A high-homogeneity, high-fluidity recycled aggregate concrete and preparation method thereof

Through the aggregate density adjustment technology, the problem of poor fluidity and homogeneity of regenerated aggregate concrete is solved, and the regenerated aggregate concrete with large flowability and high uniformity is achieved, ensuring the appearance quality and strength stability of the concrete, solving the problem of the solution. There are significant economic and environmental benefits to natural gravel shortages and construction waste pollution problems.

CN117756474BActive Publication Date: 2024-11-26CHINA CONSTRUCTION WESTERN CONSTRUCTION GROUP NO 8 (SHANGHAI) CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311783346.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-22
Publication Date
2024-11-26
Estimated Expiration
2043-12-22

AI Technical Summary

Technical Problem

There are problems with existing recycled aggregate concrete in terms of fluidity and homogeneity, resulting in rapid slump loss of concrete and difficult to meet construction requirements. Moreover, some of the recycled aggregates float after pouring large flow concrete, resulting in the appearance of concrete. Poor quality and strength stability.

Method used

Adopting aggregate density adjustment technology, the combination of modified regenerated aggregate and aggregate density adjustment slurry is suppressed to suppress the floating of small-particle regenerated aggregate, and achieve the homogeneity of regenerated aggregate concrete with large flowability of 100% regenerated aggregate, ensuring hardening. The appearance quality and strength stability of recycled aggregate concrete. The specific methods include preparing aggregate density adjustment slurry, fully stirring the regenerated aggregate and gelled material, adding modified regenerated aggregate and water reducing agent after dry mixing, to improve the flowability and mechanical properties of the concrete.

Benefits of technology

Effectively inhibit the floating of small-particle regenerated aggregate, improve the homogeneity of concrete mixture, ensure the appearance quality and strength stability of hardened regenerated aggregate concrete, and achieve efficient utilization of 100% regenerated aggregate, solving the problem of The shortage of natural gravel and construction waste pollution have great economic, environmental and social benefits.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004624379510000021
    Figure BDA0004624379510000021
  • Figure BDA0004624379510000121
    Figure BDA0004624379510000121
Patent Text Reader

Abstract

The present invention relates to a highly homogeneous and highly fluid recycled aggregate concrete and a preparation method thereof. The raw materials of the concrete per cubic meter include the following components: 350-400 kg of cementitious material, 450-550 kg of modified recycled aggregate, 500-600 kg of recycled aggregate, 700-800 kg of machine-made sand, 3.5-5 kg ​​of water reducer, and 160-180 kg of mixing water, wherein the modified recycled aggregate is modified by aggregate density adjustment slurry. The present invention comprehensively considers the difference in apparent density of recycled aggregates with different particle sizes, adopts aggregate density adjustment technology, effectively inhibits the floating of recycled aggregates with small particle sizes, realizes the homogeneity of highly fluid 100% recycled aggregate concrete mixture, and ensures the appearance quality and strength stability of hardened recycled aggregate concrete.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of concrete materials, and in particular to a highly homogeneous and highly fluid recycled aggregate concrete and a preparation method thereof. Background Art

[0002] At present, my country is still in a period of massive construction. On the one hand, new buildings need to consume a large amount of sand and gravel aggregates; on the other hand, a large number of old buildings are demolished, generating an astonishing amount of construction solid waste. The large accumulation of construction waste will bring about many problems such as land waste and environmental pollution. New application methods of construction waste are urgently needed to achieve sustainable development of the construction industry. The promotion and application of recycled aggregate concrete technology can fundamentally solve a series of problems such as the serious shortage of natural resources such as sand and stone and the environmental pollution caused by construction waste, and has great social, environmental and economic benefits.

[0003] However, there are still many technical bottlenecks in the preparation of high-fluidity concrete using 100% recycled aggregate to replace natural aggregate and apply it in the engineering field. For example: (1) The addition of recycled aggregate will cause the concrete to lose slump quickly, and the working performance will be difficult to meet the construction requirements; (2) After the high-fluidity concrete is poured, some aggregates in the recycled aggregate concrete will float up, causing problems such as poor concrete appearance quality and strength stability. This is because recycled aggregate has lower density, higher porosity, water absorption and crushing index than natural aggregate. Residual attached mortar is the main factor affecting the properties of recycled aggregate such as density, porosity, water absorption and crushing value. The particle size of recycled aggregate has a great influence on water absorption. The smaller the particle size, the greater the water absorption capacity. Because the smaller the particle size, the larger the specific surface area, and the greater the attached mortar content.

[0004] Based on this, in order to obtain recycled aggregate concrete with good working performance and high homogeneity, many researchers have carried out a lot of experimental work. In terms of mix design, appropriately increasing the amount of water reducer used in preparing concrete can improve the fluidity of concrete to a certain extent, but the state of the concrete mixture is limited by the sensitivity of the water reducer and time, and the concrete segregation and bleeding problems often occur within 30 minutes, and the concrete fluidity deteriorates within 1 to 2 hours. Alternatively, adding a thickener can change the plastic viscosity and yield stress of the paste, increase the anti-dispersion of each component of the material, and improve the stability of each component of the concrete mixture. However, the effect of the thickener is not easy to control, resulting in the concrete mixture losing its large flow characteristics. This method has not fundamentally solved the problem of concrete workability and homogeneity. In the strengthening treatment of recycled aggregate, the hardened cement mortar attached to the surface of the recycled aggregate is mainly removed by mechanical force, or the surface and microcracks of the recycled aggregate are treated with a certain active slurry or chemical reagent. Although the quality of recycled aggregates can be improved to a certain extent, thereby improving the performance of concrete, these methods are cumbersome to operate, require special equipment for grinding or long-term chemical immersion treatment, have a long cycle, and will greatly increase production costs, pollute the environment, and are difficult to meet the needs of large-scale concrete production. In terms of mixing technology, by adopting secondary or even tertiary mixing methods, the performance of concrete mixtures can be guaranteed, the aggregate-mortar interface can be improved, and the bonding strength of the interface transition zone can be increased. However, it has not fundamentally solved the uniformity problems such as the floating of large-flow recycled aggregate concrete. Summary of the invention

[0005] The purpose of the present invention is to provide a highly homogeneous and highly fluid recycled aggregate concrete and a preparation method thereof, so as to solve the problems of poor fluidity and homogeneity of recycled aggregate concrete. The present invention comprehensively considers the difference in apparent density of recycled aggregates of different particle sizes, adopts aggregate density adjustment technology, effectively suppresses the floating of small-size recycled aggregates, realizes the homogeneity of highly fluid 100% recycled aggregate concrete mixture, and ensures the appearance quality and strength stability of hardened recycled aggregate concrete.

[0006] The purpose of the present invention can be achieved by the following technical solutions:

[0007] A highly homogeneous and highly fluid recycled aggregate concrete, wherein the raw materials of each cubic meter of the concrete include the following components:

[0008]

[0009] The modified recycled aggregate is obtained by modifying the recycled aggregate with an aggregate density regulating slurry. The modified recycled aggregate contains recycled aggregate inside, and the recycled aggregate outside is attached with hardened aggregate density regulating slurry to prevent small-size aggregate from floating.

[0010] Furthermore, the gelling material comprises the following components by mass percentage:

[0011] Cement 60-80%,

[0012] Fly ash 10-25%,

[0013] Mineral powder 10-15%.

[0014] Furthermore, in the above, the cement is 42.5 grade ordinary Portland cement, the fly ash is grade II fly ash, and the mineral powder is S95 mineral powder.

[0015] Furthermore, the aggregate density adjusting slurry, based on 100 parts by weight, consists of the following components: 30-40 parts of aggregate density adjusting material, 20-30 parts of hardening material, 0.3-0.5 parts of dispersant, and the balance is water.

[0016] In the above, the aggregate density adjusting material is iron ore powder, the fineness of which is less than 10% on a 0.15 mm sieve, and the apparent density is 5000-6000 kg / m 3 .

[0017] Furthermore, in the above, the hardening material is cement, and the cement is 42.5 grade ordinary Portland cement.

[0018] Furthermore, the dispersant is a polycarboxylic acid high performance water reducing agent with a solid content of 40% and a water reducing rate of not less than 30%.

[0019] Furthermore, the particle size of the modified recycled aggregate is 5 to 10 mm, and the particle size of the recycled aggregate is 10 to 25 mm.

[0020] Furthermore, the mixed recycled aggregate composed of the modified recycled aggregate and the recycled aggregate is Class II recycled aggregate or above, with a particle size of 5 to 25 mm and continuous grading.

[0021] Furthermore, the machine-made sand has a fineness modulus of 2.6 to 3.2, an MB value of less than 1.0, and a stone powder content of 4 to 8%.

[0022] Furthermore, the water reducing agent is a polycarboxylic acid high-performance water reducing agent with a solid content of 15% and a water reduction rate of not less than 25%.

[0023] In addition, the present invention also provides a method for preparing highly homogeneous and highly fluid recycled aggregate concrete, the specific steps of which are as follows:

[0024] S1. preparing aggregate density adjustment slurry;

[0025] S2, after fully stirring the 5-10 mm recycled aggregate in the aggregate density adjustment slurry, the slurry liquid is separated and hardened in water to obtain 5-10 mm modified recycled aggregate;

[0026] S3, adding 10-25 mm recycled aggregate and cementitious material in sequence, dry mixing until uniform, to obtain a stirred mixture A;

[0027] S4, adding a portion of mixing water and the 5-10 mm modified recycled aggregate obtained in step S2 to the mixed material A obtained in step S3, stirring until uniform, to obtain a stirred mixed material B;

[0028] S5. Add a water reducing agent, machine-made sand and the remaining mixing water to the mixture B obtained in step S4 and stir to obtain a highly homogeneous and highly fluid recycled aggregate concrete.

[0029] Furthermore, in step S1, the specific steps of preparing the aggregate density adjustment slurry are as follows:

[0030] 30-40 parts of aggregate density adjusting material, 20-30 parts of hardening material, 0.3-0.5 parts of dispersant and the balance of water are fully stirred and mixed to obtain aggregate density adjusting slurry.

[0031] Furthermore, in step S2, the mass ratio of the 5-10 mm recycled aggregate to the aggregate density adjustment slurry is 1:(0.5-1).

[0032] Furthermore, in step S2, the stirring time is 3 to 5 minutes, and the hardening water curing time is 1 to 3 days.

[0033] Furthermore, in step S3, the dry mixing time is 10 to 20 seconds.

[0034] Furthermore, in step S4, the stirring time is 20 to 30 seconds.

[0035] Furthermore, in step S5, the stirring time is 60 to 90 seconds.

[0036] Furthermore, the volume ratio of the mixing water added in step S4 to the mixing water added in step S5 is 2:1.

[0037] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0038] (1) The present invention utilizes the difference in apparent density of recycled aggregates of different particle sizes. The recycled aggregates of 5 to 10 mm with a smaller apparent density are first subjected to aggregate density adjustment pretreatment technology to obtain 5 to 10 mm modified recycled aggregates with an apparent density close to that of original aggregates. The modified recycled aggregates are then combined with 10 to 25 mm recycled aggregates with an apparent density close to that of original aggregates to form a 5 to 25 mm continuously graded aggregate. This solves the problem of small-size aggregates with a smaller apparent density floating in a high-fluidity 100% recycled aggregate concrete mixture, thereby improving the homogeneity of the concrete mixture.

[0039] (2) The present invention gives full play to the role of aggregate in concrete and solves the problem of large discreteness of strength of recycled aggregate concrete by solving the problem of uniformity of spatial distribution of recycled aggregate in concrete.

[0040] (3) The present invention also fully considers the different characteristics of water absorption rate of recycled aggregates with different particle sizes, and obtains 5-10 mm modified recycled aggregates after modification and water curing with 5-10 mm recycled aggregates with higher water absorption rate, thereby reducing the consumption of free water and water reducing agent by 5-10 mm recycled aggregates with higher water absorption rate in the process of preparing concrete, and solves the problem that 100% recycled aggregate concrete is difficult to achieve high fluidity.

[0041] (4) In the preparation method of the present invention, 10-25 mm recycled aggregate and cementitious material are first added in sequence and dry-mixed for 10-20 seconds until uniform; then 2 / 3 mixing water and 5-10 mm modified recycled aggregate are added in sequence and stirred for 20-30 seconds until uniform, thereby reducing the consumption of water reducer by recycled aggregate and the surface interface defects of recycled aggregate, thereby improving the fluidity and mechanical properties of recycled aggregate concrete; finally, water reducer, machine-made sand and 1 / 3 mixing water are added and stirred for 60-90 seconds, thereby improving the homogeneity of each component of the prepared concrete and the workability of the concrete, thereby achieving high fluidity and homogeneity of each component of 100% recycled aggregate concrete.

[0042] (5) The present invention achieves 100% utilization of recycled aggregates while ensuring the performance of concrete, which can fundamentally solve a series of problems such as the serious shortage of natural stones and the environmental pollution caused by construction waste concrete waste. At the same time, it has the synergistic effect of carbon emission reduction and has great economic, environmental and social benefits. DETAILED DESCRIPTION

[0043] The present invention is described in detail below in conjunction with specific embodiments. This embodiment is implemented based on the technical solution of the present invention, and provides a detailed implementation method and a specific operation process, but the protection scope of the present invention is not limited to the following embodiments.

[0044] The raw materials in the following examples are as follows:

[0045] (1) Cement: P·O42.5 cement;

[0046] (2) Mineral powder: S95 mineral powder;

[0047] (3) Fly ash: Class II fly ash;

[0048] (4) Artificial sand: fineness modulus is 3.0, MB is 0.7, and stone powder content is 5.6%;

[0049] (5) Recycled aggregate: Recycled aggregate produced by Shanghai Xuzhong Recycling Resources Utilization Co., Ltd. is used. The performance meets the requirements of Class II recycled aggregate, with a particle size of 5 to 25 mm and continuous grading;

[0050] (6) Water reducing agent: a polycarboxylic acid high-performance water reducing agent with a water reducing rate of 28% produced by China Construction Western Construction New Materials Technology Co., Ltd.;

[0051] (7) Iron ore powder: iron ore powder supplied by Shanghai Keju Industrial Co., Ltd., with a fineness of 7.5% on a 0.15 mm sieve and an apparent density of 5500 kg / m 3 ;

[0052] (8) Mixing water: ordinary tap water.

[0053] Unless otherwise specified, the equipment used in the following examples are all conventional equipment in the art; the reagents used are all commercially available products or prepared by conventional methods in the art unless otherwise specified. Anything not described in detail in the following examples can be achieved by conventional experimental means in the art.

[0054] Some embodiments of the present invention are described in detail below. In the absence of conflict, the following embodiments and features in the embodiments may be combined with each other.

[0055] Example 1

[0056] The present embodiment provides a highly homogeneous and highly fluid recycled aggregate concrete, wherein the raw materials of each cubic meter of the concrete include the following components: 350 kg of cementitious material, 450 kg of 5-10 mm modified recycled aggregate, 600 kg of 10-25 mm recycled aggregate, 770 kg of machine-made sand, 3.5 kg of water reducer, and 160 kg of mixing water, wherein the modified recycled aggregate is obtained by modifying the recycled aggregate with an aggregate density adjusting slurry.

[0057] In this embodiment, the cementitious material is composed of 210 kg of cement, 87.5 kg of grade II fly ash and 52.5 kg of S95 mineral powder.

[0058] In this embodiment, the aggregate density adjusting slurry, based on 100 parts by weight, consists of the following components: 30 parts of iron ore powder, 20 parts of cement, 0.3 parts of water reducing agent and 49.7 parts of water.

[0059] In addition, this embodiment also provides a method for preparing highly homogeneous and highly fluid recycled aggregate concrete, the specific steps of which are as follows:

[0060] S1. 30 parts of iron ore powder, 20 parts of cement, 0.3 parts of water reducer and 49.7 parts of water are fully stirred and mixed to obtain aggregate density adjustment slurry;

[0061] S2. After fully stirring 5-10 mm recycled aggregate in aggregate density adjustment slurry for 3 minutes, the material-liquid separation hardening water curing for 1 day to obtain 5-10 mm modified recycled aggregate, wherein the mass ratio of the 5-10 mm recycled aggregate to the aggregate density adjustment slurry is 1:0.5;

[0062] S3. First, add 10-25 mm recycled aggregate and cementitious materials in sequence, dry mix for 10 seconds until uniform, then add 2 / 3 mixing water and 5-10 mm modified recycled aggregate in sequence and stir for 20 seconds until uniform, finally, add water reducer, machine-made sand and 1 / 3 mixing water and stir for 60 seconds to obtain highly uniform and highly fluid recycled aggregate concrete.

[0063] Example 2

[0064] The present embodiment provides a highly homogeneous and highly fluid recycled aggregate concrete, wherein the raw materials of each cubic meter of the concrete include the following components: 380 kg of cementitious material, 500 kg of 5-10 mm modified recycled aggregate, 520 kg of 10-25 mm recycled aggregate, 760 kg of machine-made sand, 4.0 kg of water reducer, and 165 kg of mixing water, wherein the modified recycled aggregate is obtained by modifying the recycled aggregate with an aggregate density adjusting slurry.

[0065] In this embodiment, the cementitious material is composed of 266 kg of cement, 76 kg of grade II fly ash and 38 kg of S95 mineral powder.

[0066] In this embodiment, the aggregate density adjusting slurry, based on 100 parts by weight, consists of the following components: 35 parts of iron ore powder, 25 parts of cement, 0.4 parts of water reducing agent and 39.6 parts of water.

[0067] In addition, this embodiment also provides a method for preparing highly homogeneous and highly fluid recycled aggregate concrete, the specific steps of which are as follows:

[0068] S1. 35 parts of iron ore powder, 25 parts of cement, 0.4 parts of water-reducing agent and 39.6 parts of water are fully stirred and mixed to obtain aggregate density adjustment slurry;

[0069] S2. After fully stirring 5-10 mm recycled aggregate in aggregate density adjustment slurry for 4 minutes, the material-liquid separation hardening water curing for 2 days to obtain 5-10 mm modified recycled aggregate, the mass ratio of the 5-10 mm recycled aggregate to the aggregate density adjustment slurry is 1:0.6;

[0070] S3. First, add 10-25 mm recycled aggregate and cementitious materials in sequence, dry mix for 15 seconds until uniform, then add 2 / 3 mixing water and 5-10 mm modified recycled aggregate in sequence and stir for 25 seconds until uniform, finally, add water reducer, machine-made sand and 1 / 3 mixing water and stir for 80 seconds to obtain highly uniform and highly fluid recycled aggregate concrete.

[0071] Example 3

[0072] The present embodiment provides a highly homogeneous and highly fluid recycled aggregate concrete, wherein the raw materials of each cubic meter of the concrete include the following components: 400 kg of cementitious material, 500 kg of 5-10 mm modified recycled aggregate, 550 kg of 10-25 mm recycled aggregate, 760 kg of machine-made sand, 5.0 kg of water reducer, and 175 kg of mixing water, wherein the modified recycled aggregate is obtained by modifying the recycled aggregate with an aggregate density adjusting slurry.

[0073] In this embodiment, the cementitious material is composed of 320 kg of cement, 40 kg of grade II fly ash and 40 kg of S95 mineral powder.

[0074] In this embodiment, the aggregate density adjusting slurry, based on 100 parts by weight, consists of the following components: 40 parts of iron ore powder, 30 parts of cement, 0.5 parts of water reducing agent and 29.5 parts of water.

[0075] In addition, this embodiment also provides a method for preparing highly homogeneous and highly fluid recycled aggregate concrete, the specific steps of which are as follows:

[0076] S1. Fully stir and mix 40 parts of iron ore powder, 30 parts of cement, 0.5 parts of water reducing agent and 29.5 parts of water to obtain aggregate density adjustment slurry;

[0077] S2. After fully stirring 5-10 mm recycled aggregate in aggregate density adjustment slurry for 5 minutes, the material-liquid separation hardening water curing for 3 days to obtain 5-10 mm modified recycled aggregate, wherein the mass ratio of the 5-10 mm recycled aggregate to the aggregate density adjustment slurry is 1:0.7;

[0078] S3. First, add 10-25 mm recycled aggregate and cementitious materials in sequence, dry mix for 20 seconds until uniform, then add 2 / 3 mixing water and 5-10 mm modified recycled aggregate in sequence and stir for 30 seconds until uniform, finally, add water reducer, machine-made sand and 1 / 3 mixing water and stir for 90 seconds to obtain highly uniform and highly fluid recycled aggregate concrete.

[0079] Example 4

[0080] The present embodiment provides a highly homogeneous and highly fluid recycled aggregate concrete, wherein the raw materials of each cubic meter of the concrete include the following components: 400 kg of cementitious material, 550 kg of 5-10 mm modified recycled aggregate, 500 kg of 10-25 mm recycled aggregate, 800 kg of machine-made sand, 4.8 kg of water reducer, and 180 kg of mixing water, wherein the modified recycled aggregate is obtained by modifying the recycled aggregate with an aggregate density adjusting slurry.

[0081] In this embodiment, the cementitious material is composed of 260 kg of cement, 80 kg of grade II fly ash and 60 kg of S95 mineral powder.

[0082] In this embodiment, the aggregate density adjusting slurry, based on 100 parts by weight, consists of the following components: 35 parts of iron ore powder, 25 parts of cement, 0.5 parts of water reducing agent and 39.5 parts of water.

[0083] In addition, this embodiment also provides a method for preparing highly homogeneous and highly fluid recycled aggregate concrete, the specific steps of which are as follows:

[0084] S1. 35 parts of iron ore powder, 25 parts of cement, 0.5 parts of water-reducing agent and 39.5 parts of water are fully stirred and mixed to obtain aggregate density adjustment slurry;

[0085] S2. After fully stirring 5-10 mm recycled aggregate in aggregate density adjustment slurry for 4.5 min, the material-liquid separation hardening water curing for 2.5 d obtains 5-10 mm modified recycled aggregate, wherein the mass ratio of the 5-10 mm recycled aggregate to the aggregate density adjustment slurry is 1:1;

[0086] S3. First, add 10-25 mm recycled aggregate and cementitious materials in sequence, dry mix for 15 seconds until uniform, then add 2 / 3 mixing water and 5-10 mm modified recycled aggregate in sequence and stir for 25 seconds until uniform, finally, add water reducer, machine-made sand and 1 / 3 mixing water and stir for 80 seconds to obtain highly uniform and highly fluid recycled aggregate concrete.

[0087] Example 5

[0088] The present embodiment provides a highly homogeneous and highly fluid recycled aggregate concrete, wherein the raw materials of each cubic meter of the concrete include the following components: 360 kg of cementitious material, 510 kg of 5-10 mm modified recycled aggregate, 540 kg of 10-25 mm recycled aggregate, 760 kg of machine-made sand, 4.5 kg of water reducer, and 172 kg of mixing water, wherein the modified recycled aggregate is obtained by modifying the recycled aggregate with an aggregate density adjusting slurry.

[0089] In this embodiment, the cementitious material is composed of 252 kg of cement, 54 kg of grade II fly ash and 54 kg of S95 mineral powder.

[0090] In this embodiment, the aggregate density adjusting slurry, based on 100 parts by weight, consists of the following components: 30 parts of iron ore powder, 20 parts of cement, 0.4 parts of water reducing agent and 49.6 parts of water.

[0091] In addition, this embodiment also provides a method for preparing highly homogeneous and highly fluid recycled aggregate concrete, the specific steps of which are as follows:

[0092] S1. 30 parts of iron ore powder, 20 parts of cement, 0.4 parts of water-reducing agent and 49.6 parts of water are fully stirred and mixed to obtain aggregate density adjustment slurry;

[0093] S2. After fully stirring 5-10 mm recycled aggregate in aggregate density adjustment slurry for 3.5 min, the material-liquid separation hardening water curing for 2 days to obtain 5-10 mm modified recycled aggregate, wherein the mass ratio of the 5-10 mm recycled aggregate to the aggregate density adjustment slurry is 1:0.8;

[0094] S3. First, add 10-25 mm recycled aggregate and cementitious materials in sequence, dry mix for 10 seconds until uniform, then add 2 / 3 mixing water and 5-10 mm modified recycled aggregate in sequence and stir for 30 seconds until uniform, finally, add water reducer, machine-made sand and 1 / 3 mixing water and stir for 90 seconds to obtain highly uniform and highly fluid recycled aggregate concrete.

[0095] Comparative Example 1

[0096] This comparative example provides a recycled aggregate concrete without adding aggregate density regulating materials. The raw materials of each cubic meter of the concrete include the following components: 360 kg of cementitious material, 510 kg of 5-10 mm modified recycled aggregate, 540 kg of 10-25 mm recycled aggregate, 760 kg of machine-made sand, 4.5 kg of water reducer, and 172 kg of mixing water, wherein the modified recycled aggregate is obtained by modifying the recycled aggregate with ordinary slurry.

[0097] In this embodiment, the cementitious material is composed of 252 kg of cement, 54 kg of grade II fly ash and 54 kg of S95 mineral powder.

[0098] In this embodiment, the common slurry, based on 100 parts by weight, consists of the following components: 20 parts of cement, 0.4 parts of water reducing agent and 79.6 parts of water.

[0099] In addition, this comparative example also provides a method for preparing recycled aggregate concrete without adding aggregate density adjusting materials, and the specific steps are as follows:

[0100] S1. Thoroughly stir and mix 20 parts of cement, 0.4 parts of water reducing agent and 79.6 parts of water to obtain a common slurry;

[0101] S2. After fully stirring 5-10 mm recycled aggregate in ordinary slurry for 3.5 min, the slurry and liquid are separated and hardened in water for 2 days to obtain 5-10 mm modified recycled aggregate, wherein the mass ratio of the 5-10 mm recycled aggregate to the ordinary aggregate density adjustment slurry is 1:0.8;

[0102] S3. First, add 10-25 mm recycled aggregate and cementitious materials in sequence, dry mix for 10 seconds until uniform, then add 2 / 3 mixing water and 5-10 mm modified recycled aggregate in sequence and stir for 30 seconds until uniform, finally, add water reducer, machine-made sand and 1 / 3 mixing water and stir for 90 seconds to obtain recycled aggregate concrete.

[0103] Comparative Example 2

[0104] The comparative example provides a recycled aggregate concrete which is not modified by using aggregate density regulating slurry. The raw materials of each cubic meter of the concrete include the following components: 360 kg of cementitious material, 510 kg of 5-10 mm modified recycled aggregate, 540 kg of 10-25 mm recycled aggregate, 760 kg of machine-made sand, 4.5 kg of water reducer, and 172 kg of mixing water, wherein the modified recycled aggregate is recycled aggregate modified by ordinary tap water.

[0105] In this embodiment, the cementitious material is composed of 252 kg of cement, 54 kg of grade II fly ash and 54 kg of S95 mineral powder.

[0106] In this embodiment, the 5-10 mm modified recycled aggregate is obtained by fully stirring 5-10 mm recycled aggregate in ordinary tap water for 3.5 minutes, separating the material from the liquid, and curing in hardening water for 2 days.

[0107] In addition, this comparative example also provides a method for preparing recycled aggregate concrete without using aggregate density adjustment slurry modification, and the specific steps are as follows:

[0108] S1. After fully stirring 5-10 mm recycled aggregate in ordinary tap water for 3.5 min, the material liquid is separated and hardened in water for 2 days to obtain 5-10 mm modified recycled aggregate;

[0109] S2. First, add 10-25 mm recycled aggregate and cementitious materials in sequence, dry mix for 10 seconds until uniform, then add 2 / 3 mixing water and 5-10 mm modified recycled aggregate in sequence and stir for 30 seconds until uniform, finally, add water reducer, machine-made sand and 1 / 3 mixing water and stir for 90 seconds to obtain recycled aggregate concrete.

[0110] Comparative Example 3

[0111] This comparative example provides a recycled aggregate concrete prepared by a conventional method. The raw materials of each cubic meter of the concrete include the following components: 360 kg of cementitious material, 510 kg of 5-10 mm modified recycled aggregate, 540 kg of 10-25 mm recycled aggregate, 760 kg of machine-made sand, 4.5 kg of water reducer, and 172 kg of mixing water, wherein the modified recycled aggregate is obtained by modifying the recycled aggregate with an aggregate density adjusting slurry.

[0112] In this embodiment, the cementitious material is composed of 252 kg of cement, 54 kg of grade II fly ash and 54 kg of S95 mineral powder.

[0113] In this embodiment, the aggregate density adjusting slurry, based on 100 parts by weight, consists of the following components: 30 parts of iron ore powder, 20 parts of cement, 0.4 parts of water reducing agent and 49.6 parts of water.

[0114] In addition, this comparative example also provides a method for preparing recycled aggregate concrete using a conventional preparation method, and the specific steps are as follows:

[0115] S1. 30 parts of iron ore powder, 20 parts of cement, 0.4 parts of water-reducing agent and 49.6 parts of water are fully stirred and mixed to obtain aggregate density adjustment slurry;

[0116] S2. After fully stirring 5-10 mm recycled aggregate in aggregate density adjustment slurry for 3.5 min, the material-liquid separation hardening water curing for 2 days to obtain 5-10 mm modified recycled aggregate, wherein the mass ratio of the 5-10 mm recycled aggregate to the aggregate density adjustment slurry is 1:0.8;

[0117] S3. Cement, fly ash, mineral powder, machine-made sand, recycled aggregate, modified recycled aggregate, water reducing agent and mixing water are directly mixed and stirred to obtain recycled aggregate concrete.

[0118] Comparative Example 4

[0119] This comparative example provides a recycled aggregate concrete. The raw materials of each cubic meter of the concrete include the following components: 360 kg of cementitious material, 510 kg of 5-10 mm recycled aggregate, 540 kg of 10-25 mm recycled aggregate, 760 kg of machine-made sand, 4.5 kg of water reducer, and 172 kg of mixing water.

[0120] In this embodiment, the cementitious material is composed of 252 kg of cement, 54 kg of grade II fly ash and 54 kg of S95 mineral powder.

[0121] In addition, this comparative example also provides a method for preparing recycled aggregate concrete using a conventional preparation method, and the specific steps are as follows:

[0122] The recycled aggregate concrete is obtained by directly mixing and stirring cement, fly ash, mineral powder, machine-made sand, 5-10 mm recycled aggregate, 10-25 mm recycled aggregate, water reducing agent and mixing water.

[0123] Performance Testing

[0124] Slump test: carried out in accordance with the relevant provisions of the Standard for Test Methods for Performance of Ordinary Concrete Mixtures (GB / T50080-2016);

[0125] Compressive strength test: carried out in accordance with the relevant provisions of the Standard for Test Methods for Physical and Mechanical Properties of Concrete (GB / T50081-2019);

[0126] Aggregate homogeneity test: Add the recycled aggregate concrete mixture into a 150mm*150mm*150mm test mold. After hardening, cut the test block in half along the molding direction. The mass of the upper half of the test block is recorded as m. 1 , the mass of the lower half of the test block is recorded as m 2 , aggregate homogeneity can be expressed as, Y = m 1 / m 2 , the closer Y is to 1, the more uniform the aggregate distribution of recycled aggregate concrete is and the better the homogeneity of the concrete is.

[0127] The slump, compressive strength and aggregate homogeneity of the concrete of Examples 1-5 and Comparative Examples 1-4 were tested, and the test results are shown in Table 1.

[0128] Table 1 Test results of concrete slump, compressive strength and aggregate homogeneity

[0129]

[0130] It can be seen from Example 5 and Comparative Examples 1-2 that the 5-10 mm recycled aggregate is modified by the aggregate density adjusting material, and the slump, compressive strength and aggregate homogeneity of the concrete obtained in Example 5 are greater than those of the concrete obtained in Comparative Examples 1-2, which effectively inhibits the floating of small-size recycled aggregates and improves the homogeneity of the concrete mixture.

[0131] It can be seen from Example 5 and Comparative Example 3 that the concrete is prepared by the distributed mixing method. The slump and aggregate homogeneity of the concrete obtained in Example 5 are greater than those of the concrete obtained in Comparative Example 3. First, 10-25 mm recycled aggregate and cementitious material are added in sequence and dry mixed for 10-20 seconds until uniform; then 2 / 3 mixing water and 5-10 mm modified recycled aggregate are added in sequence and stirred for 20-30 seconds until uniform, which reduces the consumption of water reducer by recycled aggregate and the interface defects on the surface of recycled aggregate, thereby improving the fluidity and mechanical properties of recycled aggregate concrete; finally, water reducer, machine-made sand and 1 / 3 mixing water are added and stirred for 60-90 seconds, which improves the homogeneity of each component of the prepared concrete and the workability of the concrete, and achieves the high fluidity of 100% recycled aggregate concrete and the homogeneity of each component.

[0132] It can be seen from Examples 1-5 and Comparative Examples 1-4 that the present invention comprehensively considers the differences in apparent density of recycled aggregates with different particle sizes, and performs aggregate density adjustment technology modification on 5-10 mm recycled aggregates, thereby effectively suppressing the floating of small-size recycled aggregates, achieving the homogeneity of high-fluidity 100% recycled aggregate concrete mixtures, and ensuring the appearance quality and strength stability of hardened recycled aggregate concrete.

[0133] The above description of the embodiments is to facilitate the understanding and use of the invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the above embodiments, and improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the present invention should be within the scope of protection of the present invention.

Claims

1. A highly homogeneous and highly fluid recycled aggregate concrete. It is characterized in that The raw materials of each cubic meter of the concrete include the following components: Cementitious material 350~400kg, Modified recycled aggregate 450~550kg, Recycled aggregate 500~600kg, Machine-made sand 700~800kg, Water reducing agent 3.5~5kg, Mixing water 160~180kg, Wherein, the modified recycled aggregate is obtained by modifying the recycled aggregate with aggregate density adjustment slurry; The aggregate density adjustment slurry is composed of the following components based on 100 parts by weight: 30-40 parts of aggregate density adjustment material, 20-30 parts of hardening material, 0.3-0.5 parts of dispersant, and the balance is water; The particle size of the modified recycled aggregate is 5-10 mm, and the particle size of the recycled aggregate is 10-25 mm; The mixed recycled aggregate composed of the modified recycled aggregate and the recycled aggregate is Class II recycled aggregate or above, with a particle size of 5 to 25 mm and continuous grading; The aggregate density adjustment material is iron ore powder, the fineness of which is less than 10% on a 0.15 mm sieve, and the apparent density is 5000-6000 kg / m 3 ; The hardening material is cement, and the cement is 42.5 grade ordinary Portland cement; The dispersant is a polycarboxylic acid high-performance water-reducing agent with a solid content of 40% and a water reduction rate of not less than 30%; The specific steps of the preparation method of the highly homogeneous and highly fluid recycled aggregate concrete are as follows: S1. preparing aggregate density adjustment slurry; S2. After fully stirring the 5-10 mm recycled aggregate in the aggregate density adjustment slurry, the slurry and liquid are separated, hardened and cured in water to obtain 5-10 mm modified recycled aggregate; S3, add 10-25 mm recycled aggregate and cementitious material in sequence, dry mix until uniform, and obtain a stirred mixture A; S4, adding a portion of mixing water and the 5-10 mm modified recycled aggregate obtained in step S2 to the mixed material A obtained in step S3, stirring until uniform, to obtain a stirred mixed material B; S5. Add a water reducing agent, machine-made sand and the remaining mixing water to the mixture B obtained in step S4 and stir to obtain a highly homogeneous and highly fluid recycled aggregate concrete.

2. A highly homogeneous and highly fluid recycled aggregate concrete according to claim 1, It is characterized in that The gelling material comprises the following components by mass percentage: Cement 60~80%, Fly ash 10~25%, Mineral powder 10~15%.

3. A highly homogeneous and highly fluid recycled aggregate concrete according to claim 2, It is characterized in that The cement is 42.5 grade ordinary Portland cement, the fly ash is grade II fly ash, and the mineral powder is S95 mineral powder.

4. The highly homogeneous and highly fluid recycled aggregate concrete according to claim 1, It is characterized in that The machine-made sand has a fineness modulus of 2.6-3.2, an MB value of <1.0, and a stone powder content of 4-8%.

5. The highly homogeneous and highly fluid recycled aggregate concrete according to claim 1, It is characterized in that The water reducing agent is a polycarboxylic acid high-performance water reducing agent with a solid content of 15% and a water reduction rate of not less than 25%.

6. The highly homogeneous and highly fluid recycled aggregate concrete according to claim 1, It is characterized in that In step S1, the specific steps of preparing the aggregate density adjustment slurry are as follows: Thoroughly stir and mix 30-40 parts of aggregate density adjusting material, 20-30 parts of hardening material, 0.3-0.5 parts of dispersant and the balance of water to obtain aggregate density adjusting slurry; In step S2, the mass ratio of the 5-10 mm recycled aggregate to the aggregate density adjustment slurry is 1:(0.5-1); In step S2, the stirring time is 3 to 5 minutes, and the hardening water curing time is 1 to 3 days; In step S3, the dry mixing time is 10 to 20 seconds; In step S4, the stirring time is 20 to 30 seconds; In step S5, the stirring time is 60 to 90 seconds; The volume ratio of the mixing water added in step S4 to the mixing water added in step S5 is 2:1.