Double-layer coated positive electrode lithium supplementing material, preparation method thereof and obtained product
Through the double-layer coated positive electrode lithium supplement material, the problem of lithium loss and material deterioration in lithium-ion batteries is solved by using vacuum sintering and water removal agent coating technology under an inert atmosphere, and the air stability and circulation stability of the battery are improved. , reduces costs and is suitable for industrial production.
Patent Information
- Application Number
- CN202411358110.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-27
- Publication Date
- 2024-11-29
AI Technical Summary
During the first charging process of existing lithium-ion batteries, the electrolyte decomposition and solid electrolyte film formation will consume lithium in the positive electrode material, resulting in a decrease in energy density and power density. The existing coating method is costly, complex and unfavorable. Industrialized production.
A double-layer coated positive electrode lithium supplement material is used to form a dense carbon cladding layer by vacuum sintering, and further coated with a water remover under an inert atmosphere to form a double-layer protective structure to improve air stability and circulation stability.
It effectively improves the air stability and battery cycle stability of lithium supplement agents, reduces surface residual alkali and battery polarization, extends the service life of lithium-ion batteries, and reduces costs, making it suitable for industrial production.
Smart Images

Figure BDA0005064200490000071
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of lithium ion batteries, and in particular relates to a double-layer coated positive electrode lithium supplement material, a preparation method thereof and the obtained product. Background Art
[0002] As a power source, lithium-ion batteries have very broad application prospects in portable electronic products, power vehicles and energy storage fields. In order to meet the increasingly urgent demand for energy in modern society, it is necessary to continue to improve the energy density and power density of lithium-ion batteries. During the first charging process of lithium-ion batteries, the electrolyte will decompose and a solid electrolyte membrane (SEI membrane for short) will form on the surface of the negative electrode. In this process, the lithium in the positive electrode material will be consumed, thereby reducing the capacity of the lithium-ion battery. In addition, the existing graphite negative electrode material has an initial irreversible lithium loss of 5-10%. To solve this problem, a positive electrode lithium supplement is usually added to offset this part of the lithium loss. However, the positive electrode lithium supplement is unstable in the air and is very easy to deteriorate, resulting in an increase in residual alkali and a gel phenomenon when homogenized.
[0003] Based on the above problems in preparation and use, existing solutions mainly adopt doping and coating methods, among which coating is the most effective improvement method, but the general coating method will lead to more serious carbon reduction, serious reduction of material capacity, uneven coating, and poor air stability. Although the pretreatment of the metal oxide layer in the CVD method can effectively slow down carbon reduction and obtain a more uniform coating layer, the cost is too high and the process is complicated, which is not conducive to industrial production.
[0004] For example, CN113178567A discloses a positive electrode lithium supplement material and a lithium ion battery including the material. Zirconium dioxide is used to coat the surface of lithium-rich lithium nickelate. Zirconium dioxide as a coating layer can protect the lithium nickelate and improve air stability. Secondly, zirconium dioxide reacts with residual lithium on the surface of the Li2NiO2 core material to reduce the residual alkali value of the material, effectively inhibit the gas production problem of the battery, and thus obtain a stable surface structure. However, this solution simply mixes, coats and sinters Li2NiO2 with nano-scale ZrO2 in a high-speed mixer, and cannot be coated evenly. There are still many exposed surfaces in contact with the air, and it has little effect on improving conductivity. CN117335022A discloses a high-stability positive electrode lithium supplement material, a preparation method thereof and a lithium ion battery. ALD is used to deposit and coat metal oxides on the surface of the lithium supplement agent to obtain a pre-coated matrix, and the carbon source is modified by a coupling agent to obtain a pre-treated carbon source; the pre-treated carbon source is pre-mixed with an organic nanopowder, and then mixed and coated with the pre-coated matrix, which can solve the problems of poor stability, high alkalinity, high impedance, poor coating effect, and impure phase caused by carbon thermal reduction of existing positive electrode lithium supplement materials. However, the process is complicated and the cost is too high, which is not conducive to industrial production. CN112490415B discloses a lithium-ion positive electrode material lithium supplement additive, and the coating layer includes a first coating layer carbon layer and a second coating layer transition metal oxide layer. The double-layer coated Li5FeO4 of the invention has uniform and controllable particle size, shortens the migration path of electrons and ions, can realize the lithium supplement performance of the Li5FeO4 material, and prolongs the service life of the lithium-ion battery. However, the first coating layer is a carbon layer, which is easy for lithium ferrite to undergo carbon reduction, resulting in a decrease in the capacity of lithium ferrite. The second coating layer is a transition metal oxide, which has a high resistivity, affecting the lithium desorption voltage of the lithium replenisher and the lithium replenishment effect. Summary of the invention
[0005] The present invention provides a double-layer coated positive electrode lithium supplement material, a preparation method thereof and the resulting product. The lithium supplement material adopts a double-layer protection method, which can more effectively cover the lithium supplement agent, solve the problem that the lithium supplement agent is easy to deteriorate, and also solve the problem that the material deteriorates due to excessive water in the process of preparing the electrode.
[0006] In order to achieve the above-mentioned object, the present invention provides a method for preparing a double-layer coated positive electrode lithium replenishing material, wherein a lithium replenishing agent is first mixed with a carbon source, vacuum sintered to obtain a carbon-coated lithium replenishing agent LixMyOz / C, and then mixed with a dehydrating agent, reacted under an inert atmosphere, and further coated with the dehydrating agent, wherein in the lithium replenishing agent LixMyOz / C, x=2~6, y=0.5~1, and z=any integer in the range of 2~4.
[0007] In the above scheme, the present invention creatively uses a double-layer protection method to improve its air stability. The first layer of carbon coating adopts vacuum sintering. Vacuum sintering is conducive to the rapid discharge of by-products to form a denser carbon coating layer. The dense coating layer can effectively isolate water and other components in the air. The outer water-removing layer can absorb moisture from the contact material and delay the deterioration of the material. The components formed by contact with water can participate in the negative electrode film formation, thereby improving the cycle stability of the battery.
[0008] Preferably, the lithium supplement is prepared by the following method:
[0009] Mixing the lithium source and the M source to obtain a precursor mixture;
[0010] The precursor is calcined at high temperature under a continuous vacuum environment to obtain the lithium supplement LixMyOz;
[0011] The lithium supplement agent is mixed with a carbon source and vacuum carbonized to obtain LixMyOz / C;
[0012] The double-layer coated lithium supplement agent can be obtained by mixing LixMyOz / C with a dehydrating agent, reacting in an inert atmosphere and then drying.
[0013] Preferably, the lithium source is selected from at least one of Li2O, LiOH, LiOH·H2O, Li2CO3, LiNO3, Li2C2O4, and CH3COOLi;
[0014] The M source is selected from at least one of the oxides, hydroxides, sulfates, chlorates and nitrates of iron, nickel, cobalt, aluminum and manganese; preferably, the M source is selected from at least one of Fe2O3, Fe3O4, NiO, CoO, Al2O3, Mn2O3, FeC2O4, Fe(NO3)3·9H2O, Ni(NO3)2, Co(NO3)2·6H2O, Al(NO3)3·9H2O, Mn(NO3)2, FeCl3, NiCl2, AlCl3, MnCl3, Fe2(SO4)3, NiSO4, CoSO4 and Mn2(SO4)3.
[0015] Preferably, the molar ratio of the lithium source to the M source is 2-6.
[0016] Preferably, the high temperature calcination temperature is 700-900°C, the time is 1-10h, and the heating rate is 15-30°C / min;
[0017] The particle size of the obtained lithium supplement agent is D50=5-8μm, D100=25μm. It can be understood that a small particle size will make the lithium supplement agent and the carbon source mix evenly, and a more uniform coating layer can be obtained, and a large particle size will cause the electrode sheet to fall off during the recycling process of the positive electrode material, affecting the cycle life.
[0018] Preferably, the carbon source is selected from at least one of phenolic resin, sulfur, polyacrylonitrile, polyvinylidene fluoride, polyvinyl pyrrolidone, polyaniline, polyvinyl alcohol, ethylene-vinyl alcohol copolymer, ethylene-acrylate copolymer, and ethylene-methyl acrylate copolymer;
[0019] Preferably, the dehydrating agent is at least one selected from dicyclohexylcarbodiimide, hexamethyldisilazane, and diisopropylcarbodiimide.
[0020] Preferably, the molar ratio of the lithium supplement agent to the carbon source and the water removing agent is 0.2-5% of the carbon source and 0.5-2% of the water removing agent;
[0021] The vacuum sintering temperature is 300-700℃, the time is 1-10h, and the heating rate is 5-10℃ / min;
[0022] The reaction was carried out at -30-0°C under an inert atmosphere for 1-3 hours.
[0023] The present invention also provides a double-layer coated positive electrode lithium supplement material prepared by the preparation method described in any one of the above technical solutions.
[0024] The present invention also provides a lithium-ion battery, which is prepared by adding the double-layer coated positive electrode lithium supplement material described in the above technical solution as an additive to a positive electrode material.
[0025] Compared with the prior art, the advantages and positive effects of the present invention are:
[0026] 1. The present invention proposes a double-layer coated positive electrode lithium supplement material, which is prepared by vacuum sintering to form a dense carbon coating layer and a water removal layer on the basis of the provided lithium supplement agent. The lithium supplement material adopts a double-layer protection method, which can more effectively cover the lithium supplement agent, solve the problem of the lithium supplement agent being easy to deteriorate, and also solve the problem of excessive water causing material deterioration during the preparation of the electrode.
[0027] 2. The addition of the carbon layer and the dehydrating agent in the present invention can reduce the residual alkali on the surface, reduce the polarization of the battery, and improve the capacity of the lithium supplement. In addition, the components formed by the dehydrating layer and water can participate in the negative electrode film formation, improve the cycle stability of the battery, and increase the battery life. In addition, compared with the use of CVD coating, the use cost is lower and the effect is better. DETAILED DESCRIPTION
[0028] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0029] Example 1
[0030] S1. Preparation of lithium iron oxide-rich material: LiOH·H2O and iron oxide were placed in a ball mill at a ratio of 5.25:1, and the mixture was milled for 4 h at a speed of 600 r / min to obtain a mixed material.
[0031] The mixed material was calcined in a vacuum atmosphere at a heating rate of 10°C / min to 800°C and kept at that temperature for 2 hours to obtain Li5FeO4 with a particle size of D50=4.34μm and D100=25μm.
[0032] S2. Preparation of carbon-coated lithium-rich lithium iron oxide: Li5FeO4 and polyaniline were mixed by vacuum ball milling at a speed of 600 r / min for 4 hours to obtain a mixed material, which was calcined in a vacuum atmosphere at a heating rate of 10°C / min to 500°C and kept at this temperature for 2 hours to obtain a carbon-coated lithium supplement Li5FeO4 / C.
[0033] S3. Preparation of double-layer coated lithium iron-rich lithium: Li5FeO4 / C and compound 1-di(cyanodimethylsilyl) sulfate were added into a reactor containing an inert atmosphere at a mass ratio of 98:2 and mixed for 0.5h. After the reaction was completed, the reaction product was freeze-dried at -10°C for 1h to obtain the final sample.
[0034] Example 2
[0035] S1. Preparation of lithium iron oxide-rich lithium carbonate material: lithium carbonate and iron oxide are placed in a ball mill at a ratio of 5.25:1, and the mixture is milled for 4 hours at a speed of 600 r / min to obtain a mixed material.
[0036] The mixed material was calcined in a vacuum atmosphere at a heating rate of 10°C / min to 900°C and kept at this temperature for 2 hours to obtain Li5FeO4 with a particle size of D50 = 4.77 μm and D100 = 24.9 μm.
[0037] S2. Preparation of carbon-coated lithium-rich lithium iron oxide: Li5FeO4 and polyacrylonitrile were mixed by vacuum ball milling at a speed of 600 r / min for 4 hours to obtain a mixed material, which was calcined in a vacuum atmosphere at a heating rate of 10°C / min to 550°C and kept at this temperature for 2 hours to obtain a carbon-coated lithium supplement Li5FeO4 / C.
[0038] S3. Preparation of double-layer coated lithium iron-rich lithium: Li5FeO4 / C and compound diisopropylcarbodiimide were added into a reactor containing an inert atmosphere at a mass ratio of 99:1 and mixed for 0.5h. After the reaction was completed, the reaction product was freeze-dried at -20°C for 1h to obtain the final sample.
[0039] Example 3
[0040] S1. Preparation of lithium iron oxide-rich material: lithium oxide and iron oxide are placed in a ball mill at a ratio of 5.25:1, and the mixture is milled for 4 hours at a speed of 600 r / min to obtain a mixed material.
[0041] The mixed material was calcined in a vacuum atmosphere at a heating rate of 10°C / min to 900°C and kept at this temperature for 2 hours to obtain Li5FeO4 with a particle size of D50 = 4.54 μm and D100 = 24.1 μm.
[0042] S2. Preparation of carbon-coated lithium-rich lithium iron oxide: Li5FeO4 and phenolic resin were mixed by vacuum ball milling at a speed of 600 r / min for 4 hours to obtain a mixed material, which was calcined in a vacuum atmosphere at a heating rate of 10°C / min to 450°C and kept at this temperature for 2 hours to obtain a carbon-coated lithium supplement Li5FeO4 / C.
[0043] S3. Preparation of double-layer coated lithium iron-rich lithium: Li5FeO4 / C and compound hexamethyldisilazane were added into a reactor containing an inert atmosphere at a mass ratio of 99:1 and mixed for 0.5h. After the reaction was completed, the reaction product was freeze-dried at -30°C for 1h to obtain the final sample.
[0044] Comparative Example 1
[0045] The difference from Example 1 is that vacuum carbon coating and dehydration layer coating are not performed, and other operating methods are exactly the same as those in Example 1.
[0046] Comparative Example 2
[0047] The difference from Example 1 is that no dehydration layer coating is performed, and other operation methods are exactly the same as those in Example 1.
[0048] Comparative Example 3
[0049] The difference from Example 1 is that the same carbon source is used, but nitrogen sintering is performed, and the other operating methods are exactly the same as Example 1.
[0050] Battery performance test
[0051] 1. Air stability test
[0052] The lithium supplement additives prepared in each embodiment and each comparative example were mixed with a conductive agent and a binder to form a pole piece, which was assembled with a lithium sheet into a half-cell for testing. The lithium supplement capacity data after being stored for different periods of time in an air atmosphere at a temperature of 30° C. and a humidity of 30% are shown in Table 1:
[0053] Table 1
[0054] 0h(mAh / g) 24h(mAh / g) Example 1 748.5 569.1 Example 2 743.3 546.5 Example 3 732.3 562.2 Comparative Example 1 768.1 286.3 Comparative Example 2 757.2 485.6 Comparative Example 3 748.5 329.5
[0055] From the capacity data at 0h shown in the examples and comparative examples in Table 1, it can be seen that the lithium replenishing capacity of Li5FeO4 itself will be affected by the coating material, resulting in a slight decrease in capacity. The data after 24h proves that the carbon coating layer formed by vacuum sintering is obviously more air stable, proving that vacuum sintering can form a denser carbon coating layer; secondly, the capacity of double-layer coated Li5FeO4 is significantly higher than that of single-layer coating, proving that the double-layer coating has a better coating effect.
[0056] 2. Full battery performance test
[0057] The lithium supplement material prepared in this embodiment is mixed with the positive electrode material LiCoO2 in a weight ratio of 5:100. When the positive electrode material is prepared, the mixture of lithium supplement material and LiCoO2: conductive carbon black (SP): polyvinylidene fluoride (PVDF) = 90:5:5 is mixed. The negative electrode active material is graphite, the lithium battery electrolyte is 1.2 mol / L LiPF6 / EC-DMC (1:1); the polypropylene microporous film is the diaphragm. The specific process of battery production includes: batching, homogenization, coating, rolling, pole ear welding, winding, top sealing, liquid injection, and formation. In order to further prove the effectiveness of the product of the present invention, we added the products of Example 1 and Comparative Example 2 to soft-pack batteries for testing, and the data are as shown in Table 2:
[0058] Table 2 Cycling performance of soft pack battery
[0059]
[0060] As can be seen from Table 2, the highly stable double-layer coated Li5FeO4 prepared by the present invention is used as an additive in lithium-ion batteries, and the battery's initial charge and discharge efficiency (above 80.9%) and capacity retention rate after 100 cycles (above 87.9%) are both higher than those of the comparative example, indicating that the material prepared by the present invention helps to improve the capacity retention rate, which should be attributed to the functional group effect of the dehydrating agent, which participates in the film formation of the positive and negative electrodes, reduces the internal resistance of the battery, improves the battery efficiency, and improves the battery cycle stability.
Claims
1. A method for preparing a double-layer coated positive electrode lithium supplement material, characterized in that: The lithium replenisher is first mixed with a carbon source, vacuum sintered to obtain a carbon-coated lithium replenisher LixMyOz / C, and then mixed with a dehydrating agent, reacted under an inert atmosphere, and further coated with the dehydrating agent, wherein in the lithium replenisher LixMyOz / C, x=2-6, y=0.5-1, and z=any integer from 2 to 4.
2. The preparation method according to claim 1, characterized in that: The lithium supplement is prepared by the following method: Mixing the lithium source and the M source to obtain a precursor mixture; The precursor is calcined at high temperature under a continuous vacuum environment to obtain the lithium supplement LixMyOz; The lithium supplement agent is mixed with a carbon source and vacuum carbonized to obtain LixMyOz / C; The double-layer coated lithium supplement agent can be obtained by mixing LixMyOz / C with a dehydrating agent, reacting in an inert atmosphere and then drying.
3. The preparation method according to claim 2, characterized in that: The lithium source is selected from at least one of Li2O, LiOH, LiOH·H2O, Li2CO3, LiNO3, Li2C2O4, and CH3COOLi; The M source is selected from at least one of Fe2O3, Fe3O4, NiO, CoO, Al2O3, Mn2O3, FeC2O4, Fe(NO3)3·9H2O, Ni(NO3)2, Co(NO3)2·6H2O, Al(NO3)3·9H2O, Mn(NO3)2, FeCl3, NiCl2, AlCl3, MnCl3, Fe2(SO4)3, NiSO4, CoSO4, and Mn2(SO4)3.
4. The preparation method according to claim 3, characterized in that: The molar ratio of the lithium source to the M source is 2-6.
5. The preparation method according to claim 2, characterized in that: The high temperature calcination temperature is 700-900℃, the time is 1-10h, and the heating rate is 15-30℃ / min; The particle size of the obtained lithium supplement agent is D50=5-8 μm, and D100=25 μm.
6. The preparation method according to claim 1, characterized in that: The carbon source is selected from at least one of phenolic resin, sulfur, polyacrylonitrile, polyvinylidene fluoride, polyvinyl pyrrolidone, polyaniline, polyvinyl alcohol, ethylene-vinyl alcohol copolymer, ethylene-acrylate copolymer and ethylene-methyl acrylate copolymer.
7. The preparation method according to claim 1, characterized in that: The dehydrating agent is selected from at least one of dicyclohexylcarbodiimide, hexamethyldisilazane and diisopropylcarbodiimide.
8. The preparation method according to claim 1, characterized in that: The content of carbon source is 0.2-5%, and the content of water removal agent is 0.5-2%; The vacuum sintering temperature is 300-700℃, the time is 1-10h, and the heating rate is 5-10℃ / min; The reaction was carried out at -30-0°C under an inert atmosphere for 1-3 h.
9. A double-layer coated positive electrode lithium supplement material prepared according to the preparation method according to any one of claims 1 to 8.
10. A lithium ion battery, characterized in that The double-layer coated positive electrode lithium supplement material according to claim 9 is added as an additive to the positive electrode material to prepare the positive electrode.