Low-carbon cement prepared by quality-divided gradient utilization of large mixing amount of coal gasification ash and preparation method of low-carbon cement

By using coal gasified ash slag, high carbon ash slag powder and medium carbon ash slag to replace fuel and raw materials, and by activating and treating high ash slag micro powder, the gasified ash slag is difficult to utilize on a large scale in the cement industry. The problem has achieved efficient resource utilization and low-carbon cement production.

CN118993587APending Publication Date: 2024-11-22TIANJIN CEMENT IND DESIGN & RES INST CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411021274.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

It is difficult to achieve large-scale utilization of coal gasified ash slag in the cement industry. Due to its physical and chemical characteristics of materials, it leads to a decline in the mechanical properties of cement, and landfill or storage causes environmental pollution and waste of resources.

Method used

Use the material-divided cascade to use coal gasified ash slag, use a large amount of high-carbon ash slag powder instead of coal powder as fuel, medium carbon ash slag instead of cement raw materials, and treat high-ash ash slag micro powder through ultrafine activation, thermal activation and chemical activation to prepare Low-carb cement.

Benefits of technology

The comprehensive utilization rate of coal gasified ash slag has been achieved by more than 60%, and the performance indicators have reached the 42.5-strength cement quality requirements, which has reduced production costs and carbon emission intensity, and saved natural resources.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118993587A_ABST
    Figure CN118993587A_ABST
Patent Text Reader

Abstract

The invention provides low-carbon cement prepared by high mixing amount of coal gasification ash and a preparation method of the low-carbon cement. The low-carbon cement comprises the following components: 95-113 parts of low-carbon clinker, 5-7 parts of desulfurized gypsum and 80-100 parts of multi-field activated high-ash ash micro powder. The high-carbon ash slag is used as fuel to calcine the cement raw material powder composed of the mixture of the medium-carbon ash slag and other cement raw material powder to obtain the low-carbon clinker, and the activated high-ash ash slag micro powder is used as a low-carbon cement component, so that a large amount of coal gasification ash slag is utilized in the low-carbon cement production process, the utilization rate of the coal gasification ash slag is increased, and the production cost is reduced. The production cost is reduced, natural resources such as limestone and clay are saved, and the carbon emission strength of the cement is greatly reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of resource utilization of solid waste, and more specifically to a low-carbon cement prepared by utilizing a large amount of coal gasification ash in a quality-differentiated and tiered manner and a preparation method thereof. Background Art

[0002] Coal gasification technology is the pillar industry of modern coal chemical industry and the main way to use coal cleanly and efficiently. Coal gasification ash is a by-product of the coal gasification process. At present, the treatment and disposal of coal gasification ash in my country is still mainly landfill or slag storage, and large-scale industrial application has not yet been achieved. Single landfill or storage will not only occupy land resources, but also cause environmental pollution and waste of resources. Therefore, there is an urgent need for large-scale and resource-based utilization of coal gasification ash.

[0003] Applying coal gasification ash to cement industry is one of the effective ways to realize large-scale resource utilization of coal gasification ash. The basic components of coal gasification ash include residual carbon and ash components. Among them, the residual carbon component has a higher calorific value and can be used as an alternative fuel for cement clinker burning; the chemical composition of the ash component is mainly CaO, SiO2, Al2O3 and Fe2O3, which can be used as a raw material or admixture for cement clinker burning. However, due to the physical and chemical characteristics of the coexistence of carbon and ash components in coal gasification ash, there are still the following problems when it is used in the cement industry:

[0004] (1) The residual carbon content in coal gasification ash is usually 15% to 20%, and the calorific value is 600 to 900 kcal / kg, which is much lower than the fuel used in traditional cement clinker burning (4500 to 6000 kcal / kg). As a result, the fuel replacement rate of coal gasification ash in the cement clinker burning process is very limited, usually not exceeding 10%.

[0005] (2) If coal gasification ash is used as an admixture to replace clinker in cement, the excessively high residual carbon content will increase the water demand of cement and weaken the matrix bonding interface. In addition, CaO, SiO2, and Al2O3 in the ash of coal gasification ash exist in the form of inert aluminosilicate polymers with high polymerization degree and poor reaction activity. The above reasons together lead to a sharp decrease in the mechanical properties of cement when coal gasification ash is used as a cement admixture to replace clinker as the amount of coal gasification ash increases.

[0006] It can be seen that the resource utilization of coal gasification ash in the cement industry, whether it is an alternative fuel or an alternative raw material, is limited by the physical and chemical properties of coal gasification ash and is difficult to achieve large-scale utilization. Therefore, it is urgent to develop a new route for the graded utilization of coal gasification ash to maximize the fuel and raw material properties of its carbon and ash components, and to achieve the preparation of low-carbon cement with all components and large amounts of coal gasification ash, which is of great significance for promoting the green, low-carbon and sustainable development of modern coal chemical industry and cement industry. Summary of the invention

[0007] In view of the above problems, the present invention provides a method for preparing low-carbon cement by utilizing coal gasification ash in a large amount in a graded and tiered manner, which is used to solve the problem in the prior art that it is difficult to utilize all components and large amounts of coal gasification ash in the production of cement.

[0008] The invention provides a low-carbon cement prepared by using coal gasification ash in a high-volume manner in a quality-differentiated and tiered manner. The low-carbon cement comprises 95 to 113 parts of low-carbon clinker, 5 to 7 parts of desulfurized gypsum, and 80 to 100 parts of multi-field activated high-ash ash powder.

[0009] Optionally, the low carbon clinker is obtained by calcining medium carbon ash composite raw material powder using high carbon ash powder obtained by grinding high carbon ash as fuel; the high carbon ash is coal gasification ash with a carbon content greater than or equal to 75%.

[0010] Optionally, the medium carbon ash composite raw material powder is obtained by mixing and homogenizing medium carbon ash, calcium raw material, silicon aluminum raw material and silicon correction raw material according to component one and then grinding them; the medium carbon ash is coal gasification ash with a carbon content of 25% to 35%.

[0011] Optionally, the component one includes: 170-180 parts of calcium raw material, 1-3 parts of silicon-aluminum raw material, 10-14 parts of silicon correction raw material, and 8-12 parts of medium carbon ash.

[0012] Optionally, the calcium raw material includes limestone, chalk, and carbide slag;

[0013] The silicon-alumina raw materials include clay, shale and fly ash;

[0014] The siliceous correction raw materials include sandstone, siltstone and diatomaceous earth.

[0015] Optionally, in the high carbon ash powder, R80μm is less than 10% and moisture is less than 1%.

[0016] Optionally, in the medium carbon ash slag composite raw meal powder, R80μm<30%, R200μm<2%, and moisture<1%.

[0017] Optionally, the calcination temperature is 1400-1500°C.

[0018] Optionally, the high-ash slag powder is prepared from high-ash slag by ultrafine activation, thermal activation and chemical activation; Optionally, the specific surface area of ​​the multi-field activated high-ash slag powder is 700-900 m 2 / kg.

[0019] The present invention also provides a method for preparing low-carbon cement by using coal gasification ash in a high-volume blending manner. The low carbon cement described in this application comprises the following steps:

[0020] Step 1, classifying the coal gasification ash to obtain high carbon ash with a carbon content greater than or equal to 75%, medium carbon ash with a carbon content greater than or equal to 25% and less than or equal to 35%, and high ash with a carbon content less than or equal to 8%;

[0021] Step 2, the medium carbon ash slag, calcium raw material, silicon aluminum raw material and silicon correction raw material are mixed and homogenized according to component one, and then ground to obtain medium carbon ash slag composite raw material powder; the high carbon ash slag is ground to obtain high carbon ash slag powder;

[0022] Step 3, using the high-carbon ash powder as fuel, calcining the medium-carbon ash composite raw material powder into low-carbon clinker;

[0023] Step 4: the low carbon clinker and desulfurized gypsum are mixed and homogenized according to the second component, and then ground to obtain low carbon clinker-gypsum mixed powder; the high ash slag is subjected to ultrafine activation, thermal activation and chemical activation to obtain multi-field activated high ash slag powder;

[0024] Step 5: Evenly mix the low-carbon clinker-gypsum mixed powder and the multi-field activated high-ash slag powder according to the three components to obtain low-carbon cement.

[0025] Optionally, in step 4, the ultrafine activation, thermal activation and chemical activation of the high-ash slag include:

[0026] Step 41, high-ash ash raw materials are fed into the steam kinetic energy mill in the step-by-step pulverizing zone, and at the same time, superheated steam airflow enters the steam kinetic energy mill in the step-by-step pulverizing zone through the steam inlet, and the airflow drives the high-ash ash to pass through the primary pulverizing chamber and the secondary pulverizing chamber in sequence for pulverization, and then the airflow drives the pulverized fine materials to enter the ultrafine powder classifier through the discharge pipe of the steam kinetic energy mill in the step-by-step pulverizing zone for sorting, and the materials within the target particle size enter the thermal activation system from the top air outlet of the ultrafine powder classifier;

[0027] Step 42, the material entering the thermal activation system is preheated by the multi-stage cyclone preheater and enters the suspension furnace. At the same time, high-temperature hot air is introduced into the suspension furnace, and the temperature in the suspension furnace is controlled at the target temperature. The high-temperature hot air carries the material from bottom to top in the suspension furnace for full thermal activation, and then enters the final cyclone preheater from the air outlet at the top of the suspension furnace for gas-solid separation; the material after gas-solid separation enters the chemical activation system;

[0028] Step 43, the material entering the chemical activation system is cooled by heat exchange in the multi-stage cyclone cooler, and then enters the mixer from the outlet of the final cyclone cooler, and cooling air is introduced into the mixer for mixing; the cooling air discharged from the mixer enters the multi-stage cyclone cooler, and the temperature of the material when entering the mixer is below 100°C; while the material enters the mixer, a chemical activator is quantitatively added to the mixer, so that the material and the chemical activator are evenly mixed in the mixer to obtain a finished material.

[0029] Optionally, in step 4, the second component includes: 95-113 parts of low-carbon clinker and 5-7 parts of desulfurized gypsum; the surface area of ​​the low-carbon clinker-gypsum mixed powder is 400-450m 2 / kg.

[0030] Optionally, in step 5, the component three includes: 100 to 120 parts of low-carbon clinker-gypsum mixed powder and 80 to 100 parts of multi-field activated high-ash slag powder.

[0031] The present invention has at least the following beneficial effects:

[0032] (1) The low-carbon cement prepared by the present invention using coal gasification ash in a high-volume blending method can achieve a comprehensive utilization rate of coal gasification ash of more than 60%, and all performance indicators meet the quality requirements of 42.5 strength grade cement.

[0033] (2) The present invention uses high-carbon ash powder to completely replace coal powder as fuel for burning low-carbon cement clinker, thereby significantly reducing the production cost of low-carbon cement.

[0034] (3) The present invention uses high-quality and step-by-step coal gasification ash to prepare low-carbon cement, and uses medium-carbon ash to partially replace the raw materials for low-carbon cement burning, thereby saving natural resources such as limestone and clay.

[0035] (4) The low-carbon cement prepared by the present invention is prepared by using a large amount of coal gasification ash in a graded manner, and high-ash ash powder activated in multiple fields is used as an active admixture. Its replacement rate for clinker reaches 40% to 50%, which greatly reduces the carbon emission intensity of cement. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0037] Figure 1 A diagram of a high-ash slag activation system provided in an embodiment of the present invention.

[0038] Reference numerals:

[0039] 1. Waste heat boiler; 2. Fan A; 3. Regulating valve; 4. Steam kinetic energy mill in cascade crushing area; 4a. Discharging pipe; 4b. Secondary crushing chamber; 4c. Primary crushing chamber; 4d. Recovery bin; 5. Ultrafine powder classifier; 6. First-stage cyclone preheater; 7. Second-stage cyclone preheater; 8. Secondary-final cyclone preheater; 9. Final cyclone preheater; 10. Suspension furnace; 11. Fan B; 12. Fan C; 13. Dust collector; 14. Tail exhaust fan; 15. Chimney; 16. First-stage cyclone cooler; 17. Final cyclone cooler; 18. Mixer; 19. Chemical activator storage bin; 20. Fan D; 21. Cooling fan; 22. Conveying chute; 23. Finished product warehouse; 24. Kiln head grate cooler; 25. Rotary kiln. DETAILED DESCRIPTION

[0040] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0041] The invention provides a low-carbon cement prepared by using coal gasification ash in a high-volume manner in a quality-differentiated and tiered manner. The low-carbon cement comprises 95 to 113 parts of low-carbon clinker, 5 to 7 parts of desulfurized gypsum, and 80 to 100 parts of multi-field activated high-ash ash powder.

[0042] Specifically, the components of low-carbon cement include low-carbon clinker, desulfurized gypsum and multi-field activated high-ash ash powder. In the preparation process of low-carbon cement, high-carbon ash with a carbon content of greater than or equal to 75% in the gasification ash is used as calcination fuel, and the calcination fuel is used to calcine the cement raw material powder composed of a mixture of medium-carbon ash with a carbon content of 25% to 35% in the gasification ash and other cement raw material powders; the desulfurized gypsum in this application is desulfurized gypsum that complies with GB / T 21371 "Industrial Reproduction Gypsum for Cement". High-ash ash powder is obtained by activating gasification ash with a carbon content of less than or equal to 8%. A large amount of gasification ash is used in the entire low-carbon cement preparation process. On the premise that all performance indicators meet the quality requirements of 42.5 strength grade cement, the production cost is reduced, natural resources such as limestone and clay are saved, and the carbon emission intensity of cement is greatly reduced.

[0043] In a possible implementation, the low carbon clinker is obtained by calcining medium carbon ash composite raw meal powder using high carbon ash powder obtained by grinding high carbon ash as fuel; the high carbon ash is coal gasification ash with a carbon content greater than or equal to 75%.

[0044] Specifically, through the coal gasification ash separation technology, the high carbon ash with a carbon content of 75% or more is used as a fuel for calcining raw meal powder in the cement production process, and the medium carbon ash composite raw meal powder is used as a raw material for cement clinker production, and the medium carbon ash composite raw meal powder is calcined into low carbon clinker by burning the high carbon ash. In this application, the calorific value of the high carbon ash is not less than 5300kcal / kg.

[0045] In a possible implementation, the medium carbon ash composite raw material powder is obtained by mixing and homogenizing medium carbon ash, calcium raw material, silicon aluminum raw material and silicon correction raw material according to component one and then grinding them; the medium carbon ash is coal gasification ash with a carbon content of 25% to 35%.

[0046] Specifically, the medium carbon ash composite raw material powder includes medium carbon ash, calcium raw materials, silicon-aluminum raw materials and silicon correction raw materials. Among them, the medium carbon ash is an industrial waste and also contains chemical components that can be used in cement production, such as silicates and other oxides. The calcium raw materials mainly provide calcium oxide, which is the main active ingredient in cement; the silicon-aluminum raw materials are used to provide silicates and aluminates, which are important components that react with calcium oxide to form cementitious materials; the silicon correction raw materials adjust the silicon dioxide content in the raw materials to ensure the balance of chemical components. The chemical composition of the medium carbon ash includes: carbon content 25% to 35%, CaO ≥ 10%, SiO2 ≥ 30%, Al2O3 ≥ 8%, Fe2O3 ≥ 10%, MgO < 3%, alkali content < 1.2%.

[0047] In a possible implementation, the component one includes: 170-180 parts of calcium raw material, 1-3 parts of silicon-aluminum raw material, 10-14 parts of silicon correction raw material, and 8-12 parts of medium carbon ash.

[0048] In a possible implementation, the calcium raw material includes limestone, chalk, and carbide slag;

[0049] The silicon-alumina raw materials include clay, shale and fly ash;

[0050] The siliceous correction raw materials include sandstone, siltstone and diatomaceous earth.

[0051] Specifically, the calcium raw materials include but are not limited to limestone, chalk, carbide slag, etc., and the chemical composition of the calcium raw materials includes: CaO ≥ 45%, MgO < 3%, and alkali content < 0.4%.

[0052] Silica-alumina raw materials include but are not limited to clay, shale, fly ash, etc. The chemical composition of the silica-alumina raw materials should meet the following requirements: SiO2≥40%, Al2O3≥30%, and alkali content<1.2%.

[0053] Siliceous correction raw materials include but are not limited to sandstone, siltstone, diatomaceous earth, etc. The chemical composition of the siliceous correction raw materials should meet the following requirements: SiO2 ≥ 80%, alkali content < 1.2%.

[0054] In a possible implementation manner, in the high carbon ash powder, R80 μm is less than 10% and moisture is less than 1%.

[0055] In a possible implementation manner, in the medium carbon ash slag composite raw meal powder, R80 μm is less than 30%, R200 μm is less than 2%, and moisture is less than 1%.

[0056] In one possible implementation, the calcination temperature is 1400-1500°C.

[0057] Specifically, calcining at a high temperature of 1400-1500°C helps to improve the combustion efficiency of the fuel and achieve energy saving. Preferably, the calcining temperature is 1450°C.

[0058] In a possible implementation, the high-ash ash powder is prepared from high-ash ash by ultrafine activation, thermal activation and chemical activation; the high-ash ash is coal gasification ash with a carbon content of less than or equal to 8%.

[0059] Specifically, ultrafine activation refers to grinding high-ash slag to reduce its particle size and significantly increase the specific surface area of ​​high-ash slag, thereby improving its chemical reactivity and physical activity. Thermal activation refers to the fact that during the heating process of high-ash slag, certain substances inside it will undergo physical or chemical changes, such as crystal structure transformation and chemical bond breaking. These changes increase the specific surface area of ​​the slag and increase the number of surface active sites, thereby improving its reactivity and application value. In addition, during the thermal activation process, the color of the high-ash slag will also change, turning into a gray color that is easily accepted by the public. Chemical activation refers to mixing a chemical activator directly with high-ash slag, and then performing appropriate treatment (such as stirring, grinding, etc.) to allow the activator to fully contact and react with the slag. The chemical activator reacts chemically with certain components in the slag, resulting in changes in the structure, morphology or surface properties of the slag.

[0060] The carbon content of high-ash slag is ≤8%, and f-CaO is ≤0.5%. f-CaO refers to calcium oxide that exists in a free state. When the content exceeds a certain amount, it will have an adverse effect on the performance of the produced cement. Therefore, controlling the content of f-CaO is crucial to ensuring the quality and stability of cement.

[0061] In a possible embodiment, the specific surface area of ​​the multi-field activated high-ash ash powder is 700-900m 2 / kg, and the 28d activity index is ≥90%. When the multi-field activated high-ash slag powder is mixed with cement, after 28 days of standard curing, its compressive strength reaches 90% or more compared with the pure cement mortar test block. This high activity index shows that the high-ash slag powder can effectively ensure the strength and durability of concrete when mixed with other cement components.

[0062] The present invention provides a method for preparing low-carbon cement by utilizing coal gasification ash in a large amount in a quality-differentiated and stepwise manner, comprising the following steps:

[0063] Step 1: Classify the coal gasification ash into high carbon ash with a carbon content greater than or equal to 75%, medium carbon ash with a carbon content greater than or equal to 25% and less than or equal to 35%, and high ash with a carbon content less than or equal to 8%.

[0064] Step 2, the medium carbon ash slag, calcium raw material, silicon aluminum raw material and silicon correction raw material are mixed and homogenized according to component one, and then ground to obtain medium carbon ash slag composite raw material powder; the high carbon ash slag is ground to obtain high carbon ash slag powder;

[0065] Step 3, using the high-carbon ash powder as fuel, calcining the medium-carbon ash composite raw material powder into low-carbon clinker;

[0066] Step 4: the low carbon clinker and desulfurized gypsum are mixed and homogenized according to the second component, and then ground to obtain low carbon clinker-gypsum mixed powder; the high ash slag is subjected to ultrafine activation, thermal activation and chemical activation to obtain multi-field activated high ash slag powder;

[0067] Step 5: Evenly mix the low-carbon clinker-gypsum mixed powder and the multi-field activated high-ash slag powder according to the three components to obtain low-carbon cement.

[0068] Specifically, step 1, based on the coal gasification ash carbon ash separation and sorting technology, the coal gasification ash discharged from the factory is separated to separate high carbon ash with a carbon content ≥75%, medium carbon ash with a carbon content greater than or equal to 25% and less than or equal to 35%, and high ash ash with a carbon content ≤8%. In this application, the separated, step 2, according to component one, respectively weigh the corresponding number of medium carbon ash, calcium raw material, silicon aluminum raw material and silicon correction raw material, mix them evenly, and then use a grinding equipment to grind them to achieve the particle size and moisture content requirements that can ensure the quality and performance of cement production, and obtain medium carbon ash composite raw material powder.

[0069] Step 3: Use the separated high-carbon ash with a carbon content greater than or equal to 75% as fuel for calcining raw meal powder in the cement production process, and use the medium-carbon ash composite raw meal powder obtained in step 2 as a raw material for cement clinker production, and calcine the medium-carbon ash composite raw meal powder into low-carbon clinker by burning the high-carbon ash.

[0070] Step 4: Weigh low-carbon clinker and desulfurized gypsum according to a certain component ratio, mix and homogenize, and then grind the mixture to obtain a low-carbon clinker-gypsum mixed powder with a particle size and moisture content that meets the quality and performance of cement production.

[0071] The high-ash slag is activated in multiple fields to produce high-ash slag powder. The multiple field activation process includes three parts, namely ultrafine activation, thermal activation and chemical activation.

[0072] Step 5: Mechanically mix the low-carbon clinker-gypsum mixed powder and the multi-field activated high-ash slag powder evenly according to component three to obtain a graded low-carbon cement prepared by using a large amount of coal gasification slag.

[0073] The comprehensive utilization rate of coal gasification ash in the process of preparing low-carbon cement by the method of the present invention reaches more than 60%, and the low-carbon cement meets the quality requirements of 42.5 strength grade cement.

[0074] In a possible implementation, in step 4, the ultrafine activation, thermal activation and chemical activation of the high-ash slag include:

[0075] Step 41, high-ash ash raw materials are fed into the steam kinetic energy mill 4 in the step-by-step pulverizing area, and at the same time, superheated steam airflow enters the steam kinetic energy mill 4 in the step-by-step pulverizing area through the steam inlet, and the airflow drives the high-ash ash to pass through the primary pulverizing chamber 4c and the secondary pulverizing chamber 4b in sequence for pulverization, and then the airflow drives the pulverized fine materials to enter the ultrafine powder classifier 5 through the discharge pipe 4a of the steam kinetic energy mill 4 in the step-by-step pulverizing area for sorting, and the materials within the target particle size enter the thermal activation system from the top air outlet of the ultrafine powder classifier 5;

[0076] Step 42, the material entering the thermal activation system is preheated by the multi-stage cyclone preheater and enters the suspension furnace 10, and at the same time, high-temperature hot air is introduced into the suspension furnace 10, and the temperature in the suspension furnace 10 is controlled at the target temperature. The high-temperature hot air carries the material from bottom to top in the suspension furnace 10 for full thermal activation, and then enters the final cyclone preheater 9 from the top air outlet of the suspension furnace 10 for gas-solid separation; the material after gas-solid separation enters the chemical activation system;

[0077] Step 43, the material entering the chemical activation system is cooled by heat exchange in the multi-stage cyclone cooler, and then enters the mixer 18 from the outlet of the final cyclone cooler 17, and the cooling air is introduced into the mixer 18 for mixing; the cooling air discharged from the mixer 18 enters the multi-stage cyclone cooler, and the temperature of the material when entering the mixer 18 is below 100° C. At the same time as the material enters the mixer 18, a chemical activator is quantitatively added to the mixer 18, so that the material and the chemical activator are evenly mixed in the mixer 18 to obtain a finished material.

[0078] Specifically, according to the material direction:

[0079] Step 1, high-ash coal gasification ash raw materials enter the steam kinetic energy mill 4 in the step-by-step crushing area, and are crushed in turn through the primary crushing chamber 4c and the secondary crushing chamber 4b, and then enter the ultra-fine powder classifier 5 through the discharge pipe 4a through the top shrinkage of the steam kinetic energy mill 4 in the step-by-step crushing area. During the process, the materials with larger particles in the crushing chamber enter the recovery bin 4d of the steam kinetic energy mill 4 in the step-by-step crushing area, are discharged through the bottom flap valve, and re-enter the steam kinetic energy mill 4 in the step-by-step crushing area through the feed port conveying chute 22 for re-crushing. After the materials enter the ultra-fine powder classifier 5, the materials with qualified particle size enter the thermal activation system with the airflow from the top outlet of the ultra-fine powder classifier 5, and the materials with unqualified particle size are discharged from the bottom outlet of the ultra-fine powder classifier 5 and re-enter the steam kinetic energy mill 4 in the step-by-step crushing area for crushing.

[0080] Step 2: After the material enters the thermal activation system, it is preheated in sequence by the first-stage cyclone preheater 6 to the second-stage cyclone preheater 8 in the multi-stage preheater, and then enters the suspension furnace 10 from the bottom feed port of the suspension furnace 10. The material moves from bottom to top in the suspension furnace 10, enters the final cyclone preheater 9 from the top outlet of the suspension furnace 10, and enters the chemical activation system from the bottom outlet of the final cyclone preheater 9 after gas-solid separation. The carbon content of the material after thermal activation is less than 1%, and the color is gray.

[0081] Step 3, after the material enters the chemical activation system, it passes through the first-stage cyclone cooler 16 to the final-stage cyclone cooler 17 in the multi-stage cyclone cooler in sequence, and performs heat exchange cooling with the cooling air in the system step by step, and then enters the mixer 18 from the bottom discharge port of the final-stage cyclone cooler 17. The temperature of the material when entering the mixer 18 is below 100°C. When the material enters the mixer 18, at the same time, the chemical activator storage bin 19 quantitatively adds the chemical activator to the mixer 18, and the material and the chemical activator are cooled, mixed and activated in the mixing chamber of the mixer 18, and then enter the conveying chute 22 from the bottom discharge port of the mixer 18 and are transported to the finished product warehouse 23 for storage.

[0082] According to the direction of air flow:

[0083] Step 1, kiln head grate cooler 24 is connected to the kiln head of rotary kiln 25. The hot air in the low temperature zone of cement kiln head grate cooler 24 is introduced into AQC waste heat boiler 1 through fan A2, and the superheated steam generated enters the waste heat power generation system one way, and passes through regulating valve 3 through the high pressure nozzle of steam kinetic energy mill 4 in step crushing area to form high-speed airflow in the crushing chamber of steam kinetic energy mill 4 in step crushing area, driving the material to accelerate impact, collision, friction and crushing in the crushing chamber. The airflow in steam kinetic energy mill 4 in step crushing area carries the crushed material through discharge pipe 4a of steam kinetic energy mill 4 in step crushing area and enters superfine powder classifier 5.

[0084] Step 2, the airflow carries the qualified particle size materials from the top outlet of the ultrafine powder concentrator 5 into the first-stage cyclone preheater 6 of the thermal activation system. After the gas and solid are separated in the first-stage cyclone preheating, the airflow is introduced into the dust collector 13 through the fan C12 from the top outlet of the first-stage cyclone preheater 6. After filtering and dust removal, the airflow is discharged from the chimney 15 through the tail exhaust fan 14. The hot air in the medium temperature zone of the cement kiln head grate cooler 24 is introduced into the suspension furnace 10 from the bottom air inlet of the suspension furnace 10 through the fan B11, and moves from bottom to top in the suspension furnace 10 carrying the preheated materials. After the materials are fully thermally activated, they are discharged from the top outlet of the suspension furnace 10 into the final cyclone preheater 9. The hot air from the suspension furnace 10 carries the heat-activated material, and after gas-solid separation in the final cyclone preheater 9, it enters the first-stage cyclone preheater 6 from the top outlet of the final cyclone preheater 9 through the next-final cyclone preheater 8 and the second-stage cyclone preheater 7 in sequence. In the process, the material is preheated by heat exchange with the counter-flowing material step by step, and then enters the dust collector 13 from the top outlet of the first-stage cyclone preheater 6 through the fan C12, and is discharged from the chimney 15 through the tail exhaust fan 14 after filtering and dust removal.

[0085] Step 3, the cooling fan 21 introduces cooling air into the mixer 18 from the lower air inlet of the mixer 18, fully cools and mixes the materials and chemical activators in the mixing chamber of the mixer 18, and then enters the multi-stage cyclone cooler in sequence from the top air outlet of the mixer 18. In the process, the materials are cooled by heat exchange with the materials flowing in the reverse direction step by step. The top air outlet of the first-stage cyclone cooler 16 passes the hot air after heat exchange in the multi-stage cyclone cooler into the multi-stage cyclone preheater through the fan D20.

[0086] In a possible implementation, the second component includes: 95-113 parts of low-carbon clinker and 5-7 parts of desulfurized gypsum; the surface area of ​​the low-carbon clinker-gypsum mixed powder is 400-450m 2 / kg.

[0087] In a possible implementation, in step 5, component three includes: 100-120 parts of low-carbon clinker-gypsum mixed powder and 80-100 parts of multi-field activated high-ash slag powder.

[0088] The present invention is further illustrated by the following examples.

[0089] Embodiment 1:

[0090] In parts by weight, weigh 170 parts of calcium raw material, 3 parts of silicon-aluminum raw material, 10 parts of silicon correction raw material, and 8 parts of medium carbon ash. Mix and homogenize the raw materials and grind them together to R 80μm <30%、R 200μm <2%, moisture<1%, and medium carbon ash slag composite raw material powder is obtained.

[0091] Grind the high carbon ash to R80μm The high carbon ash powder is prepared by calcining the medium carbon ash composite raw material powder at 1450℃ with the high carbon ash powder as fuel to obtain low carbon clinker.

[0092] Weigh 95 parts of low-carbon clinker and 5 parts of desulfurized gypsum by weight, mix and homogenize them, and grind them together to a specific surface area of ​​450m 2 / kg, low carbon clinker-gypsum mixed powder was obtained. Another 100 parts of the specific surface area after multi-field activation was 900m 2 / kg of multi-field activated high-ash slag powder is mechanically mixed evenly with low-carbon clinker-gypsum mixed powder to produce a graded low-carbon cement prepared with a large amount of coal gasification ash.

[0093] Embodiment 2:

[0094] In parts by weight, weigh 180 parts of calcium raw material, 1 part of silicon-aluminum raw material, 14 parts of silicon correction raw material, and 12 parts of medium carbon ash. Mix and homogenize the raw materials and grind them together to R 80μm <30%、R 200μm <2%, moisture<1%, and medium carbon ash slag composite raw material powder is obtained.

[0095] Grind the high carbon ash to R 80μm The high carbon ash powder is prepared by calcining the medium carbon ash composite raw material powder at 1450℃ with the high carbon ash powder as fuel to obtain low carbon clinker.

[0096] Weigh 95 parts of low-carbon clinker and 5 parts of desulfurized gypsum by weight, mix and homogenize them, and grind them together to a specific surface area of ​​450m 2 / kg, low carbon clinker-gypsum mixed powder was obtained. Another 100 parts of the specific surface area after multi-field activation was 900m 2 / kg of multi-field activated high-ash slag powder is mechanically mixed evenly with low-carbon clinker-gypsum mixed powder to produce a graded low-carbon cement prepared with a large amount of coal gasification ash.

[0097] Embodiment 3:

[0098] In parts by weight, weigh 175 parts of calcium raw material, 2 parts of silicon-aluminum raw material, 12 parts of silicon correction raw material, and 10 parts of medium carbon ash. Mix and homogenize the raw materials and grind them together to R 80μm <30%、R 200μm <2%, moisture<1%, and medium carbon ash slag composite raw material powder is obtained.

[0099] Grind the high carbon ash to R 80μmThe high carbon ash powder is prepared by calcining the medium carbon ash composite raw material powder at 1450℃ with the high carbon ash powder as fuel to obtain low carbon clinker.

[0100] In parts by weight, 105 parts of low carbon clinker and 6 parts of desulfurized gypsum were weighed, the two were mixed and homogenized, and then ground together to a specific surface area of ​​400m 2 / kg, low carbon clinker-gypsum mixed powder was obtained. Another 90 parts were weighed and activated in multiple fields to obtain a specific surface area of ​​700m 2 / kg of multi-field activated high-ash slag powder is mechanically mixed evenly with low-carbon clinker-gypsum mixed powder to produce a graded low-carbon cement prepared with a large amount of coal gasification ash.

[0101] Embodiment 4:

[0102] In parts by weight, weigh 180 parts of calcium raw material, 1 part of silicon-aluminum raw material, 14 parts of silicon correction raw material, and 12 parts of medium carbon ash. Mix and homogenize the raw materials and grind them together to R 80μm <30%、R 200μm <2%, moisture<1%, and medium carbon ash slag composite raw material powder is obtained.

[0103] Grind the high carbon ash to R 80μm The high carbon ash powder is prepared by calcining the medium carbon ash composite raw material powder at 1450℃ with the high carbon ash powder as fuel to obtain low carbon clinker.

[0104] In parts by weight, 113 parts of low carbon clinker and 7 parts of desulfurized gypsum were weighed, mixed and homogenized, and then ground together to a specific surface area of ​​400m 2 / kg, low carbon clinker-gypsum mixed powder was obtained. Another 80 parts were weighed and the specific surface area was 700m 2 / kg of multi-field activated high-ash slag powder is mechanically mixed evenly with low-carbon clinker-gypsum mixed powder to produce a graded low-carbon cement prepared with a large amount of coal gasification ash.

[0105] Embodiment 5:

[0106] In parts by weight, weigh 170 parts of calcium raw material, 3 parts of silicon-aluminum raw material, 14 parts of silicon correction raw material, and 8 parts of medium carbon ash. Mix and homogenize the raw materials and grind them together to R 80μm <30%、R 200μm <2%, moisture<1%, and medium carbon ash slag composite raw material powder is obtained.

[0107] Grind the high carbon ash to R 80μm The high carbon ash powder is prepared by calcining the medium carbon ash composite raw material powder at 1450℃ with the high carbon ash powder as fuel to obtain low carbon clinker.

[0108] In parts by weight, 113 parts of low carbon clinker and 7 parts of desulfurized gypsum were weighed, mixed and homogenized, and then ground together to a specific surface area of ​​450m 2 / kg, low carbon clinker-gypsum mixed powder was obtained. Another 80 parts were weighed and the specific surface area after multi-field activation was 900m 2 / kg of multi-field activated high-ash slag powder is mechanically mixed evenly with low-carbon clinker-gypsum mixed powder to produce a graded low-carbon cement prepared with a large amount of coal gasification ash.

[0109] Embodiment 6:

[0110] In parts by weight, weigh 180 parts of calcium raw material, 1 part of silicon-aluminum raw material, 10 parts of silicon correction raw material, and 12 parts of medium carbon ash. Mix and homogenize the raw materials and grind them together to R 80μm <30%、R 200μm <2%, moisture<1%, and medium carbon ash slag composite raw material powder is obtained.

[0111] Grind the high carbon ash to R 80μm The high carbon ash powder is prepared by calcining the medium carbon ash composite raw material powder at 1450℃ with the high carbon ash powder as fuel to obtain low carbon clinker.

[0112] Weigh 95 parts of low-carbon clinker and 5 parts of desulfurized gypsum by weight, mix and homogenize them, and grind them together to a specific surface area of ​​450m 2 / kg, low carbon clinker-gypsum mixed powder was obtained. Another 100 parts of the specific surface area after multi-field activation was 900m 2 / kg of multi-field activated high-ash slag powder is mechanically mixed evenly with low-carbon clinker-gypsum mixed powder to produce a graded low-carbon cement prepared with a large amount of coal gasification ash.

[0113] Comparative Example:

[0114] The comparative example is PO42.5 ordinary Portland cement that complies with GB175-2023 "General Portland Cement".

[0115] The cement in Examples 1 to 6 and the comparative example was tested for performance. The 3d and 28d flexural and compressive strengths of the cement were tested according to GB / T17671-2021 "Test Method for Cement Mortar Strength (ISO Method)", and the standard consistency water requirement, setting time and stability of the cement were tested according to GB / T1346-2011 "Test Method for Standard Consistency Water Consumption, Setting Time and Stability of Cement". The test results are shown in Table 1.

[0116] Table 1 Performance data of low carbon cement

[0117]

[0118] As shown in Table 1, the low-carbon cement prepared by using a large amount of coal gasification ash in the quality-separated cascade in the present invention has a 3d compressive strength of 17.7-21.8MPa and a 28d compressive strength of 43.6-46.6MPa. Its mechanical properties meet the mechanical property requirements for 42.5 strength grade cement in GB175-2023 "General Portland Cement", and the initial setting time, final setting time and volume stability are all qualified. The low-carbon cement prepared by using a large amount of coal gasification ash in the quality-separated cascade in the present invention greatly reduces the cement production cost and carbon emission intensity, while realizing the large-scale resource utilization of coal gasification ash, with significant environmental and economic benefits.

[0119] Although the preferred embodiments of the present invention have been described, those skilled in the art may make other changes and modifications to these embodiments once they have learned the basic creative concept. Therefore, the appended claims are intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of the present invention.

[0120] Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.

Claims

1. A low-carbon cement prepared by using coal gasification ash in large quantities in a graded and graded manner. It is characterized in that The low-carbon cement comprises 95-113 parts of low-carbon clinker, 5-7 parts of desulfurized gypsum, and 80-100 parts of multi-field activated high-ash ash powder.

2. According to claim 1, a low-carbon cement prepared by using coal gasification ash in a high-volume blending method. It is characterized in that The low-carbon clinker is prepared by calcining medium-carbon ash composite raw material powder using high-carbon ash powder obtained by grinding high-carbon ash as fuel; the high-carbon ash is coal gasification ash with a carbon content greater than or equal to 75%.

3. The low carbon cement prepared by using coal gasification ash in a high amount in a quality-differentiated and graded manner according to claim 2, It is characterized in that The medium carbon ash composite raw material powder is prepared by mixing and homogenizing medium carbon ash, calcium raw material, silicon aluminum raw material and silicon correction raw material according to component one and then grinding them; the medium carbon ash is coal gasification ash with a carbon content of 25% to 35%.

4. The low carbon cement prepared by using high-quality graded coal gasification ash as claimed in claim 3, It is characterized in that The first component comprises: 170-180 parts of calcium raw material, 1-3 parts of silicon-aluminum raw material, 10-14 parts of silicon correction raw material, and 8-12 parts of medium carbon ash.

5. The low carbon cement prepared by using coal gasification ash in a high amount in a quality-differentiated and graded manner according to claim 4, It is characterized in that The calcium raw materials include limestone, chalk and carbide slag; The silicon-alumina raw materials include clay, shale and fly ash; The siliceous correction raw materials include sandstone, siltstone and diatomaceous earth.

6. The low carbon cement prepared by using high-quality graded coal gasification ash as claimed in claim 2, It is characterized in that In the high carbon ash powder, R80μm is less than 10% and moisture is less than 1%.

7. The low carbon cement prepared by using high-quality graded coal gasification ash as claimed in claim 2, It is characterized in that In the medium carbon ash slag composite raw meal powder, R80μm is less than 30%, R200μm is less than 2%, and moisture is less than 1%.

8. The low carbon cement prepared by using high-quality graded coal gasification ash as claimed in claim 2, It is characterized in that The calcination temperature is 1400-1500°C.

9. The low carbon cement prepared by using high-quality graded coal gasification ash as claimed in claim 1, It is characterized in that The high-ash ash powder is prepared from high-ash ash by ultrafine activation, thermal activation and chemical activation; the high-ash ash is coal gasification ash with a carbon content of less than or equal to 8%.

10. The low carbon cement prepared by using high-quality graded coal gasification ash as claimed in claim 1, It is characterized in that The specific surface area of ​​the multi-field activated high-ash slag powder is 700-900m 2 / kg.

11. A method for preparing low-carbon cement by using coal gasification ash in large quantities in a step-by-step manner. It is characterized in that The method for preparing the low carbon cement according to any one of claims 1 to 10 comprises the following steps: Step 1, classifying the coal gasification ash to obtain high carbon ash with a carbon content greater than or equal to 75%, medium carbon ash with a carbon content greater than or equal to 25% and less than or equal to 35%, and high ash with a carbon content less than or equal to 8%; Step 2, the medium carbon ash slag, calcium raw material, silicon aluminum raw material and silicon correction raw material are mixed and homogenized according to component one, and then ground to obtain medium carbon ash slag composite raw material powder; the high carbon ash slag is ground to obtain high carbon ash slag powder; Step 3, using the high-carbon ash powder as fuel, calcining the medium-carbon ash composite raw material powder into low-carbon clinker; Step 4, mixing and homogenizing the low carbon clinker and desulfurized gypsum according to component 2, and then grinding to obtain low carbon clinker-gypsum mixed powder; The high-ash slag is subjected to ultrafine activation, thermal activation and chemical activation to obtain multi-field activated high-ash slag micro powder; Step 5: Evenly mix the low-carbon clinker-gypsum mixed powder and the multi-field activated high-ash slag powder according to the three components to obtain low-carbon cement.

12. A method for preparing low carbon cement by using coal gasification ash in a high-volume blending method according to claim 11, It is characterized in that In step 4, the ultrafine activation, thermal activation and chemical activation of the high-ash slag include: Step 41, high-ash ash raw materials are fed into the steam kinetic energy mill in the step-by-step pulverizing zone, and at the same time, superheated steam airflow enters the steam kinetic energy mill in the step-by-step pulverizing zone through the steam inlet, and the airflow drives the high-ash ash to pass through the primary pulverizing chamber and the secondary pulverizing chamber in sequence for pulverization, and then the airflow drives the pulverized fine materials to enter the ultrafine powder classifier through the discharge pipe of the steam kinetic energy mill in the step-by-step pulverizing zone for sorting, and the materials within the target particle size enter the thermal activation system from the top air outlet of the ultrafine powder classifier; Step 42, the material entering the thermal activation system is preheated by the multi-stage cyclone preheater and enters the suspension furnace. At the same time, high-temperature hot air is introduced into the suspension furnace, and the temperature in the suspension furnace is controlled at the target temperature. The high-temperature hot air carries the material from bottom to top in the suspension furnace for full thermal activation, and then enters the final cyclone preheater from the air outlet at the top of the suspension furnace for gas-solid separation; the material after gas-solid separation enters the chemical activation system; Step 43, the material entering the chemical activation system is cooled by heat exchange in the multi-stage cyclone cooler, and then enters the mixer from the outlet of the final cyclone cooler, and cooling air is introduced into the mixer for mixing; the cooling air discharged from the mixer enters the multi-stage cyclone cooler, and the temperature of the material when entering the mixer is below 100°C; while the material enters the mixer, a chemical activator is quantitatively added to the mixer, so that the material and the chemical activator are evenly mixed in the mixer to obtain a finished material.

13. The method for preparing low carbon cement by using coal gasification ash in a high amount in a quality-differentiated and step-by-step manner according to claim 11, It is characterized in that In step 4, the second component includes: 95-113 parts of low-carbon clinker and 5-7 parts of desulfurized gypsum; the surface area of ​​the low-carbon clinker-gypsum mixed powder is 400-450m 2 / kg.

14. The method for preparing low carbon cement by using coal gasification ash in a high amount in a quality-differentiated and stepwise manner according to claim 11, It is characterized in that In step 5, the component three includes: 100 to 120 parts of low-carbon clinker-gypsum mixed powder and 80 to 100 parts of multi-field activated high-ash slag powder.

Citation Information

Cited By

  • Multi-source solid waste low-carbon cement based on graded gradient utilization of coal gasification slag and preparation method of multi-source solid waste low-carbon cement

    CN122212517A