Method for treating garbage fly ash by using manganese slag
Through the deammonization and desulfurization treatment of electrolytic manganese slag and waste fly ash, combined with gel technology of chitosan and calcium alginate, the problem of difficult dioxin pollution in the existing technology is solved, and manganese slag and fly ash is realized Reuse of ash and efficient preparation of cement active materials reduce costs and improve mechanical properties.
Patent Information
- Application Number
- CN202411073460.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-06
- Publication Date
- 2024-11-22
AI Technical Summary
In the prior art, when treating electrolytic manganese slag and waste incineration fly ash, it is difficult to effectively reduce the content of dioxin pollutants, and the curing/stabilization method cannot take into account the treatment of dioxin, resulting in low resource recycling and utilization efficiency.
By mixing the pretreated manganese slag and waste fly ash for deamination and desulfurization, use chitosan and calcium alginate to form a gel, and load the electrolytic manganese slag to achieve catalytic decomposition and adsorption of dioxins, reducing toxicity. And carbonize under high temperature conditions to form a silicon carbide skeleton to improve the mechanical properties of cement active materials.
The cost of electrolytic manganese slag treatment is reduced, the processing efficiency of dioxin is improved, the reuse of resources and the efficient preparation of cement active materials is realized, and some cement raw materials are replaced, and the mechanical properties of cement active materials are improved.
Smart Images

Figure BDA0004981528230000111
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of resource recycling, and in particular to a method for treating garbage fly ash by utilizing manganese slag. Background Art
[0002] Electrolytic manganese slag is the acidic waste residue produced by acid hydrolysis, neutralization, impurity removal and filtration of manganese ore in the process of electrolytic manganese production. It has the characteristics of high viscosity and low activity, and contains more sulfates and heavy metals such as manganese and chromium.
[0003] Waste incineration fly ash is a powdery granular substance captured by a bag filter after the flue gas generated by the waste incineration process undergoes high-temperature denitrification, rapid cooling (or waste heat utilization), dry (or semi-dry) deacidification, and activated carbon powder rotary spraying. Waste incineration fly ash contains heavy metal pollutants and dioxin pollutants.
[0004] In the related art, the treatment methods for waste incineration fly ash include cement-based solidification / stabilization method. Although the solidification / stabilization method has a good solidification effect on heavy metals, it cannot take into account the treatment of dioxins therein; the related art also adopts the combined treatment of electrolytic manganese slag and waste fly ash, and the combined treated material is used for the preparation of cementitious materials, but there is still a problem of high dioxin.
[0005] Application Contents
[0006] The present application is made in view of the above-mentioned problems, and its purpose is to provide a method for treating garbage fly ash using manganese slag, which realizes the recycling of resources.
[0007] Specifically, the first aspect of the present application provides a method for treating garbage fly ash using manganese slag, comprising the following steps:
[0008] The pre-treated manganese slag and the garbage fly ash are mixed and then subjected to deammoniation and desulfurization treatments in sequence to obtain cement active material;
[0009] The method for preparing the pretreated manganese slag comprises the following steps:
[0010] The electrolytic manganese slag, chitosan, calcium alginate and acid are mixed, the solid-liquid separation is performed, and the mixture is dried.
[0011] According to one of the technical solutions of this application, at least the following beneficial effects are achieved:
[0012] The present application adopts garbage fly ash as a deamination agent for pre-treating manganese slag. Through the coordinated treatment of the two, the cost of electrolytic manganese slag treatment is reduced. The manganese element in the electrolytic manganese slag also has a certain catalytic effect, which can catalyze the decomposition of organic matter such as dioxins. At the same time, dioxins are treated during desulfurization to reduce the toxicity of garbage fly ash. At the same time, the calcium, silicon and aluminum elements contained in the fly ash are used to obtain cement active materials after desulfurization treatment, which can replace part of the raw materials for cement preparation.
[0013] In the present application, the nitrogen element in the electrolytic manganese slag is removed through deamination treatment, and the gas after deamination can be recycled to produce ammonia water, thereby realizing the resource utilization of nitrogen element; at the same time, the competitive adsorption effect of excess ammonia nitrogen on the active catalytic sites of the electrolytic manganese slag is eliminated, thereby improving the treatment effect of dioxins.
[0014] In the present application, chitosan and calcium alginate are also used to treat the electrolytic manganese slag. Chitosan is positively charged in aqueous solution, while alginate ions are negatively charged and carboxylated polyvinyl alcohol is negatively charged. The three have an electrostatic force in the aqueous solution, thereby forming a gel in the aqueous solution; and the electrolytic manganese slag will be loaded on the surface of the gel to obtain pretreated manganese slag; the pretreated manganese slag has certain adsorption properties and oxidative degradation capabilities, and after the pretreated manganese slag is mixed with garbage fly ash, the pretreated manganese slag can stably adsorb the garbage fly ash, further improving the treatment efficiency.
[0015] Chitosan and alginate ions are carbonized under high temperature conditions. Under high temperature conditions, silica and carbon react to produce a silicon carbide skeleton, thereby further improving the mechanical properties of the final cement active material.
[0016] According to some embodiments of the present application, the mass ratio of the pretreated manganese slag to the garbage fly ash is 0.5 to 2.5:1.
[0017] According to some embodiments of the present application, the mass fraction of calcium in the garbage fly ash is 20% to 45%.
[0018] According to some embodiments of the present application, the mass fraction of silicon in the garbage fly ash is 1% to 3%.
[0019] According to some embodiments of the present application, the mass fraction of iron in the garbage fly ash is 1% to 2%.
[0020] According to some embodiments of the present application, the deamination temperature is 300°C to 500°C.
[0021] According to some embodiments of the present application, the deamination time is 0.5h to 1h.
[0022] According to some embodiments of the present application, the desulfurization time is 1 hour to 5 hours.
[0023] According to some embodiments of the present application, the desulfurization temperature is 1000°C to 1300°C.
[0024] By controlling the desulfurization temperature, the dioxin treatment efficiency is improved.
[0025] According to some embodiments of the present application, the electrolytic manganese slag includes 20% to 40% by mass of silicon dioxide.
[0026] According to some embodiments of the present application, the electrolytic manganese slag includes 30% to 40% by mass of sulfur trioxide.
[0027] According to some embodiments of the present application, the electrolytic manganese slag includes 5% to 10% manganese oxide by mass.
[0028] According to some embodiments of the present application, the electrolytic manganese slag includes ferric oxide in an amount of 5% to 10% by mass.
[0029] According to some embodiments of the present application, the electrolytic manganese slag includes ammonium sulfate in an amount of 3% to 5% by mass.
[0030] According to some embodiments of the present application, the mass ratio of the electrolytic manganese slag to chitosan is 100:2-5.
[0031] According to some embodiments of the present application, the mass ratio of the electrolytic manganese slag to calcium alginate is 100:2-5.
[0032] According to some embodiments of the present application, the mass ratio of the electrolytic manganese slag to the carboxylated polyvinyl alcohol is 100:1-2.
[0033] According to some embodiments of the present application, the acid includes at least one of hydrogen chloride and sulfuric acid.
[0034] According to some embodiments of the present application, the method for preparing the pretreated manganese slag comprises the following steps:
[0035] S1, mixing electrolytic manganese slag, chitosan, acid and water and reacting them to obtain a first mixture;
[0036] S2, mixing the first mixture, carboxylated polyvinyl alcohol and calcium alginate, reacting, separating the solid and liquid, collecting the solid phase and drying.
[0037] According to some embodiments of the present application, the method for preparing the carboxylated polyvinyl alcohol comprises the following steps:
[0038] After mixing vinyl acetate, acrylic acid, an initiator and a solvent, a first mixture is prepared;
[0039] The first mixture is alcoholyzed to obtain carboxylated polyvinyl alcohol.
[0040] According to some embodiments of the present application, the molar ratio of vinyl acetate to acrylic acid is 0.001 to 0.01:100.
[0041] According to some embodiments of the present application, the alcoholysis uses an alcohol solution of sodium hydroxide.
[0042] According to some embodiments of the present application, the molar ratio of vinyl acetate to initiator is 0.05 to 0.1:100.
[0043] According to some embodiments of the present application, the solvent is methanol or ethanol.
[0044] According to some embodiments of the present application, the mass volume ratio of the vinyl acetate and the solvent is 1 g: 1 mL to 3 mL.
[0045] According to some embodiments of the present application, the initiator is azobisisobutyronitrile.
[0046] According to some embodiments of the present application, the mixing temperature is 50°C to 70°C.
[0047] According to some embodiments of the present application, the mixing time is 4 hours to 6 hours.
[0048] According to some embodiments of the present application, the concentration of the alcoholic solution of sodium hydroxide is 0.8 mol / L to 1 mol / L.
[0049] According to some embodiments of the present application, the molar ratio of sodium hydroxide to vinyl acetate is 0.02-0.03:1.
[0050] According to some embodiments of the present application, the pH of the reaction in step S1 is 4-6.
[0051] According to some embodiments of the present application, the reaction time in step S1 is 1 h to 2 h.
[0052] According to some embodiments of the present application, the reaction time in step S2 is 1 h to 2 h.
[0053] According to some embodiments of the present application, the deaminated tail gas is used for preparing ammonia water.
[0054] The ammonia water obtained in the above steps is returned to the front-end electrolytic manganese process for use.
[0055] According to some embodiments of the present application, the desulfurized tail gas is used for preparing sulfuric acid.
[0056] The sulfuric acid prepared in the above steps is returned to the front-end electrolytic manganese process for use. DETAILED DESCRIPTION
[0057] In order to make the purpose, technical solutions and advantages of the present application clearer, the present application is described and illustrated below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not intended to limit the present application. Based on the embodiments provided in the present application, all other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of the present application.
[0058] Obviously, the following descriptions are only some examples or embodiments of the present application. For ordinary technicians in this field, the present application can also be applied to other similar scenarios without creative work. In addition, it can also be understood that although the efforts made in this development process may be complicated and lengthy, for ordinary technicians in the field related to the content disclosed in this application, some changes in design, manufacturing or production based on the technical content disclosed in this application are just conventional technical means, and should not be understood as insufficient content disclosed in this application.
[0059] However, unnecessary detailed descriptions may be omitted. For example, detailed descriptions of well-known matters and repeated descriptions of substantially the same structures may be omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate understanding by those skilled in the art. In addition, the following description is provided for those skilled in the art to fully understand the present application and is not intended to limit the subject matter described in the claims.
[0060] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.
[0061] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.
[0062] "Scope" disclosed in the present application is limited in the form of lower limit and upper limit, and a given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of a special range. The scope limited in this way can be including end values or not including end values, and can be arbitrarily combined, that is, any lower limit can be combined with any upper limit to form a scope. For example, if the scope of 60-120 and 80-110 is listed for a specific parameter, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range values 1 and 2 are listed, and if the maximum range values 3, 4 and 5 are listed, the following scope can be all expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In the present application, unless otherwise specified, the numerical range "ab" represents the abbreviation of any real number combination between a and b, wherein a and b are real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" are listed in this document, and "0-5" is just an abbreviation of these numerical combinations. In addition, when a parameter is expressed as an integer ≥ 2, it is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0063] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.
[0064] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.
[0065] If there is no special explanation, all steps of the present application can be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), which means that step (c) may be added to the method in any order. For example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.
[0066] If there is no special explanation, the "include" and "comprising" mentioned in this application are open-ended or closed-ended. For example, the "include" and "comprising" may mean that other components not listed may also be included or only the listed components may be included or only the listed components may be included.
[0067] If not specifically stated, in this application, the term "or" is inclusive. For example, the phrase "A or B" means "A, B, or both A and B". More specifically, any of the following conditions satisfies the condition "A or B": A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).
[0068] The electrolytic manganese slag selected in the examples and comparative examples of the present application is composed of the following components by mass fraction:
[0069] SO3 33.1%, SiO2 25.2%, CaO 14.6%, MnO 9.2%, Fe2O3 7.3%, MgO 2.6%, Al2O3 2.4%, (NH4)2SO4 3.8% and other components (loss on ignition and other inevitable impurities).
[0070] The garbage fly ash in the examples and comparative examples of the present application is composed of the following elements by mass fraction:
[0071] Ca 33.78%, Cl 32.97%, Na 8.24%, S 4.76%, Si 2.11%, Al 0.7%, Fe 1.05%, Mg 2.79%, K 5.79%, Pb 0.27%, Zn 0.23% and other components (loss on ignition and other inevitable impurities).
[0072] The preparation method of carboxylated polyvinyl alcohol in the examples and comparative examples of the present application consists of the following steps:
[0073] Vinyl acetate, an initiator (azobisisobutyronitrile) and a solvent are mixed (the molar ratio of vinyl acetate to the initiator is 0.08:100, and the mass volume ratio of vinyl acetate to the solvent is 1 g:3 mL), and acrylic acid is then added dropwise to the mixture (dripped over 30 minutes) for reaction (the molar ratio of vinyl acetate to acrylic acid is 1:0.002; the reaction time is 5 hours, and the reaction atmosphere is nitrogen) to obtain a first mixture;
[0074] The first mixture and a sodium hydroxide methanol solution (the molar concentration of sodium hydroxide is 1 mol / L) are mixed (the molar ratio of vinyl acetate to sodium hydroxide is 1:0.02) and then alcoholyzed at 50°C for 30 minutes to obtain a gel product PVA. After the reaction is completed, the PVA obtained by alcoholysis is dissolved in water at 90°C, filtered to remove insoluble impurities, and cooled to room temperature.
[0075] The product was precipitated three times using methanol as a precipitant, and then filtered and dried to obtain carboxylated polyvinyl alcohol.
[0076] Example 1
[0077] This embodiment is a method for treating garbage fly ash using manganese slag, which consists of the following steps:
[0078] The pre-treated manganese slag and the garbage fly ash are mixed and then subjected to deammoniation and desulfurization treatments in sequence to obtain cement active material;
[0079] The mass ratio of pretreated manganese slag to garbage fly ash is 2:1.
[0080] The deamination temperature is 500°C.
[0081] The deamination time is 1 h.
[0082] The desulfurization time is 2h.
[0083] The desulfurization temperature is 1200℃.
[0084] The method for preparing pretreated manganese slag comprises the following steps:
[0085] S1, mixing electrolytic manganese slag, chitosan, acid (35% concentrated hydrochloric acid) and water (the mass volume ratio of electrolytic manganese slag to water is 1g:500mL) and reacting (the reaction pH is 5 and the reaction time is 2h) to obtain a first mixture;
[0086] S2. The first mixture, carboxylated polyvinyl alcohol and calcium alginate are mixed and reacted (reaction time is 2 hours), solid-liquid separation is performed, and the solid phase is collected and dried (dried at 80° C.).
[0087] The mass ratio of electrolytic manganese slag to chitosan is 100:4.
[0088] The mass ratio of electrolytic manganese slag to calcium alginate is 100:3.
[0089] The mass ratio of electrolytic manganese slag to carboxylated polyvinyl alcohol is 100:1.8.
[0090] In this embodiment, the deaminated tail gas is used for the preparation of ammonia water.
[0091] In this embodiment, the desulfurized tail gas is used to prepare sulfuric acid.
[0092] Example 2
[0093] This embodiment is a method for treating garbage fly ash using manganese slag, which consists of the following steps:
[0094] The pre-treated manganese slag and the garbage fly ash are mixed and then subjected to deammoniation and desulfurization treatments in sequence to obtain cement active material;
[0095] The mass ratio of pretreated manganese slag to garbage fly ash is 0.5:1.
[0096] The deamination temperature is 400°C.
[0097] The deamination time is 0.5h.
[0098] The desulfurization time is 5h.
[0099] The desulfurization temperature is 1000℃.
[0100] The method for preparing pretreated manganese slag comprises the following steps:
[0101] S1, mixing electrolytic manganese slag, chitosan, acid (35% concentrated hydrochloric acid) and water (the mass volume ratio of electrolytic manganese slag to water is 1g:500mL) and reacting (the reaction pH is 5 and the reaction time is 2h) to obtain a first mixture;
[0102] S2. The first mixture, carboxylated polyvinyl alcohol and calcium alginate are mixed and reacted (reaction time is 2 hours), solid-liquid separation is performed, and the solid phase is collected and dried (dried at 80° C.).
[0103] The mass ratio of electrolytic manganese slag to chitosan is 100:2.
[0104] The mass ratio of electrolytic manganese slag to calcium alginate is 100:5.
[0105] The mass ratio of electrolytic manganese slag to carboxylated polyvinyl alcohol is 100:1.
[0106] In this embodiment, the deaminated tail gas is used for the preparation of ammonia water.
[0107] In this embodiment, the desulfurized tail gas is used to prepare sulfuric acid.
[0108] Example 3
[0109] This embodiment is a method for treating garbage fly ash using manganese slag, which consists of the following steps:
[0110] The pre-treated manganese slag and the garbage fly ash are mixed and then subjected to deammoniation and desulfurization treatments in sequence to obtain cement active material;
[0111] The mass ratio of pretreated manganese slag to garbage fly ash is 2.5:1.
[0112] The deamination temperature is 300°C.
[0113] The deamination time is 1 h.
[0114] The desulfurization time is 1h.
[0115] The desulfurization temperature is 1300℃.
[0116] The method for preparing pretreated manganese slag comprises the following steps:
[0117] S1, mixing electrolytic manganese slag, chitosan, acid (35% concentrated hydrochloric acid) and water (the mass volume ratio of electrolytic manganese slag to water is 1g:500mL) and reacting (the reaction pH is 5 and the reaction time is 2h) to obtain a first mixture;
[0118] S2. The first mixture, carboxylated polyvinyl alcohol and calcium alginate are mixed and reacted (the reaction time is 2 hours), the solid-liquid separation is performed, the solid phase is collected, and dried (dried at 80° C.).
[0119] The mass ratio of electrolytic manganese slag to chitosan is 100:5.
[0120] The mass ratio of electrolytic manganese slag to calcium alginate is 100:2.
[0121] The mass ratio of electrolytic manganese slag to carboxylated polyvinyl alcohol is 100:2.
[0122] In this embodiment, the deaminated tail gas is used for the preparation of ammonia water.
[0123] In this embodiment, the desulfurized tail gas is used to prepare sulfuric acid.
[0124] Example 4
[0125] This embodiment is a method for treating garbage fly ash using manganese slag, which consists of the following steps:
[0126] The pre-treated manganese slag and the garbage fly ash are mixed and then subjected to deammoniation and desulfurization treatments in sequence to obtain cement active material;
[0127] The mass ratio of pretreated manganese slag to garbage fly ash is 1:1.
[0128] The deamination temperature is 500°C.
[0129] The deamination time is 1 h.
[0130] The desulfurization time is 4h.
[0131] The desulfurization temperature is 1200℃.
[0132] The method for preparing pretreated manganese slag comprises the following steps:
[0133] S1, mixing electrolytic manganese slag, chitosan, acid (35% concentrated hydrochloric acid) and water (the mass volume ratio of electrolytic manganese slag to water is 1g:500mL) and reacting (the reaction pH is 5 and the reaction time is 2h) to obtain a first mixture;
[0134] S2. The first mixture, carboxylated polyvinyl alcohol and calcium alginate are mixed and reacted (reaction time is 2 hours), solid-liquid separation is performed, and the solid phase is collected and dried (dried at 80° C.).
[0135] The mass ratio of electrolytic manganese slag to chitosan is 100:3.
[0136] The mass ratio of electrolytic manganese slag to calcium alginate is 100:4.
[0137] The mass ratio of electrolytic manganese slag to carboxylated polyvinyl alcohol is 100:1.2.
[0138] In this embodiment, the deaminated tail gas is used for the preparation of ammonia water.
[0139] In this embodiment, the desulfurized tail gas is used to prepare sulfuric acid.
[0140] Example 5
[0141] This embodiment is a method for treating garbage fly ash using manganese slag, which consists of the following steps:
[0142] The pre-treated manganese slag and the garbage fly ash are mixed and then subjected to deammoniation and desulfurization treatments in sequence to obtain cement active material;
[0143] The mass ratio of pretreated manganese slag to garbage fly ash is 1.5:1.
[0144] The deamination temperature is 500°C.
[0145] The deamination time is 1 h.
[0146] The desulfurization time is 2h.
[0147] The desulfurization temperature is 1100°C.
[0148] The method for preparing pretreated manganese slag comprises the following steps:
[0149] S1, mixing electrolytic manganese slag, chitosan, acid (35% concentrated hydrochloric acid) and water (the mass volume ratio of electrolytic manganese slag to water is 1g:500mL) and reacting (the reaction pH is 5 and the reaction time is 2h) to obtain a first mixture;
[0150] S2. The first mixture, carboxylated polyvinyl alcohol and calcium alginate are mixed and reacted (reaction time is 2 hours), solid-liquid separation is performed, and the solid phase is collected and dried (dried at 80° C.).
[0151] The mass ratio of electrolytic manganese slag to chitosan is 100:4.
[0152] The mass ratio of electrolytic manganese slag to calcium alginate is 100:3.
[0153] The mass ratio of electrolytic manganese slag to carboxylated polyvinyl alcohol is 100:1.
[0154] In this embodiment, the deaminated tail gas is used for the preparation of ammonia water.
[0155] In this embodiment, the desulfurized tail gas is used to prepare sulfuric acid.
[0156] Comparative Example 1
[0157] This comparative example is a method for treating garbage fly ash using manganese slag, which differs from Example 1 in that:
[0158] In this comparative example, the manganese slag is not pretreated but directly mixed with the garbage fly ash for deammoniation and desulfurization.
[0159] Comparative Example 2
[0160] This comparative example is a method for treating garbage fly ash using manganese slag, which differs from Example 1 in that:
[0161] In the preparation method of the pretreated manganese slag in this comparative example, carboxylated polyvinyl alcohol and chitosan are not added.
[0162] Comparative Example 3
[0163] This comparative example is a method for treating garbage fly ash using manganese slag, which differs from Example 1 in that:
[0164] In the preparation method of the pretreated manganese slag in this comparative example, chitosan is not added.
[0165] Comparative Example 4
[0166] This comparative example is a method for treating garbage fly ash using manganese slag, which differs from Example 1 in that:
[0167] In the preparation method of the pretreated manganese slag in this comparative example, no calcium alginate is added.
[0168] Comparative Example 5
[0169] This comparative example is a method for treating garbage fly ash using manganese slag, which differs from Example 1 in that:
[0170] In the preparation method of the pretreated manganese slag in this comparative example, no carboxylated polyvinyl alcohol is added.
[0171] The heavy metal leaching concentration of cementitious materials is determined by the acetic acid buffer solution method (HJ / T 300); the dioxins are determined by isotope dilution high-resolution gas chromatography-high-resolution mass spectrometry (HJ 77.4); the compressive strength is determined in accordance with GBT25993 (humidity 95%, temperature 20℃±1℃, and test after 28d curing).
[0172] The compressive strength test mortar of the present application is prepared in the following manner.
[0173] The proportion of mortar used in the test is:
[0174] 225g of cement, 225g of cement active material (prepared in Examples 1 to 5 and Comparative Examples 1 to 5), 1350g of standard sand and 225g of water.
[0175] The performance test results of this embodiment and the comparative example are shown in Table 1.
[0176] Table 1
[0177]
[0178] Compared with the prior art, in which a large amount of deamination agent needs to be added to the electrolytic manganese slag for deamination, which increases the disposal cost, the treatment method of the embodiment of the present application rationally utilizes another waste - waste incineration fly ash as a deamination agent, and reduces the cost of electrolytic manganese slag disposal while co-disposing fly ash. The use of electrolytic manganese slag to co-dispose fly ash shortens the production process of existing cement active materials and reduces costs; when pre-treatment manganese slag is desulfurized at high temperature, dioxins are completely decomposed, reducing production costs. Resource utilization is achieved by recovering ammonia, sulfur and heavy metal elements in pre-treatment manganese slag and waste incineration fly ash.
[0179] It should be noted that the present application is not limited to the above-mentioned embodiments. The above-mentioned embodiments are only examples, and the embodiments having the same structure as the technical idea and exerting the same effect within the scope of the technical solution of the present application are all included in the technical scope of the present application. In addition, without departing from the scope of the main purpose of the present application, various modifications that can be thought of by those skilled in the art to the embodiments and other methods of combining some of the constituent elements in the embodiments are also included in the scope of the present application.
Claims
1. A method for treating garbage fly ash using manganese slag, It is characterized in that The following steps are involved: The pre-treated manganese slag and the garbage fly ash are mixed and then subjected to deammoniation and desulfurization treatments in sequence to obtain cement active material; The method for preparing the pretreated manganese slag comprises the following steps: The electrolytic manganese slag, chitosan, carboxylated polyvinyl alcohol, calcium alginate and acid are mixed, solid-liquid separation is performed, and drying is performed.
2. The method according to claim 1, It is characterized in that The mass ratio of the pretreated manganese slag to the garbage fly ash is 0.5 to 2.5:1; And / or, the mass fraction of calcium in the garbage fly ash is 20% to 45%; And / or, the mass fraction of silicon in the garbage fly ash is 1% to 3%; And / or, the mass fraction of iron in the garbage fly ash is 1% to 2%.
3. The method according to claim 1, It is characterized in that The deamination temperature is 300°C to 500°C; And / or, the deamination time is 0.5h to 1h; And / or, the desulfurization time is 1h to 5h; And / or, the desulfurization temperature is 1000°C to 1300°C.
4. The method according to claim 1, It is characterized in that The electrolytic manganese slag includes 20% to 40% by mass of silicon dioxide; And / or, the electrolytic manganese slag comprises 30% to 40% by mass of sulfur trioxide; And / or, the electrolytic manganese slag includes 5% to 10% by mass of manganese oxide; And / or, the electrolytic manganese slag includes 5% to 10% by mass of ferric oxide; And / or, the electrolytic manganese slag includes 3% to 5% by mass of ammonium sulfate.
5. The method according to claim 1, It is characterized in that The mass ratio of the electrolytic manganese slag to chitosan is 100:2-5; And / or, the mass ratio of the electrolytic manganese slag to calcium alginate is 100:2-5; And / or, the mass ratio of the electrolytic manganese slag to the carboxylated polyvinyl alcohol is 100:1-2; And / or, the preparation method of the carboxylated polyvinyl alcohol comprises the following steps: After mixing vinyl acetate, acrylic acid, an initiator and a solvent, a first mixture is prepared; alcoholyzing the first mixture to obtain carboxylated polyvinyl alcohol; and / or, the molar ratio of vinyl acetate to acrylic acid is 0.001 to 0.01:100; And / or, the alcoholysis adopts an alcohol solution of sodium hydroxide; and / or, the molar ratio of vinyl acetate to initiator is 0.05 to 0.1:100; And / or, the solvent is methanol or ethanol.
6. The method according to claim 1, It is characterized in that The acid includes at least one of hydrogen chloride and sulfuric acid.
7. The method according to claim 1, It is characterized in that The method for preparing the pretreated manganese slag comprises the following steps: S1, mixing electrolytic manganese slag, chitosan, acid and water and reacting them to obtain a first mixture; S2, mixing the first mixture, carboxylated polyvinyl alcohol and calcium alginate, reacting, separating the solid and liquid, collecting the solid phase and drying.
8. The method according to claim 7, It is characterized in that The pH of the reaction in step S1 is 4 to 6; And / or, the reaction time in step S1 is 1 h to 2 h.
9. The method according to claim 7, It is characterized in that The reaction time in step S2 is 1 h to 2 h.
10. The method according to claim 1, It is characterized in that The deammonified tail gas is used for preparing ammonia water; And / or, the desulfurized tail gas is used to prepare sulfuric acid.