High-weather-resistance colorless double-plating anti-reflection coated glass for photovoltaic module and preparation method of high-weather-resistance colorless double-plating anti-reflection coated glass
Through the double-layer anti-reflective film technology and the design of core-shell structure silicon sol, the blue problem of high weather resistance double-plating photovoltaic glass panels is solved, and the colorless and uniform coated glass is achieved, which improves the power generation efficiency and weather resistance of photovoltaic modules.
Patent Information
- Application Number
- CN202411120307.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-11-22
Smart Images

Figure CN118993567A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of glass processing, and relates to a highly weather-resistant colorless double-plated anti-reflection coated glass for photovoltaic modules and a preparation method thereof. Background Art
[0002] Against the backdrop of the rapid development of the global solar photovoltaic market, the pursuit of high-power solar crystalline silicon cells has never stopped. At the same time, solar panels are subdivided into different types according to different usage environments. Photovoltaic glass companies have also put forward demands for glass front panels such as colorless photovoltaics and offshore photovoltaics.
[0003] However, due to the relatively harsh marine environment, while paying attention to the weather resistance of the film surface, corresponding requirements are also put forward for the appearance of the battery cells; the conventional high-weather resistance double-coated photovoltaic glass panel film surface appears blue or light blue, so the photovoltaic glass front plate appears blue or light blue, and under the premise of high weather resistance, it is impossible to meet the use demand for colorless photovoltaic glass front plate; therefore, it is necessary to develop a method that can solve the blue or light blue problem of the anti-reflection film layer and achieve the colorless demand of the anti-reflection layer film surface.
[0004] Existing technical problems:
[0005] 1) Roller coating is the first choice for AR glass coating due to its advantages of high-speed automated operation, fast coating speed and high production efficiency. However, while roller coating brings us convenience in large-scale production, it also has some defects, such as fast solvent evaporation and easy change of coating viscosity during roller coating, which leads to messy evaporation marks on the coating surface; it not only affects the appearance, but also has a great impact on the overall performance.
[0006] 2) How to improve the weather resistance of solar photovoltaic modules while avoiding the problem of the film layer appearing blue or light blue.
[0007] 3) Production scale-up and processes that match the production workshop. Summary of the invention
[0008] The object of the present invention can be achieved through the following technical solutions: According to the production characteristics of photovoltaic glass, the present invention provides a method for preparing highly weather-resistant colorless double-coated anti-reflection coated glass for photovoltaic modules.
[0009] According to the thin film optical principle, the double-layer anti-reflection film technology is used to design and develop two anti-reflection film coating solutions with different refractive indices, which are successively coated on the solar photovoltaic glass to form a high anti-reflection coated glass with a gradient refractive index. The refractive index satisfies, where n0<n1<n2<n3 are the refractive indices of air, top film, bottom film, and glass respectively. By adjusting the refractive index of the bottom film and the top film to match, the photovoltaic anti-reflection glass can have a broadband anti-reflection effect in the spectral range of 380~1100nm, greatly improving the power generation efficiency of photovoltaic modules. At the same time, the bottom coating liquid is specially designed to form a dense film layer. The cationic silica sol and epoxy silane polymer work together to greatly enhance the bonding with the glass and can also play a role in bonding the top layer. The top layer is a core-shell structured silica sol, which is a mixture of large-particle cationic fluorinated silicone-acrylic emulsion and small-particle cationic styrene emulsion. The core-shell structured silica sol is obtained by reacting with a silicon source substance. The lower surface free energy of the fluorinated silicone-acrylic emulsion is utilized to make the core-shell silica sol with the silicone-acrylic emulsion as the core automatically tend to the surface during the film-forming process, thereby automatically forming an upper layer of core-shell structured silica layer mainly composed of large-particle size. The large-particle core-shell particles have a particle size larger than the film thickness, and will form micro-convexities on the surface of the film. This special structure is beneficial to global transmittance enhancement, and the transmittance curve is flatter, making the coated glass light in color and low in color difference.
[0010] The highly weather-resistant colorless double-plated anti-reflection coated glass for photovoltaic modules and the preparation method thereof comprise the following steps:
[0011] (1) Preparation of bottom layer high weather-resistant colorless film coating solution
[0012] 52g of tetraethyl silicate 40, 60g of isopropanol, 18g of water and 1g of glacial acetic acid were mixed evenly, hydrolyzed at room temperature for 48h, then heated to 80°C for reaction for 2h, and cooled to room temperature to obtain a silica prepolymer.
[0013] Add a certain amount of silica prepolymer, methyltrimethoxysilane, isopropanol, cationic silica sol, cationic surfactant, propylene glycol butyl ether, fluorosilane and aluminate coupling agent into a four-necked flask and mix evenly. The temperature automatically rises to 50°C due to heat release. Let it stand for 2 hours and naturally cool to room temperature. Add a certain amount of epoxy silane polymer, mix evenly, and finally dilute it with isopropanol to a solid content of 3-10% to obtain a bottom layer high weather-resistant colorless film coating solution.
[0014]
[0015] The innovation of the bottom anti-reflection coating liquid is the use of cationic silica sol, fluorosilane, aluminate coupling agent and epoxy silane polymer. It is the special physical properties (activity) of these four raw materials that strengthen the bonding between the bottom layer and the glass and between the bottom layer and the top layer. The aluminate coupling agent and fluorosilicone resin have excellent thermal stability and weather resistance, which makes the film layer not easy to fall off, making the double-layer highly weather-resistant colorless film of the present invention have stronger weather resistance than the existing double-layer film technology.
[0016] (2) Preparation of high weather-resistant colorless film coating solution of silica sol with core-shell structure 1. Preparation of fluorine-containing cationic silicone-acrylic emulsion
[0017] The fluorinated cationic silicone-acrylic emulsion is prepared by soap-free emulsion polymerization, and the steps are as follows:
[0018] (1) Methyl acrylate, methyl methacrylate, butyl acrylate, vinyl triethoxysilane, hexafluorobutyl methacrylate double-bond silane coupling agent, and dodecafluoroheptyl methacrylate are uniformly mixed to prepare a mixed monomer for later use;
[0019] (2) Adding a polymerizable cationic monomer and water into a four-necked flask, stirring to dissolve and disperse uniformly, then adding 1 / 4 to 1 / 3 of the above-mentioned mixed monomer and stirring at high speed to prepare a pre-emulsion;
[0020] The water bath was heated to 50-90°C and mechanically stirred at 150-200 rpm. After the temperature stabilized, part of the initiator 2,2'-azobis(2-methylpropionamidine) dihydrochloride (V-50) was added and reacted for a period of time. After the solution showed a blue glow, the remaining mixed monomers and the remaining initiator V-50 were added dropwise at the same time. The addition was completed within 3-4 hours. After the addition was completed, the reaction temperature was raised to 90°C and kept warm for 30-60 minutes to improve the conversion rate of the mixed monomers. Finally, the latex mixture was cooled to 40-50°C, the pH was adjusted to 1-2 with hydrochloric acid, and then filtered to remove the residual coagulant to obtain a cationic fluorinated silicone acrylic emulsion.
[0021] The double bond-containing silane coupling agent is one or more of γ-methacryloxypropyltrimethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, and 3-(methacryloxy)propyltrimethoxysilane;
[0022] The polymerizable cationic monomer is one or more of methacryloyloxyethyl trimethyl ammonium chloride, dimethyl diallyl ammonium chloride, acryloyloxyethyl trimethyl ammonium chloride, and methacryloyloxy-N,N-dimethyl-N-alkyl ammonium chloride.
[0023] 2. Preparation of cationic polystyrene emulsion
[0024] Cationic polystyrene emulsion was prepared by the method in reference patent CN105964195A.
[0025] 3. Preparation of coating solution
[0026] (1) mixing the above-mentioned fluorine-containing cationic silicone acrylic emulsion and cationic polystyrene emulsion in proportion and mixing them with a solvent;
[0027] (2) adding a silicon source material and reacting for 4 to 24 hours at 15 to 50° C. under stirring to obtain a core-shell structure silica sol;
[0028] (3) The core-shell structure silica sol is diluted to 3-10% with a solvent to obtain a highly weather-resistant colorless film coating solution.
[0029] The above-mentioned fluorine-containing cationic silicone acrylic emulsion accounts for 5-50% of the cationic polystyrene emulsion;
[0030] The average particle size of the fluorine-containing cationic silicone acrylic emulsion is 120 to 200 nm;
[0031] The particle size of the cationic polystyrene emulsion is 50 to 100 nm;
[0032] The above solvent is one or more of water, methanol, alcohol, isopropanol, ethylene glycol methyl ether, ethylene glycol butyl ether, propylene glycol methyl ether, propylene glycol butyl ether, N,N-dimethylformamide, N,N-dimethylacetamide, ethyl acetate, butyl acetate, propylene glycol methyl ether acetate, propylene glycol ethyl ether, xylene, and cyclohexanone;
[0033] 4. Preparation of coated glass
[0034] (1) After the bottom anti-reflection film coating liquid is coated in the first coating room, it enters the curing furnace for curing at a curing temperature of 60 to 250° C. and a curing time of 1 to 5 minutes to obtain glass coated with the bottom anti-reflection film;
[0035] (2) The top anti-reflection film coating liquid is roll-coated on the glass coated with the bottom anti-reflection film in the second coating room, and then baked and cured at 80-250° C., and then put into a tempering furnace and tempered at 500-700° C. to obtain a high anti-reflection coated glass with a gradient refractive index.
[0036] The invention introduces one or more auxiliary agents selected from the group consisting of leveling agent, auxiliary solvents ethylene glycol methyl ether, ethylene glycol butyl ether, propylene glycol methyl ether, propylene glycol butyl ether, N,N-dimethylformamide, N,N-dimethylacetamide, ethyl acetate, butyl acetate, propylene glycol methyl ether acetate, propylene glycol ethyl ether, xylene and cyclohexanone into the existing conventional double-plating technical route technical route formula system to modify it and improve the uniformity of the film surface; introduces weathering modifiers such as cationic silica sol, fluorosilane, aluminate coupling agent and epoxy silane polymer to improve the adhesion and weather resistance of the film layer; adjusts the thickness and refractive index of the bottom layer and the surface layer, and combines the local production process to achieve colorless and uniform coated glass.
[0037] In the preparation process of silica sol in the bottom coating liquid, at least one of the weathering modifiers fluorosilane, aluminate coupling agent, silane coupling agent, acrylic resin, epoxy resin, trifluoroethylene-vinyl ester copolymer and isocyanate is introduced; in the preparation of silica sol in the core-shell structure of the surface layer, at least one of the modification aids N,N-dimethylformamide, N,N-dimethylacetamide, ethyl acetate, butyl acetate, propylene glycol methyl ether, propylene glycol methyl ether acetate, propylene glycol ethyl ether, xylene and cyclohexanone is introduced to modify the uniformity of the film surface, and the same weathering modifier as the bottom layer is introduced; the core-shell structure silica sol is prepared. The thickness and refractive index of the bottom and surface layers are adjusted to achieve a colorless film surface.
[0038] The technical problem to be solved by the present invention is to invent a highly weather-resistant colorless double-plated anti-reflection coated glass for photovoltaic modules and a preparation method thereof, so as to improve the weather resistance and colorlessness of the film surface.
[0039] 1) Provided are a highly weather-resistant colorless double-plated anti-reflection coated glass for photovoltaic modules and a preparation method thereof.
[0040] 2) Improve the quality of coated glass products.
[0041] 3) Increase profits by developing differentiated products while keeping costs unchanged. BRIEF DESCRIPTION OF THE DRAWINGS
[0042] Figure 1 This is the Lab color model diagram of the film surface. DETAILED DESCRIPTION
[0043] The following are specific embodiments of the present invention and the accompanying drawings to further describe the technical solution of the present invention, but the present invention is not limited to these embodiments.
[0044] According to the thin film optical principle, the double-layer anti-reflection film technology is used to design and develop two anti-reflection film coating solutions with different refractive indices, which are successively coated on the solar photovoltaic glass to form a high anti-reflection coated glass with a gradient refractive index. The refractive index satisfies, where n0<n1<n2<n3 are the refractive indices of air, top film, bottom film, and glass respectively. By adjusting the refractive index of the bottom film and the top film to match, the photovoltaic anti-reflection glass can have a broadband anti-reflection effect in the spectral range of 380~1100nm, greatly improving the power generation efficiency of photovoltaic modules. At the same time, the bottom coating liquid is specially designed to form a dense film layer. The cationic silica sol and epoxy silane polymer work together to greatly enhance the bonding with the glass and can also play a role in bonding the top layer. The top layer is a core-shell structured silica sol, which is a mixture of large-particle cationic fluorinated silicone-acrylic emulsion and small-particle cationic styrene emulsion. The core-shell structured silica sol is obtained by reacting with a silicon source substance. The lower surface free energy of the fluorinated silicone-acrylic emulsion is utilized to make the core-shell silica sol with the silicone-acrylic emulsion as the core automatically tend to the surface during the film-forming process, thereby automatically forming an upper layer of core-shell structured silica layer mainly composed of large-particle size. The large-particle core-shell particles have a particle size larger than the film thickness, and will form micro-convexities on the surface of the film. This special structure is beneficial to global transmittance enhancement, and the transmittance curve is flatter, making the coated glass light in color and low in color difference.
[0045] The highly weather-resistant colorless double-plated anti-reflection coated glass for photovoltaic modules and the preparation method thereof comprise the following steps:
[0046] (1) Preparation of bottom layer high weather-resistant colorless film coating solution
[0047] 52g of tetraethyl silicate 40, 60g of isopropanol, 18g of water and 1g of glacial acetic acid were mixed evenly, hydrolyzed at room temperature for 48h, then heated to 80°C for reaction for 2h, and cooled to room temperature to obtain a silica prepolymer.
[0048] Add a certain amount of silica prepolymer, methyltrimethoxysilane, isopropanol, cationic silica sol, cationic surfactant, propylene glycol butyl ether, fluorosilane and aluminate coupling agent into a four-necked flask and mix evenly. The temperature automatically rises to 50°C due to heat release. Let it stand for 2 hours and naturally cool to room temperature. Add a certain amount of epoxy silane polymer, mix evenly, and finally dilute it with isopropanol to a solid content of 3-10% to obtain a bottom layer high weather-resistant colorless film coating solution.
[0049]
[0050] The innovation of the bottom anti-reflection coating liquid is the use of cationic silica sol, fluorosilane, aluminate coupling agent and epoxy silane polymer. It is the special physical properties (activity) of these four raw materials that strengthen the bonding between the bottom layer and the glass and between the bottom layer and the top layer. The aluminate coupling agent and fluorosilicone resin have excellent thermal stability and weather resistance, which makes the film layer not easy to fall off, making the double-layer highly weather-resistant colorless film of the present invention have stronger weather resistance than the existing double-layer film technology.
[0051] (2) Preparation of high weather-resistant colorless film coating solution of silica sol with core-shell structure 1. Preparation of fluorine-containing cationic silicone acrylic emulsion
[0052] The fluorinated cationic silicone-acrylic emulsion is prepared by soap-free emulsion polymerization, and the steps are as follows:
[0053] (1) Methyl acrylate, methyl methacrylate, butyl acrylate, vinyl triethoxysilane, hexafluorobutyl methacrylate double-bond silane coupling agent, and dodecafluoroheptyl methacrylate are uniformly mixed to prepare a mixed monomer for later use;
[0054] (2) Adding a polymerizable cationic monomer and water into a four-necked flask, stirring to dissolve and disperse uniformly, then adding 1 / 4 to 1 / 3 of the above-mentioned mixed monomer and stirring at high speed to prepare a pre-emulsion;
[0055] The water bath was heated to 50-90°C and mechanically stirred at 150-200 rpm. After the temperature stabilized, part of the initiator 2,2'-azobis(2-methylpropionamidine) dihydrochloride (V-50) was added and reacted for a period of time. After the solution showed a blue glow, the remaining mixed monomers and the remaining initiator V-50 were added dropwise at the same time. The addition was completed within 3-4 hours. After the addition was completed, the reaction temperature was raised to 90°C and kept warm for 30-60 minutes to improve the conversion rate of the mixed monomers. Finally, the latex mixture was cooled to 40-50°C, the pH was adjusted to 1-2 with hydrochloric acid, and then filtered to remove the residual coagulant to obtain a cationic fluorinated silicone acrylic emulsion.
[0056] The double bond-containing silane coupling agent is one or more of γ-methacryloxypropyltrimethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, and 3-(methacryloxy)propyltrimethoxysilane;
[0057] The polymerizable cationic monomer is one or more of methacryloyloxyethyl trimethyl ammonium chloride, dimethyl diallyl ammonium chloride, acryloyloxyethyl trimethyl ammonium chloride, and methacryloyloxy-N,N-dimethyl-N-alkyl ammonium chloride.
[0058] 2. Preparation of cationic polystyrene emulsion
[0059] Cationic polystyrene emulsion was prepared by referring to the method in patent CN105964195A.
[0060] 3. Preparation of coating solution
[0061] (1) mixing the above-mentioned fluorine-containing cationic silicone acrylic emulsion and cationic polystyrene emulsion in proportion and mixing them with a solvent;
[0062] (2) adding a silicon source material and reacting for 4 to 24 hours at 15 to 50° C. under stirring to obtain a core-shell structure silica sol;
[0063] (3) The core-shell structure silica sol is diluted to 3-10% with a solvent to obtain a highly weather-resistant colorless film coating solution.
[0064] The above-mentioned fluorine-containing cationic silicone acrylic emulsion accounts for 5-50% of the cationic polystyrene emulsion;
[0065] The average particle size of the fluorine-containing cationic silicone acrylic emulsion is 120 to 200 nm;
[0066] The particle size of the cationic polystyrene emulsion is 50 to 100 nm;
[0067] The above solvent is one or more of water, methanol, alcohol, isopropanol, ethylene glycol methyl ether, ethylene glycol butyl ether, propylene glycol methyl ether, propylene glycol butyl ether, N,N-dimethylformamide, N,N-dimethylacetamide, ethyl acetate, butyl acetate, propylene glycol methyl ether acetate, propylene glycol ethyl ether, xylene, and cyclohexanone;
[0068] 5. Preparation of coated glass
[0069] (1) After the bottom anti-reflection film coating liquid is coated in the first coating room, it enters the curing furnace for curing at a curing temperature of 60 to 250° C. and a curing time of 1 to 5 minutes to obtain glass coated with the bottom anti-reflection film;
[0070] (2) The top anti-reflection film coating liquid is roll-coated on the glass coated with the bottom anti-reflection film in the second coating room, and then baked and cured at 80-250° C., and then put into a tempering furnace and tempered at 500-700° C. to obtain a high anti-reflection coated glass with a gradient refractive index.
[0071] The invention introduces one or more auxiliary agents selected from the group consisting of leveling agent, auxiliary solvents ethylene glycol methyl ether, ethylene glycol butyl ether, propylene glycol methyl ether, propylene glycol butyl ether, N,N-dimethylformamide, N,N-dimethylacetamide, ethyl acetate, butyl acetate, propylene glycol methyl ether acetate, propylene glycol ethyl ether, xylene and cyclohexanone into the existing conventional double-plating technical route technical route formula system to modify it and improve the uniformity of the film surface; introduces weathering modifiers such as cationic silica sol, fluorosilane, aluminate coupling agent and epoxy silane polymer to improve the adhesion and weather resistance of the film layer; adjusts the thickness and refractive index of the bottom layer and the surface layer, and combines the local production process to achieve colorless and uniform coated glass.
[0072] Detection performance:
[0073] 1) Film color difference measurement: ΔE≤1.5, a value: -0.5~0.5, b value: -2~0.5; the appearance is colorless, such as Figure 1 As shown;
[0074] 2) The light transmittance reaches 93.90% to 94.20%, the curve has no obvious peaks, no monochromatic light reflection, and good continuous production stability;
[0075] 3) Strengthened weathering test: Referring to the national standard GB / T30984.1-2015, the constant temperature and humidity can exceed the national standard by 5 times, reaching more than 5000h (the national standard is 1000h); the wet-freeze performance exceeds the national standard by 14 times, reaching more than 3360h (the national standard is 240h); the ultraviolet radiation can exceed the national standard by 9 times, reaching more than 135KW.h (the national standard is 15KW.h); the salt spray can exceed the national standard by 7 times, reaching more than 672h (the national standard is 96h); the PCT can exceed the national standard by 1.5 times, reaching 72h (the national standard is 48h); the transmittance change value after the test ΔT≤1%.
[0076]
[0077]
[0078]
[0079]
[0080] The specific embodiments described herein are merely examples of the spirit of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in similar ways, but they will not deviate from the spirit of the present invention or exceed the scope defined by the appended claims.
Claims
1. A method for preparing highly weather-resistant colorless double-coated anti-reflection coated glass for photovoltaic modules, characterized in that: The steps include: 1) Preparation of bottom layer high weather-resistant colorless film coating solution 52g of tetraethyl silicate 40, 60g of isopropanol, 18g of water and 1g of glacial acetic acid were mixed evenly, hydrolyzed at room temperature for 48h, then heated to 80°C for reaction for 2h, and cooled to room temperature to obtain a silica prepolymer; Add a certain amount of silica prepolymer, methyltrimethoxysilane, isopropanol, cationic silica sol, cationic surfactant, propylene glycol butyl ether, fluorosilane, and aluminate coupling agent into a four-necked flask and mix evenly. The temperature automatically rises to 50°C due to heat release, and the temperature is naturally cooled to room temperature for 2 hours. A certain amount of epoxy silane oligomer is added and mixed evenly. Finally, the solid content is diluted with isopropanol to 3-10%, and the bottom layer high weather-resistant colorless film coating solution is obtained. 2) Preparation of top core-shell structure silica sol highly weather-resistant colorless film coating solution Preparation of Fluorinated Cationic Silicone-Acrylic Emulsion The fluorinated cationic silicone-acrylic emulsion is prepared by soap-free emulsion polymerization, and the steps are as follows: (1) Methyl acrylate, methyl methacrylate, butyl acrylate, vinyl triethoxysilane, hexafluorobutyl methacrylate double-bond silane coupling agent, and dodecafluoroheptyl methacrylate are uniformly mixed to prepare a mixed monomer for later use; (2) Adding a polymerizable cationic monomer and water into a four-necked flask, stirring to dissolve and disperse uniformly, then adding 1 / 4 to 1 / 3 of the above-mentioned mixed monomer and stirring at high speed to prepare a pre-emulsion; The water bath is heated to 50-90°C, and mechanical stirring is performed at 150-200 rpm. After the temperature stabilizes, a portion of the initiator 2,2'-azobis(2-methylpropionamidine) dihydrochloride (V-50) is added, and the reaction is continued for a period of time. After the solution emits a blue light, the remaining mixed monomers and the remaining initiator V-50 are added dropwise at the same time, and the addition is completed within 3-4 hours. After the addition is completed, the reaction temperature is raised to 90°C and the reaction is kept warm for 30-60 minutes to improve the conversion rate of the mixed monomers. Finally, the latex mixture is cooled to 40-50°C, the pH is adjusted to 1-2 with hydrochloric acid, and then filtered to remove the residual coagulant to obtain a cationic fluorinated silicone acrylic emulsion; Preparation of Cationic Polystyrene Emulsion Cationic polystyrene emulsion was prepared by referring to the method in patent CN105964195A; Coating solution preparation (1) mixing the above-mentioned fluorine-containing cationic silicone acrylic emulsion and cationic polystyrene emulsion in proportion and mixing them with a solvent; (2) adding a silicon source material and reacting for 4 to 24 hours at 15 to 50° C. under stirring to obtain a core-shell structure silica sol; (3) diluting the core-shell structure silica sol to 3-10% with a solvent to obtain a highly weather-resistant colorless film coating solution; Coated glass preparation (1) After the bottom anti-reflection film coating liquid is coated in the first coating room, it enters the curing furnace for curing at a curing temperature of 60 to 250° C. and a curing time of 1 to 5 minutes to obtain glass coated with the bottom anti-reflection film; (2) The top anti-reflection film coating liquid is roll-coated on the glass coated with the bottom anti-reflection film in the second coating room, and then baked and cured at 80-250° C., and then put into a tempering furnace and tempered at 500-700° C. to obtain a high anti-reflection coated glass with a gradient refractive index.
2. The method for preparing a highly weather-resistant colorless double-coated anti-reflection coated glass for photovoltaic modules according to claim 1, characterized in that: The double bond-containing silane coupling agent is one or more of γ-methacryloxypropyltrimethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, and 3-(methacryloxy)propyltrimethoxysilane.
3. The method for preparing a highly weather-resistant colorless double-coated anti-reflection coated glass for photovoltaic modules according to claim 1, characterized in that: The polymerizable cationic monomer is one or more of methacryloyloxyethyl trimethyl ammonium chloride, dimethyl diallyl ammonium chloride, acryloyloxyethyl trimethyl ammonium chloride, and methacryloyloxy-N,N-dimethyl-N-alkyl ammonium chloride.
4. The method for preparing a highly weather-resistant colorless double-coated anti-reflection coated glass for photovoltaic modules according to claim 1, characterized in that: The fluorine-containing cationic silicone acrylic emulsion accounts for 5 to 50% of the cationic polystyrene emulsion.
5. The method for preparing a highly weather-resistant colorless double-coated anti-reflection coated glass for photovoltaic modules according to claim 1, characterized in that: The average particle size of the fluorinated cationic silicone acrylic emulsion is 120-200nm.
6. The method for preparing a highly weather-resistant colorless double-coated anti-reflection coated glass for photovoltaic modules according to claim 1, characterized in that: The particle size of cationic polystyrene emulsion is 50-100nm.
7. The method for preparing highly weather-resistant colorless double-coated anti-reflection coated glass for photovoltaic modules according to claim 1, characterized in that: The solvent is one or more of water, methanol, alcohol, isopropanol, ethylene glycol methyl ether, ethylene glycol butyl ether, propylene glycol methyl ether, propylene glycol butyl ether, N,N-dimethylformamide, N,N-dimethylacetamide, ethyl acetate, butyl acetate, propylene glycol methyl ether acetate, propylene glycol ethyl ether, xylene, and cyclohexanone.
Citation Information
Patent Citations
Nanometer core-shell silicon dioxide microsphere as well as preparation and application of antireflection composite coating solution
CN105964195A
Weather-proof double-layer high-antireflection coated glass and preparation method thereof
CN111362589A
Hydrophobic coating liquid, glass and preparation method thereof
CN113930155A
Film coating liquid capable of reducing chromatic aberration, preparation method and application of film coating liquid in photovoltaic glass
CN114621639A
Method of manufacturing highly durable waterdrop slidable coating film
JP2004250253A
Cited By
Tempering corrosion-resistant colored coated glass and preparation process thereof
CN119371115A
A tempered corrosion-resistant colored coated glass and its preparation process
CN119371115B
High-transmittance coating liquid as well as preparation method and application thereof
CN121427037A
Nanometer core-shell particle and preparation method thereof, anti-reflection coating liquid and application of anti-reflection coating liquid
CN121610017A