PAA to the slurry, wherein the mass ratio of cobalt phosphate to the washed material is 0.005:1, and the mass ratio of the dispersant to the washed material is 0.01:1, and stirring is continued until the water is evaporated, and the evaporated mixture is placed in a vacuum drying oven for drying to obtain an intermediate, wherein the surface residual alkali of the intermediate is characterized by a lithium hydroxide content of 0.40wt% and a lithium carbonate content of 0.1wt%;

[0055] (4) The intermediate obtained in step (3) is kept warm at 300° C. for 4 h in a pure oxygen atmosphere to obtain a composite positive electrode material.

[0056] Example 5

[0057] This embodiment provides a method for preparing a composite positive electrode material, and the specific steps and parameters are as follows:

[0058] (1) The nickel-cobalt precursor is uniformly mixed with LiOH, Al2O3, and ZrO2, and the mixture is kept at 400°C for 5 hours and then kept at 800°C for 15 hours in a pure oxygen atmosphere to obtain a ternary positive electrode material, wherein the molar ratio of lithium salt to the nickel-cobalt precursor, aluminum source, and ZrO2 is 1.03:1:0.024:0.005, and the residual alkali on the surface of the material is characterized by a lithium hydroxide content of 0.52wt% and a lithium carbonate content of 0.42wt%;

[0059] (2) Pour the ternary positive electrode material obtained in step (1) and water into a water washing tank in a mass ratio of 1:0.6 to form a slurry, and then perform slurry washing. After washing, the slurry is filtered to obtain a washed material.

[0060] (3) mixing the washed material obtained in step (2) with water in a mass ratio of 1:0.6 to obtain a slurry, pouring the slurry into a washing beaker and heating it in a water bath at a temperature of 70° C., and adding nickel phosphate and dispersant PAA to the slurry, wherein the mass ratio of nickel phosphate to the washed material is 0.005:1, and the mass ratio of the dispersant to the washed material is 0.01:1, and stirring is continued until the water is evaporated, and the evaporated mixture is placed in a vacuum drying oven for drying to obtain an intermediate, wherein the surface residual alkali of the intermediate is characterized by a lithium hydroxide content of 0.39wt% and a lithium carbonate content of 0.11wt%;

[0061] (4) The intermediate obtained in step (3) is kept at 400° C. for 5 h in a pure oxygen atmosphere to obtain a composite positive electrode material.

[0062] Example 6

[0063] The present embodiment provides a method for preparing a composite positive electrode material, wherein the specific steps and parameters are the same as those of Embodiment 1, except that step (3) does not contain a dispersant, i.e., in step (3), the washed material obtained in step (2) is mixed with water at a mass ratio of 1:0.6 to obtain a slurry, the slurry is poured into a washed beaker and heated in a water bath at a temperature of 80° C., and cobalt phosphate is added to the slurry at a mass ratio of cobalt phosphate to the washed material of 0.003:1, the mixture is stirred continuously until the water is evaporated, and the evaporated mixture is placed in a vacuum drying oven for drying to obtain an intermediate.

[0064] Comparative Example 1

[0065] This comparative example provides a method for preparing a composite positive electrode material, wherein the specific steps and parameters are the same as those of Example 1, except that step (3) does not contain magnesium phosphate, that is, the washed material obtained in step (2) is mixed with water in a mass ratio of 1:1, poured into a water-washing beaker and heated in a water bath at a heating temperature of 80°C, and a dispersant polyacrylic acid (PAA) is added thereto at a mass ratio of the dispersant to the washed material of 0.05:1, and the mixture is continuously stirred until the water is evaporated, and the evaporated mixture is placed in a vacuum drying oven for drying to obtain an intermediate.

[0066] Comparative Example 2

[0067] This comparative example provides a method for preparing a composite positive electrode material, wherein the specific steps and parameters are the same as those of Example 1, except that step (2) is not included, namely, (1) uniformly mixing a nickel-cobalt precursor with Li2CO3, Al2O3 and ZrO2, and heat-keeping the mixture at 500°C for 5 h in a pure oxygen atmosphere, and then heat-keeping the mixture at 720°C for 10 h to obtain a ternary positive electrode material, wherein the molar ratio of lithium salt to nickel-cobalt precursor, aluminum source and ZrO2 is 1.05:1:0.023:0.0038;

[0068] (2) Mixing the positive electrode material obtained in step (1) with water in a mass ratio of 1:0.6, pouring into a water-washed beaker and heating in a water bath at a heating temperature of 80° C., and simultaneously adding cobalt phosphate and dispersant polyacrylic acid (PAA) thereto, wherein the mass ratio of cobalt phosphate to the water-washed material is 0.003:1, and the mass ratio of the dispersant to the water-washed material is 0.05:1, and stirring is continued until the water is evaporated, and the evaporated mixture is placed in a vacuum drying oven for drying to obtain an intermediate;

[0069] (3) The intermediate obtained in step (3) is kept at 600° C. for 6 h in a pure oxygen atmosphere to obtain a composite positive electrode material.

[0070] Comparative Example 3

[0071] This comparative example provides a method for preparing a composite positive electrode material, and the specific steps and parameters are as follows:

[0072] (1) uniformly mixing the nickel-cobalt precursor with Li2CO3, Al2O3 and ZrO2, and keeping the mixture at 500°C for 5 hours and then at 720°C for 10 hours in a pure oxygen atmosphere to obtain a ternary positive electrode material, wherein the molar ratio of lithium salt to the nickel-cobalt precursor, aluminum source and ZrO2 is 1.05:1:0.023:0.0038;

[0073] (2) Pour the ternary positive electrode material obtained in step (1) and water into a water washing tank in a mass ratio of 1:0.6 to form a slurry, and then perform slurry washing. After washing, the slurry is filtered to obtain a washed material.

[0074] (3) uniformly mixing the washed material, cobalt phosphate and dispersant polyacrylic acid (PAA), and drying the mixture in a vacuum drying oven to obtain an intermediate, wherein the mass ratio of cobalt phosphate to the washed material is 0.003:1, and the mass ratio of the dispersant to the washed material is 0.05:1;

[0075] (4) The intermediate obtained in step (3) is kept at 600° C. for 6 h in a pure oxygen atmosphere to obtain a composite positive electrode material.

[0076] Experimental Example 1

[0077] The surface residual alkali of the composite positive electrode materials obtained in Examples 1-6 and Comparative Examples 1-3 was tested, and the test results are shown in Table 1. By comparing the surface residual alkali of the washed material in Example 1 with the surface residual alkali of the composite positive electrode material finally obtained, it can be seen that the surface residual alkali of the positive electrode material can be further reduced by the wet coating of phosphate on the washed positive electrode material of the present invention. At the same time, compared with the composite positive electrode material obtained by the preparation method of Comparative Examples 1-3, the present invention can effectively reduce the surface residual alkali of the positive electrode material by coating phosphate during the washing process.

[0078] Experimental Example 2

[0079] The composite positive electrode material lithium ion battery positive electrode material prepared in Examples 1-6 and Comparative Examples 1-3 is used to prepare a button cell, and the preparation method of the button cell is as follows: nickel cobalt aluminum lithium positive electrode material, polyvinylidene fluoride (PVDF) as a binder, conductive carbon black (SP) as a conductive agent, and N-methylpyrrolidone (NMP) as a solvent are mixed in a dosage ratio of 96.9g:1.9g:1.6g:220mL, stirred to make a slurry, coated on a copper foil, and dried and rolled to obtain a positive electrode sheet; lithium hexafluorophosphate (LiPF6) is used as an electrolyte, and a mixture of ethylene carbonate (EC) and diethyl carbonate (DEC) in a volume ratio of 1:1 is used as a solvent to prepare an electrolyte with an electrolyte concentration of 1 mol / L; a metal lithium sheet is used as a counter electrode, and a polypropylene (PP) film is used as a diaphragm, and the button cells are assembled in an argon-filled glove box.

[0080] The electrochemical performance tests were carried out on button cells of composite positive electrode materials for lithium ion batteries prepared in Examples 1-6 and Comparative Examples 1-3, respectively. The tests were carried out using a Wuhan Blue Electric CT2001A battery tester with a charge and discharge voltage range of 2.5-4.25 V. The capacity retention rates after 50 cycles at charge and discharge rates of 0.2C and 0.5C were tested, respectively. The test results are shown in Table 1.

[0081] Table 1 Electrical performance test results of composite positive electrode materials

[0082]

[0083]

[0084] According to the data in Table 1, it can be seen that compared with Comparative Examples 1-3, the composite positive electrode material obtained by wet-coating phosphate in the present invention can effectively improve the capacity of the battery. At the same time, whether the charge and discharge rate is 0.2C or 0.5C, the cycle performance is still excellent, which proves that the composite positive electrode material provided by the present invention has good stability.

[0085] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the invention.

Claims

1. A method for preparing a composite positive electrode material, characterized in that: The following steps are included: S1, mixing the positive electrode material from which the residual alkali on the surface has been removed with water to obtain a slurry, adding phosphate to the slurry at a certain temperature, mixing, and performing solid-liquid separation to obtain an intermediate; S2, calcining the intermediate under an oxygen atmosphere to obtain a composite positive electrode material.

2. The preparation method according to claim 1, characterized in that: In step S1, the material added to the slurry also includes a dispersant; and / or, The mass ratio of the phosphate to the positive electrode material after washing is (0.001-0.005):

1.

3. The preparation method according to claim 2, characterized in that: The mass ratio of the positive electrode material from which the residual alkali on the surface is removed to the water is 1:(0.6-1); and / or, The mass ratio of the dispersant to the positive electrode material after washing is (0.01-0.1):

1.

4. The preparation method according to claim 2, characterized in that: The phosphate is at least one of magnesium phosphate, nickel phosphate, cobalt phosphate and manganese phosphate; and / or, The dispersant is at least one of carboxymethyl cellulose, polyacrylic acid and D-650.

5. The method for preparing a composite positive electrode material according to claim 4, characterized in that: The temperature in step S1 is provided by a water bath method, and the temperature is 60-100° C.; and / or, The solid-liquid separation step includes at least one of evaporation or drying.

6. The method for preparing a composite positive electrode material according to claim 5, characterized in that: The calcination temperature in step S2 is 300-600°C and the calcination time is 4-6h; and / or, In the step S1, the method for removing residual alkali on the surface includes washing the positive electrode material with water by mixing water with the positive electrode material, wherein the mass ratio of the positive electrode material to water is 1:(0.6-1).

7. The method for preparing a composite positive electrode material according to any one of claims 1 to 6, characterized in that: The preparation method of the positive electrode material comprises the following steps: in an oxygen atmosphere, calcining a nickel-cobalt precursor, a lithium source, an alloy element material, and a doping element material at a first temperature for a first time, and then calcining at a second temperature for a second time to obtain the positive electrode material.

8. The method for preparing a composite positive electrode material according to claim 7, characterized in that: The lithium source is at least one of lithium carbonate and lithium hydroxide; and / or, The alloy element material is at least one of aluminum oxide, aluminum carbonate and aluminum sulfate; and / or, The doping element is at least one of zirconium oxide, titanium oxide or cerium oxide.

9. The method for preparing a composite positive electrode material according to claim 8, characterized in that: The molar ratio of the lithium source, the nickel-cobalt precursor, the lithium source, the alloy element material and the doping element material is (1.01-1.06):1:(0.022-0.025):(0.002-0.005); and / or, The first temperature is 300-600° C., and the first time is 4-6 hours; and / or, The second temperature is 700-800° C., and the second time is 10-15 hours.

10. A composite positive electrode material, characterized in that: The composite positive electrode material is prepared by the method for preparing the composite positive electrode material according to any one of claims 1 to 9.