Optical glass and optical element
By optimizing the composition combination of optical glass, eliminating PbO and As2O3, combining SiO2, B2O3 and other components, the problems of optical glass in environmental load and coloring are solved, and the effects of high refractive index and low coloring are achieved. It is suitable for optical components such as optical fibers. .
Patent Information
- Application Number
- CN202411083212.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2017-04-05
- Filing Date
- 2017-04-18
- Publication Date
- 2024-11-22
AI Technical Summary
The existing optical glass has adverse effects on environmental load during manufacturing, processing or use, and the reduction of coloring is difficult to achieve, while maintaining a high refractive index.
Using combinations of SiO2, B2O3, Na2O, CaO, BaO, ZnO, ZrO2, La2O3 and other components, PbO and As2O3 are excluded, and the component ratio is optimized to form optical glass without environmental load components to ensure high refractive index and low coloring.
It realizes optical glass without environmental load components, maintains a moderately high refractive index and reduces coloring, and is suitable for core materials for optical components such as optical fibers.
Smart Images

Figure BDA0004984401670000111
Abstract
Description
[0001] Related Applications
[0002] This application is a divisional application of Chinese Patent Application No. 201780088292.0 (the filing date is deemed to be 2017.04.18), whose invention name is “Optical Glass and Optical Elements” and was filed on September 11, 2019 (the date when the PCT application entered the national phase), and claims all the priorities and rights of the original application and cites the entire contents of the original application specification, etc. as a whole. Technical Field
[0003] The invention relates to optical glass and optical element. Background Art
[0004] In recent years, glass with high transmittance has been used in various products such as light guides, endoscopes, and exposure devices. In addition, in these uses of glass, it is necessary to have a glass with a high transmittance and a moderately high refractive index, specifically, a refractive index (nd) in the range of about 1.58 to 1.66.
[0005] As a glass that meets this demand, for example, Patent Document 1 discloses that by basically being composed of SiO2-La2O3-BaO-RO-R'2O system (R = Mg, Ca, Sr, Zn and Pb, R' = Li, Na and K) and setting it to a predetermined composition, an optical glass having excellent light transmittance in a short wavelength region can be obtained, specifically, an optical glass having a coloring degree of 35 to 36, wherein the coloring degree represents a wavelength showing 80% transmittance in units of 10 nm. Furthermore, the refractive index of the optical glass is roughly within the above range.
[0006] Prior art literature
[0007] Patent Literature
[0008] Patent Document 1: Japanese Patent Application Laid-Open No. 60-046945 Summary of the invention
[0009] Problems that the invention aims to solve
[0010] However, the optical glass disclosed in Patent Document 1 is substantially reduced in coloration by using at least one of PbO and As2O3 as an essential component, and therefore, there is a problem of adversely affecting the environmental load during manufacturing or use. In addition, for these optical glasses, further reduction in coloration is also desired.
[0011] Therefore, the present invention is completed in order to advantageously solve the above-mentioned problems, and its object is to provide an optical glass which does not contain components that have an adverse effect on environmental load and is less colored while maintaining a moderately high refractive index. In addition, the present invention also aims to provide an optical element using the optical glass and which is less colored while maintaining a moderately high refractive index.
[0012] Means for solving problems
[0013] The technical solution for solving the technical problem is as follows.
[0014] That is, the optical glass of the present invention is characterized in that it has a composition containing, by mass%, SiO2 of 30% to 47%, B2O3 of 0% to 10%, Na2O of 3% to 12%, Li2O of 0% to 5%, CaO of 0% to 3.8%, BaO of 28% to 43%, ZnO of 3% to 16%, ZrO2 of 0% to 8%, La2O3 of 0% to 15% (wherein the composition is a composition without considering Sb2O3), and does not contain PbO, As2O3, and K2O. The optical glass does not contain components that have an adverse effect on environmental load and has less coloring while maintaining a moderately high refractive index.
[0015] Here, in this specification, “does not include” means intentionally not to include, that is, does not substantially (basically) include.
[0016] In the optical glass of the present invention, the refractive index (nd) is preferably 1.58 or more and 1.66 or less.
[0017] In the optical glass of the present invention, preferably, the degree of tint (λ80) is 34 or less.
[0018] In the optical glass of the present invention, preferably, the ratio of the BaO content in the total content of MgO, CaO, SrO, and BaO is 91 mass % or more.
[0019] Preferably, the optical glass of the present invention does not contain MgO and SrO.
[0020] Preferably, the optical glass of the present invention contains Sb2O3 in an outer percentage (outer percentage: outer percentage) of 1 mass % or less.
[0021] The optical glass of the present invention is preferably used as core glass for optical fibers.
[0022] The optical element of the present invention is characterized by comprising the optical glass of the present invention. The optical element has a low coloration while maintaining a moderately high refractive index.
[0023] Effects of the Invention
[0024] Based on the present invention, it is possible to provide an optical glass that does not contain components that have an adverse effect on environmental load and is less colored while maintaining a moderately high refractive index. In addition, based on the present invention, it is also possible to provide an optical element that uses the optical glass and is less colored while maintaining a moderately high refractive index. DETAILED DESCRIPTION
[0025] (Optical Glass)
[0026] Next, the optical glass of the present invention will be described in detail.
[0027] The optical glass of the present invention is characterized in that it has a composition, in mass %, containing SiO2 of 30% or more and 47% or less, B2O3 of 0% or more and 10% or less, Na2O of 3% or more and 12% or less, Li2O of 0% or more and 5% or less, CaO of 0% or more and 3.8% or less, BaO of 28% or more and 43% or less, ZnO of 3% or more and 16% or less, ZrO2 of 0% or more and 8% or less, La2O3 of 0% or more and 15% or less (wherein the composition is a composition without considering Sb2O3), and does not contain PbO, As2O3 and K2O.
[0028] It should be noted that, from the viewpoint of further reducing coloration, preferably, the optical glass of the present invention is only constituted as follows: optionally containing Sb2O3, and having a composition containing, in mass %, SiO2 of 30% or more and 47% or less, B2O3 of 0% or more and 10% or less, Na2O of 3% or more and 12% or less, Li2O of 0% or more and 5% or less, CaO of 0% or more and 3.8% or less, BaO of 28% or more and 43% or less, ZnO of 3% or more and 16% or less, ZrO2 of 0% or more and 8% or less, and La2O3 of 0% or more and 15% or less (wherein the composition is a composition without taking Sb2O3 into account).
[0029] <ingredients>
[0030] First, the reason for limiting the composition of the optical glass to the above-mentioned specified range in the present invention is explained. It should be noted that the "%" of the components other than Sb2O3 described below, unless otherwise specified, represents "mass %" and is set to the mass % calculated without considering the optionally included Sb2O3.
[0031] [SiO2]
[0032] SiO2 is an essential component in the optical glass of the present invention, which can form a network structure of the glass and inhibit crystallization when the glass is formed, thereby improving the chemical durability of the glass. If the proportion of SiO2 in the optical glass is less than 30%, the effect of inhibiting crystallization and improving chemical durability cannot be fully obtained. On the other hand, if the proportion of SiO2 in the optical glass exceeds 47%, the viscosity of the glass melt becomes high and the meltability deteriorates, so it is possible to increase the coloring of the obtained optical glass. Therefore, the proportion of SiO2 in the optical glass of the present invention is set to more than 30% and less than 47%. From the same viewpoint, the proportion of SiO2 in the optical glass of the present invention is preferably more than 31%, more preferably more than 32%, and also preferably less than 46%, more preferably less than 45%.
[0033] [B2O3]
[0034] B2O3 is an optional component in the optical glass of the present invention. Like SiO2, this component can form a network structure of glass and inhibit crystallization when the glass is formed. In addition, B2O3 is a component that can promote intermittent reaction and / or adjust the viscosity of the glass melt when manufacturing optical glass. However, if the proportion of B2O3 in the optical glass exceeds 10%, it is possible to cause phase separation and fail to obtain the desired performance. Therefore, the proportion of B2O3 in the optical glass of the present invention is set to more than 0% and less than 10%. From the same viewpoint, the proportion of B2O3 in the optical glass of the present invention is preferably less than 9.5%, more preferably less than 9%.
[0035] [SiO2+B2O3]
[0036] Here, in the optical glass of the present invention, from the viewpoint of fully suppressing crystallization when the glass is formed, the total ratio of SiO2 and B2O3 is preferably 37% or more, and more preferably 38% or more. In addition, in the optical glass of the present invention, from the viewpoint of obtaining a desired refractive index, the total ratio of SiO2 and B2O3 is preferably 55% or less, and more preferably 53% or less.
[0037] [Na2O]
[0038] Na2O is an essential component in the optical glass of the present invention. This component promotes intermittent reaction and / or reduces the viscosity of the glass melt when manufacturing the optical glass, and greatly helps to improve the glass solubility, as well as improve the transmittance and reduce coloring of the optical glass. If the proportion of Na2O in the optical glass is less than 3%, the effects of improving the above-mentioned glass solubility cannot be obtained. On the other hand, if the proportion of Na2O in the optical glass exceeds 12%, it is possible that the glass is easily crystallized when formed and the desired performance cannot be obtained. Therefore, the proportion of Na2O in the optical glass of the present invention is set to be greater than 3% and less than 12%. From the same point of view, the proportion of Na2O in the optical glass of the present invention is preferably greater than 3.8%, more preferably greater than 4%, further preferably greater than 5%, and also preferably less than 11%, more preferably less than 10.5%.
[0039] [Li2O]
[0040] Li2O is an optional component in the optical glass of the present invention, which brings the same effect as Na2O. In addition, by using Li2O and Na2O together, a mixed alkali effect can be brought about. However, if the proportion of Li2O in the optical glass exceeds 5%, it is possible that the glass will be easily crystallized when formed and the desired performance cannot be obtained. Therefore, the proportion of Li2O in the optical glass of the present invention is set to more than 0% and less than 5%. From the same point of view, the proportion of Li2O in the optical glass of the present invention is preferably less than 4%, more preferably less than 3.5%.
[0041] [Na2O+Li2O]
[0042] Here, in the optical glass of the present invention, from the viewpoint of further improving the glass meltability and further reducing the coloring of the optical glass, the total ratio of Na2O and Li2O is preferably 3.8% or more, more preferably 4% or more.
[0043] [K2O]
[0044] Like Na2O and Li2O, K2O is also an alkali metal oxide, and this component has a tendency to show similar performance to these components. However, if K2O is selected as an alkali metal oxide and used in optical glass, the viscosity of the glass melt at the same temperature is high and the glass meltability is poor compared to when Na2O or Li2O is used, so it is necessary to increase the melting temperature. And, as a result, the transmittance and coloration of the optical glass will be adversely affected. Therefore, from the viewpoint of effectively obtaining the desired performance, the optical glass of the present invention does not contain K2O.
[0045] [MgO]
[0046] MgO is a component that can improve the stability of glass in a small amount. However, in the MgO raw materials that are easily available on the market, most of them contain transition metals to a certain extent, and these transition metals can cause the coloring (transmittance reduction) of glass as impurities. Therefore, from the viewpoint of being difficult to raise high-purity raw materials and suppressing the coloring of optical glass, it is preferred that MgO is not used when manufacturing the optical glass of the present invention, in other words, it is preferred that the optical glass of the present invention does not contain MgO.
[0047] [CaO]
[0048] CaO is an optional component in the optical glass of the present invention, which can improve the stability and solubility of the glass and adjust the refractive index. However, if the proportion of CaO in the optical glass exceeds 3.8%, it is difficult to obtain the desired refractive index. In this case, in order to achieve the desired refractive index, it is necessary to use a component that can reduce the transmittance to adjust the refractive index. Therefore, the proportion of CaO in the optical glass of the present invention is set to be greater than 0% and less than 3.8%. From the same point of view, the proportion of CaO in the optical glass of the present invention is preferably less than 3.7%, more preferably less than 3.5%.
[0049] [SrO]
[0050] Similar to MgO, SrO is also a component that can improve the stability of glass in a small amount. However, similar to MgO, in the SrO raw materials that are easily available on the market, there are many cases where transition metals are included to a certain extent, and the transition metals can cause the coloring of glass (transmittance reduction) as impurities. Therefore, from the viewpoint of being difficult to raise high-purity raw materials and the viewpoint of suppressing the coloring of optical glass, it is preferred that SrO is not used when manufacturing the optical glass of the present invention. In other words, it is preferred that the optical glass of the present invention does not contain SrO.
[0051] [BaO]
[0052] BaO is an essential component in the optical glass of the present invention, and this component can bring the following effects: improve the refractive index, reduce the melting temperature, and suppress the degradation of the transmittance of short wavelengths. If the proportion of BaO in the optical glass is less than 28%, it is possible that the refractive index cannot be improved and the desired refractive index cannot be obtained, and the melting temperature will become higher, thereby being unable to avoid the degradation of the transmittance of short wavelengths. On the other hand, if the proportion of BaO in the optical glass exceeds 43%, it is possible that the stability of the glass deteriorates and crystallizes, thereby being unable to obtain the desired performance. Therefore, the proportion of BaO in the optical glass of the present invention is set to be greater than 28% and less than 43%. From the same viewpoint, the proportion of BaO in the optical glass of the present invention is preferably greater than 28.5%, more preferably greater than 29%, and also preferably less than 42%, more preferably less than 41%.
[0053] [MgO+CaO+SrO+BaO]
[0054] Here, in the optical glass of the present invention, from the viewpoint of effectively improving the refractive index, the total ratio of MgO, CaO, SrO and BaO is preferably 28% or more, more preferably 28.5% or more, and further preferably 29% or more. In addition, in the optical glass of the present invention, from the viewpoint of fully suppressing the stability degradation of the glass and crystallization, the total ratio of MgO, CaO, SrO and BaO is preferably 43% or less, more preferably 42% or less, and further preferably 40% or less.
[0055] [BaO / (MgO+CaO+SrO+BaO)]
[0056] In addition, in the optical glass of the present invention, the ratio of BaO content in the total content of MgO, CaO, SrO and BaO is preferably 91% by mass or more. By making the above ratio 91% by mass or more, optical constants such as refractive index can be within the desired range, and transmittance can be improved and coloring can be fully reduced. From the same viewpoint, in the optical glass of the present invention, the ratio of BaO content in the total content of MgO, CaO, SrO and BaO is preferably 91.3% or more, and more preferably 91.5% or more.
[0057] [ZnO]
[0058] ZnO is an essential component in the optical glass of the present invention, which can increase the refractive index of the glass, improve the chemical durability of the glass, and reduce the melting temperature. If the proportion of ZnO in the optical glass is less than 3%, it is possible that the desired refractive index cannot be obtained. On the other hand, if the proportion of ZnO in the optical glass exceeds 16%, it is possible that the stability of the glass deteriorates and crystallizes, thereby failing to obtain the desired performance. Therefore, the proportion of ZnO in the optical glass of the present invention is set to be greater than 3% and less than 16%. From the same viewpoint, the proportion of ZnO in the optical glass of the present invention is preferably greater than 4%, more preferably greater than 5%, further preferably less than 15%, more preferably less than 13.5%.
[0059] [ZrO2]
[0060] ZrO2 is an optional component in the optical glass of the present invention, which can suppress the degradation of the transmittance of short wavelengths, while increasing the refractive index of the glass and the chemical durability of the glass. However, if the proportion of ZrO2 in the optical glass exceeds 8%, it is possible that the melting temperature becomes high and the stability of the glass deteriorates and crystallizes, thereby failing to obtain the desired performance. Therefore, the proportion of ZrO2 in the optical glass of the present invention is set to be above 0% and below 8%. From the same viewpoint, the proportion of ZrO2 in the optical glass of the present invention is preferably below 7%, more preferably below 6%.
[0061] [La2O3]
[0062] La2O3 is an optional component in the optical glass of the present invention, which can relatively suppress the degradation of the transmittance of short wavelengths, while increasing the refractive index of the glass and the chemical durability of the glass. However, if the proportion of La2O3 in the optical glass exceeds 15%, it is possible that the stability of the glass will deteriorate and crystallize, thereby failing to obtain the desired performance. Therefore, the proportion of La2O3 in the optical glass of the present invention is set to be greater than 0% and less than 15%. From the same viewpoint, the proportion of La2O3 in the optical glass of the present invention is preferably less than 12%, more preferably less than 10.5%.
[0063] [ZrO2+La2O3]
[0064] Here, in the optical glass of the present invention, from the viewpoint of effectively improving the refractive index, the total ratio of ZrO2 and La2O3 is preferably 0.5% or more. In addition, in the optical glass of the present invention, from the viewpoint of fully suppressing the stability degradation of the glass and crystallization, the total ratio of ZrO2 and La2O3 is preferably 15% or less, and more preferably 13% or less.
[0065] [Nb2O5, Ta2O5]
[0066] Nb2O5 and Ta2O5 are components that can increase the refractive index, but they also deteriorate the transmittance at short wavelengths. Therefore, from the viewpoint of suppressing coloration, the optical glass of the present invention preferably does not contain Nb2O5 and Ta2O5.
[0067] [Sb2O3, degassing ingredients]
[0068] The optical glass of the present invention may optionally contain a small amount (for example, 1% by mass or less in terms of external proportion) of Sb2O3, which can function as a clarifier during manufacture. In addition, the optical glass of the present invention may optionally contain a small amount (for example, 1% or less in the optical glass) of an industrially known degassing component.
[0069] [PbO, As2O3]
[0070] The high toxicity of PbO and As2O3 limits the application range of products and also has an adverse effect on the environmental load during manufacturing, processing or use. Therefore, the optical glass of the present invention does not contain PbO and As2O3.
[0071] [Other ingredients]
[0072] Unless departing from the purpose of the present invention, the optical glass of the present invention may contain components other than the above components, for example, GeO2, Y2O3, Gd2O3, Ga2O3, In2O3, etc.
[0073] <Refractive Index (nd)>
[0074] Preferably, the refractive index (nd) of the optical glass of the present invention having the above composition is 1.58 or more and 1.66 or less. If the refractive index of the optical glass is within the above range, for example, when the optical glass is used in the core of an optical fiber, the numerical aperture (NA) of the optical fiber can be appropriately increased. In addition, the refractive index (nd) of the optical glass is preferably 1.59 or more, more preferably 1.65 or less, and further preferably 1.64 or less.
[0075] It should be noted that the refractive index (nd) of the optical glass can be adjusted, for example, by limiting the overall composition within a predetermined range and adjusting the amount of components that may affect the refractive index when preparing the optical glass.
[0076] <Coloring degree (λ80)>
[0077] Preferably, the coloring degree (λ80) of the optical glass of the present invention having the above composition is 34 or less. If the coloring degree (λ80) of the optical glass is 34 or less, the coloring is sufficiently reduced, and the optical glass can be preferably used as, for example, core glass of an optical fiber, especially an optical fiber for long-distance transmission.
[0078] It should be noted that the tint degree (λ80) of the optical glass can be adjusted, for example, by limiting the overall composition within a specified range when preparing the optical glass and adjusting the amount of components that may affect the tint degree or transmittance.
[0079] In addition, in this specification, "the degree of coloration of the optical glass (λ80)" means: the spectral transmittance (including reflection loss) is measured using a 10 mm thick optical glass sample that has been polished on both sides, and the wavelength at which the spectral transmittance shows 80% is rounded to the first integer and expressed in units of 10 nm.
[0080] <Manufacturing of optical glass>
[0081] The optical glass of the present invention only needs to satisfy the above-mentioned requirements on components, and the production method thereof is not particularly limited, and the conventional production method may be used.
[0082] For example, first, oxides, hydroxides, carbonates, nitrates, etc. are prepared as raw materials of various components that can be included in the optical glass of the present invention, these raw materials are weighed to reach a specified ratio and uniformly mixed, and the obtained mixture is used as a glass blending raw material. Then, the raw material is put into a heat-resistant container that is not reactive with glass raw materials, such as a crucible composed of platinum, alumina, quartz, etc., and heated to 1000°C to 1400°C in an electric furnace to melt it, and stirred at appropriate times to clarify and homogenize it. Then, after casting it into a mold preheated to an appropriate temperature, it is slowly cooled in an electric furnace to eliminate strain, thereby being able to produce the optical glass of the present invention.
[0083] <Application of optical glass>
[0084] The optical glass of the present invention can be used in optical elements such as various lenses, optical fibers, filter substrates, etc., without particular limitation. In particular, the glass of the present invention has little coloration while maintaining a moderately high refractive index, and therefore can be preferably used as a core glass for optical fibers, especially long-distance transmission optical fibers, to manufacture optical fibers with large apertures.
[0085] (Optical Components)
[0086] The optical element of the present invention is characterized by comprising the optical glass of the present invention. Since the optical element of the present invention uses the optical glass of the present invention as a raw material, it has a moderately high refractive index and is less colored.
[0087] It should be noted that, from the viewpoint of obtaining the desired performance, the optical element of the present invention preferably satisfies the aforementioned necessary conditions related to the composition of each component for the optical glass of the present invention, and more preferably the optical element of the present invention satisfies the aforementioned various necessary conditions considered to be preferred for the optical glass of the present invention.
[0088] The types of optical elements are not limited. Typical optical elements include: aspheric lenses, spherical lenses, or lenses such as plano-concave lenses, plano-convex lenses, biconcave lenses, biconvex lenses, convex meniscus lenses, and concave meniscus lenses; microlenses; lens arrays; lenses with diffraction gratings; prisms; prisms with lens functions, etc. As optical elements, preferably, lenses such as convex meniscus lenses, concave meniscus lenses, biconvex lenses, biconcave lenses, plano-convex lenses, and plano-concave lenses; prisms; and diffraction gratings can be exemplified. Each of the above lenses can be an aspheric lens or a spherical lens. The surface can be provided with an anti-reflection film or a local reflection film with wavelength selectivity, etc. as needed.
[0089] It should be noted that the manufacturing method of the optical element is not particularly limited as long as the optical glass of the present invention is used as a raw material, and the existing manufacturing method can be used. For example, the optical element can be manufactured by melting the optical glass of the present invention, obtaining a preform (preformed glass raw material) from the obtained molten glass, and then, the preform is precision pressed.
[0090] Example
[0091] Hereinafter, the optical glass of the present invention will be specifically described with reference to Examples and Comparative Examples, but the present invention is not limited to these Examples.
[0092] Prepare oxides, hydroxides, carbonates and nitrates corresponding to the components listed in Table 1, weigh these components so that they reach 100 g after vitrification, and mix them uniformly, and use the obtained mixture as a glass preparation raw material. Then, put the raw material into a platinum crucible, heat it to 1000°C to 1400°C in an electric furnace to melt it, and stir it at appropriate times to achieve homogenization. Then, cast the homogenized melt into a preheated mold and slowly cool it in an electric furnace, thereby obtaining the optical glasses of Examples 1 to 14 and Comparative Examples 1 to 2, respectively.
[0093] Then, the refractive index (nd) and the degree of coloration (λ80) were measured for each optical glass. It should be noted that the refractive index (nd) was measured using the "KPR-200" manufactured by Kalnew Optical Industry Co., Ltd. In addition, the degree of coloration (λ80) was obtained by preparing a 10 mm thick optical glass sample that was polished on both sides and measuring the spectral transmittance including reflection loss using the "U-4100" manufactured by Hitachi High-Technologies Co., Ltd. and based on the wavelength at which the spectral transmittance shows 80%.
[0094] Table 1 shows the measurement results.
[0095]
[0096] As shown in Table 1, the compositions of the optical glasses of Examples 1 to 14 of the present invention are all within the above-specified ranges, so the refractive index (nd) is moderately high at 1.58 to 1.66, and the coloration degree (λ80) is 34 or less, indicating little coloration.
[0097] Industrial Applicability
[0098] Based on the present invention, it is possible to provide an optical glass that does not contain components that have an adverse effect on environmental load and is less colored while maintaining a moderately high refractive index. In addition, based on the present invention, it is possible to provide an optical element that uses the optical glass and is less colored while maintaining a moderately high refractive index.
[0099] The present invention also relates to the following technical solutions:
[0100] Item 1. An optical glass, characterized in that:
[0101] In mass %, including
[0102] SiO2 is 30% or more and 47% or less,
[0103] B2O3 is 0% or more and 10% or less,
[0104] Na2O is 3% or more and 12% or less,
[0105] Li2O is 0% or more and 5% or less,
[0106] CaO is 0% or more and 3.8% or less,
[0107] BaO is 28% or more and 43% or less,
[0108] ZnO is 3% or more and 16% or less,
[0109] ZrO2 is 0% or more and 8% or less,
[0110] The composition of La2O3 is 0% or more and 15% or less,
[0111] Wherein, the composition does not take into account the composition of Sb2O3;
[0112] Furthermore, PbO, As2O3 and K2O are not contained.
[0113] Item 2. The optical glass according to Item 1, wherein the refractive index nd is 1.58 to 1.66.
[0114] Item 3. The optical glass according to Item 1 or 2, wherein the coloring degree λ80 is 34 or less.
[0115] Item 4. The optical glass according to any one of Items 1 to 3, wherein a ratio of a BaO content in a total content of MgO, CaO, SrO, and BaO is 91 mass % or more.
[0116] Item 5. The optical glass according to any one of Items 1 to 4, wherein the optical glass does not contain MgO and SrO.
[0117] Item 6. The optical glass according to any one of Items 1 to 5, wherein the optical glass contains Sb 2 O 3 in an external proportion of 1 mass % or less.
[0118] Item 7. The optical glass according to any one of Items 1 to 6, wherein the optical glass is a core glass for an optical fiber.
[0119] Item 8. An optical element comprising the optical glass according to any one of Items 1 to 6.
Claims
1. An optical glass, characterized in that: In mass %, by containing only SiO2 is 30% or more and 44.13% or less, B2O3 is 0% or more and 10% or less, Na2O is 3% or more and 12% or less, Li2O is 0% or more and 5% or less, CaO is 0% or more and 3.8% or less, BaO is 28% or more and 43% or less, ZnO is 3% or more and 16% or less, ZrO2 is 0% or more and 8% or less, The composition is composed of La2O3 of 0% or more and 15% or less. Wherein, the composition does not take into account the composition of Sb2O3; The optical glass optionally contains one or more selected from GeO2, Y2O3, Gd2O3, Ga2O3 and In2O3, and optionally contains Sb2O3 in an external proportion of 1 mass % or less, Furthermore, it does not contain PbO, As2O3 and K2O; The optical glass has a coloration degree λ80 of 34 or less.
2. The optical glass according to claim 1, wherein: The refractive index nd is greater than or equal to 1.58 and less than or equal to 1.
66.
3. The optical glass according to claim 1 or 2, wherein: The ratio of the BaO content in the total content of CaO and BaO is 91 mass % or more.
4. The optical glass according to claim 1 or 2, wherein: The optical glass is core glass for optical fibers. An optical element comprising the optical glass according to any one of claims 1 to 4.
Citation Information
Patent Citations
Optical Glass And Optical Element
CN102372430A
Optical glass
CN103241941A
Highly transmissive glasses with high solarisation resistance, use thereof and method for production thereof
CN104039725A
Optical glass, optical glass blank, glass material for press molding use, optical element, and methods respectively for producing said products
CN104981439A
Optical glass, glass gob for press molding and optical device
JP2005179142A