Recycled asphalt concrete and preparation method thereof

By using SBS modified asphalt, recycling asphalt mixture and modified microporous silica in asphalt concrete, the utilization rate of waste asphalt and the performance of asphalt concrete are improved, and the problems of asphalt hardening and cracking are solved. It has achieved improvements in high-temperature rutting resistance and low-temperature crack resistance.

CN118993618AActive Publication Date: 2024-11-22GUANGZHOU CITY POLYTECHNIC
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411106809.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-11-22
Estimated Expiration
2044-08-13

AI Technical Summary

Technical Problem

In the prior art, the amount of waste asphalt mixture in asphalt concrete is limited, resulting in asphalt hardening and brittleness, poor viscoelastic performance, easy to cause cracking problems, and difficult to effectively utilize and recover asphalt, affecting pavement performance and environment.

Method used

Use SBS modified asphalt, recycled asphalt mixture, modified microporous silica, waste mineral oil, guaia, dioctyl phthalate, curing agent and anti-aging agent to improve the recycling of asphalt mixture The amount of addition of modified microporous silica is prepared by specific preparation methods to enhance the high-temperature rut resistance and low-temperature crack resistance of asphalt concrete.

Benefits of technology

The proportion of recycled asphalt mixture is significantly improved, the high-temperature rutting resistance and low-temperature crack resistance of recycled asphalt concrete is enhanced, the bending and pulling failure strength is improved, the cracking problem is solved, and the use requirements of the surface layer of the expressway is met.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004991059890000161
    Figure BDA0004991059890000161
  • Figure BDA0004991059890000162
    Figure BDA0004991059890000162
Patent Text Reader

Abstract

The invention discloses recycled asphalt concrete as well as a preparation method and application thereof. The recycled asphalt concrete is prepared from the following raw materials: SBS modified asphalt, a recycled asphalt mixture, aggregate, modified microporous silicon dioxide, waste mineral oil, guaiacol, dioctyl phthalate, a curing agent and an anti-aging agent. Modified microporous silicon dioxide, waste mineral oil, guaiacol, dioctyl phthalate, a curing agent and an anti-aging agent are used for regenerating aged asphalt in a recycled asphalt mixture, and aggregate and SBS modified asphalt are used as auxiliary materials, so that the recycled asphalt concrete is prepared. The proportion of the recycled asphalt mixture in the recycled asphalt concrete is increased to 50% or above, and the recycled asphalt concrete has good high-temperature rut resistance, low-temperature crack resistance and the like and is high in flexural-tensile breaking strength.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of asphalt, and in particular to a regenerated asphalt concrete and a preparation method of the regenerated asphalt concrete. Background Art

[0002] Asphalt concrete pavement will slowly age under natural conditions after a period of use, which can easily cause the asphalt to harden and become brittle, and lose its proper physical properties, thus affecting road performance. Coupled with the effects of water and vehicle load, the road surface disease will be aggravated. With the increasing number of pavement maintenance and renovation and expansion projects, the amount of waste asphalt will become larger and larger. Recycling asphalt pavements that do not meet performance standards can make full use of the waste generated by the original asphalt pavement, save a lot of asphalt, reduce construction costs, and at the same time reduce the occupation of land resources by waste and protect the environment.

[0003] At present, the content of waste asphalt mixture in hot recycling technology is generally not more than 30%, and it is rarely used in the surface layer of highways. The main reason is that the asphalt in the waste asphalt mixture ages, becomes hard and brittle, and its viscoelastic properties deteriorate, making the hot recycled asphalt concrete prone to cracking problems, such as temperature cracking and fatigue cracking. The higher the content of old materials, the more serious the cracking problem.

[0004] Therefore, in view of the shortcomings of the prior art, it is necessary to provide a regenerated asphalt concrete and a preparation method of the regenerated asphalt concrete to solve the shortcomings of the prior art. Summary of the invention

[0005] One of the purposes of the present invention is to avoid the shortcomings of the prior art and provide a regenerated asphalt concrete which can increase the amount of recycled asphalt mixture while ensuring the quality, thereby increasing the effect of waste utilization.

[0006] The above-mentioned purpose of the present invention is achieved by the following technical measures:

[0007] Provided is a recycled asphalt concrete, the raw materials of which include SBS modified asphalt, recycled asphalt mixture, aggregate, modified microporous silica, waste mineral oil, guaiac wood oil, dioctyl phthalate, curing agent and anti-aging agent.

[0008] The modified microporous silica is prepared by the following steps:

[0009] A1, adding 3,7-dimethyl-6-octen-1-ol to tetrahydrofuran, and adding 4-cyclohexanonecarboxylic acid and sodium hydroxide to obtain an intermediate;

[0010] A2, adding microporous silica to hydrochloric acid, stirring and filtering to obtain pretreated microporous silica;

[0011] A3. Add the intermediate to acetone, then add the pretreated microporous silica, and heat to obtain modified microporous silica.

[0012] The regenerated asphalt concrete of the present invention, measured in parts by weight,

[0013] SBS modified asphalt: 10 parts;

[0014] Recycled asphalt mixture: 40 to 50 parts;

[0015] Aggregate: 10 to 25 parts;

[0016] Modified microporous silica: 3 to 5 parts;

[0017] Waste mineral oil: 0.5 to 2 parts;

[0018] Guaiac wood oil: 0.1 to 0.5 parts;

[0019] Dioctyl phthalate: 0.05 to 0.1 parts;

[0020] Curing agent: 0.05 to 0.1 parts;

[0021] Anti-aging agent: 0.05 to 0.1 parts.

[0022] Furthermore, the regenerated asphalt concrete of the present invention, in parts by weight,

[0023] SBS modified asphalt: 10 parts;

[0024] Recycled asphalt mixture: 44 parts;

[0025] Aggregate: 18 parts;

[0026] Modified microporous silica: 3.8 parts;

[0027] Waste mineral oil: 1.1 parts;

[0028] Guaiac wood oil: 0.3 parts;

[0029] Dioctyl phthalate: 0.08 parts;

[0030] Curing agent: 0.07 parts;

[0031] Anti-aging agent: 0.06 parts.

[0032] Preferably, the modified microporous silica is prepared by the following steps:

[0033] A1. In parts by weight, add 100 parts of 3,7-dimethyl-6-octen-1-ol to 200-300 parts of tetrahydrofuran, and add 60-80 parts of 4-cyclohexanonecarboxylic acid and 10-20 parts of sodium hydroxide, stir at 30° C. to 40° C. for 14 h to 18 h, and salt out and dry to obtain an intermediate;

[0034] A2, adding 10 parts of microporous silica to 10 to 20 parts of 0.5 mol / L to 2 mol / L hydrochloric acid solution, stirring for 1 h to 3 h, filtering, and obtaining pretreated microporous silica;

[0035] A3. Add 3 to 5 parts of the intermediate to 10 to 20 parts of acetone, then add 5 parts of pretreated microporous silica, heat to 70°C to 90°C, stir for 1 to 3 hours, filter and dry to obtain modified microporous silica.

[0036] Preferably, the modified microporous silica is prepared by the following steps:

[0037] A1. In parts by weight, 100 parts of 3,7-dimethyl-6-octen-1-ol were added to 250 parts of tetrahydrofuran, and 66 parts of 4-cyclohexanonecarboxylic acid and 13.6 parts of sodium hydroxide were added, and the mixture was stirred at 37° C. for 16 hours, and then salted out and dried to obtain an intermediate;

[0038] A2, adding 10 parts of microporous silica to 15.5 parts of 1.2 mol / L hydrochloric acid solution, stirring for 2 hours, filtering, and obtaining pretreated microporous silica;

[0039] A3. Add 4 parts of the intermediate to 17 parts of acetone, then add 5 parts of pretreated microporous silica, heat to 82°C, stir for 2 hours, filter and dry to obtain modified microporous silica.

[0040] Preferably, the anti-aging agent is polyethylene naphthalate or phenyl-α-naphthylamine.

[0041] Preferably, the curing agent is polyetheramine or catechol.

[0042] The second object of the present invention is to provide a method for preparing regenerated asphalt concrete by avoiding the shortcomings of the prior art. The regenerated asphalt concrete prepared by the method can increase the amount of recycled asphalt mixture added while ensuring the quality, thereby increasing the effect of waste utilization.

[0043] The above-mentioned purpose of the present invention is achieved by the following technical measures:

[0044] A method for preparing the above-mentioned regenerated asphalt concrete is provided, comprising the following steps:

[0045] S1, modified microporous silica, waste mineral oil, guaiac wood oil, dioctyl phthalate, a curing agent and an anti-aging agent are mixed and stirred to obtain a mixture;

[0046] S2, crushing the recycled asphalt mixture;

[0047] S3, heating the SBS modified asphalt, then adding the recycled asphalt mixture to the SBS modified asphalt, and then adding the mixture to obtain a recycled asphalt mixture;

[0048] S4. Adding the aggregate to the recycled asphalt mixture to obtain recycled asphalt concrete.

[0049] Preferably, the above preparation method comprises the following steps:

[0050] S1, modified microporous silica, waste mineral oil, guaiac wood oil, dioctyl phthalate, a curing agent and an anti-aging agent are mixed and stirred, and heated to 100° C. to 120° C. to obtain a mixture;

[0051] S2, crushing the recycled asphalt mixture to an average particle size of less than 0.2 cm, and heating to 100°C to 110°C;

[0052] S3, heating the SBS modified asphalt to 100°C to 110°C, then adding the recycled asphalt mixture to the SBS modified asphalt, and then adding the mixture to obtain a recycled asphalt mixture;

[0053] S4. Adding the aggregate to the recycled asphalt mixture to obtain recycled asphalt concrete.

[0054] The invention discloses a regenerated asphalt concrete, a preparation method and application thereof, wherein the raw materials of the regenerated asphalt concrete contain SBS modified asphalt, recycled asphalt mixture, aggregate, modified microporous silica, waste mineral oil, guaiac wood oil, dioctyl phthalate, a curing agent and an anti-aging agent; the modified microporous silica is prepared by the following steps: A1, adding 3,7-dimethyl-6-octen-1-ol to tetrahydrofuran, and adding 4-cyclohexanone carboxylic acid and sodium hydroxide to obtain an intermediate; A2, adding the microporous silica to hydrochloric acid, stirring and filtering to obtain pretreated microporous silica; A3, adding acetone to the intermediate, then adding the pretreated microporous silica, heating to obtain the modified microporous silica. The modified microporous silica, waste mineral oil, guaiac wood oil, dioctyl phthalate, curing agent and anti-aging agent of the present invention are used to regenerate aged asphalt in recycled asphalt mixture, and aggregate and SBS modified asphalt are used to prepare a regenerated asphalt concrete. The proportion of the recycled asphalt mixture in the regenerated asphalt concrete is increased to more than 50%. The regenerated asphalt concrete has good high-temperature rutting resistance and low-temperature cracking resistance, and has high flexural tensile strength. DETAILED DESCRIPTION

[0055] The technical scheme of the present invention is further described in conjunction with the following examples. Unless otherwise specified in the following examples, the raw materials used in each example are commercially available products. Aggregate refers to crushed stone, gravel, slag, natural sand, artificial sand, stone chips, cement, mineral powder, fly ash, etc. used in the mixture, which plays the role of skeleton and filling in the mixture. Waste mineral oil is selected from tar, petroleum residue oil, deasphalted oil, heavy distillate oil, waste lubricating oil, white oil, lubricating oil base oil, etc.

[0056] Example 1

[0057] A regenerated asphalt concrete, the raw materials of which include SBS modified asphalt, recycled asphalt mixture, aggregate, modified microporous silica, waste mineral oil, guaiac wood oil, dioctyl phthalate, curing agent and antioxidant. The antioxidant is polyethylene naphthalate. The curing agent is polyetheramine. The waste mineral oil in this embodiment is a mixture of tar, petroleum residue and deasphalted oil, and the weight ratio of the three is 1:1:1, and the waste mineral oil is pre-filtered, precipitated, flashed, vacuum distilled and hydrofined. The aggregate of the present invention is natural sand.

[0058] In the regenerated asphalt concrete, in parts by weight,

[0059] SBS modified asphalt: 10 parts;

[0060] Recycled asphalt mixture: 40 parts;

[0061] Aggregate: 25 parts;

[0062] Modified microporous silica: 5 parts;

[0063] Waste mineral oil: 2 parts;

[0064] Guaiac wood oil: 0.5 parts;

[0065] Dioctyl phthalate: 0.1 part;

[0066] Curing agent: 0.1 part;

[0067] Anti-aging agent: 0.1 parts.

[0068] The modified microporous silica is prepared by the following steps:

[0069] A1. In parts by weight, 100 parts of 3,7-dimethyl-6-octen-1-ol were added to 200 parts of tetrahydrofuran, and 80 parts of 4-cyclohexanonecarboxylic acid and 10 parts of sodium hydroxide were added, and the mixture was stirred at 30° C. for 14 hours, and salted out and dried to obtain an intermediate;

[0070] A2, adding 10 parts of microporous silica to 10 parts of 2 mol / L hydrochloric acid solution, stirring for 3 hours, filtering, and obtaining pretreated microporous silica;

[0071] A3. Add 3 parts of the intermediate to 10 parts of acetone, then add 5 parts of pretreated microporous silica, heat to 70°C, stir for 1 hour, filter and dry to obtain modified microporous silica.

[0072] The method for preparing regenerated asphalt concrete in this embodiment comprises the following steps:

[0073] S1, modified microporous silica, waste mineral oil, guaiac wood oil, dioctyl phthalate, a curing agent and an anti-aging agent are mixed and stirred, and heated to 100° C. to obtain a mixture;

[0074] S2, crushing the recycled asphalt mixture to an average particle size of less than 0.2 cm, and heating to 100°C;

[0075] S3, heating the SBS modified asphalt to 100°C, then adding the recycled asphalt mixture to the SBS modified asphalt, and then adding the mixture to obtain a recycled asphalt mixture;

[0076] S4. Adding the aggregate to the recycled asphalt mixture to obtain recycled asphalt concrete.

[0077] Example 2

[0078] A regenerated asphalt concrete, the raw materials of which include SBS modified asphalt, recycled asphalt mixture, aggregate, modified microporous silica, waste mineral oil, guaiac wood oil, dioctyl phthalate, curing agent and antioxidant. The antioxidant is phenyl-α-naphthylamine. The curing agent is catechol. The waste mineral oil in this embodiment is a mixture of tar, petroleum residue and deasphalted oil, and the weight ratio of the three is 1:1:1, and the waste mineral oil is pre-filtered, precipitated, flashed, vacuum distilled and hydrofined. The aggregate of the present invention is natural sand.

[0079] In the regenerated asphalt concrete, in parts by weight,

[0080] SBS modified asphalt: 10 parts;

[0081] Recycled asphalt mixture: 50 parts;

[0082] Aggregate: 10 parts;

[0083] Modified microporous silica: 3 parts;

[0084] Waste mineral oil: 0.5 parts;

[0085] Guaiac wood oil: 0.1 part;

[0086] Dioctyl phthalate: 0.05 parts;

[0087] Curing agent: 0.05 parts;

[0088] Anti-aging agent: 0.05 parts.

[0089] The modified microporous silica is prepared by the following steps:

[0090] A1. In parts by weight, 100 parts of 3,7-dimethyl-6-octen-1-ol were added to 300 parts of tetrahydrofuran, and 60 parts of 4-cyclohexanonecarboxylic acid and 20 parts of sodium hydroxide were added, and the mixture was stirred at 40° C. for 18 hours, and salted out and dried to obtain an intermediate;

[0091] A2, adding 10 parts of microporous silica to 20 parts of 0.5 mol / L hydrochloric acid solution, stirring for 1 hour, filtering, and obtaining pretreated microporous silica;

[0092] A3. Add 5 parts of the intermediate to 20 parts of acetone, then add 5 parts of pretreated microporous silica, heat to 90°C, stir for 3 hours, filter and dry to obtain modified microporous silica.

[0093] The method for preparing regenerated asphalt concrete in this embodiment comprises the following steps:

[0094] S1, modified microporous silica, waste mineral oil, guaiac wood oil, dioctyl phthalate, a curing agent and an antioxidant are mixed and stirred, and heated to 110° C. to obtain a mixture;

[0095] S2, crushing the recycled asphalt mixture to an average particle size of less than 0.2 cm and heating it to 110°C;

[0096] S3, heating the SBS modified asphalt to 110°C, then adding the recycled asphalt mixture to the SBS modified asphalt, and then adding the mixture to obtain a recycled asphalt mixture;

[0097] S4. Adding the aggregate to the recycled asphalt mixture to obtain recycled asphalt concrete.

[0098] Example 3

[0099] A regenerated asphalt concrete, the raw materials of which include SBS modified asphalt, recycled asphalt mixture, aggregate, modified microporous silica, waste mineral oil, guaiac wood oil, dioctyl phthalate, curing agent and antioxidant. The antioxidant is polyethylene naphthalate. The curing agent is polyetheramine. The waste mineral oil in this embodiment is a mixture of tar, petroleum residue and deasphalted oil, and the weight ratio of the three is 1:1:1, and the waste mineral oil is pre-filtered, precipitated, flashed, vacuum distilled and hydrofined. The aggregate of the present invention is natural sand.

[0100] In the regenerated asphalt concrete, in parts by weight,

[0101] SBS modified asphalt: 10 parts;

[0102] Recycled asphalt mixture: 44 parts;

[0103] Aggregate: 18 parts;

[0104] Modified microporous silica: 3.8 parts;

[0105] Waste mineral oil: 1.1 parts;

[0106] Guaiac wood oil: 0.3 parts;

[0107] Dioctyl phthalate: 0.08 parts;

[0108] Curing agent: 0.07 parts;

[0109] Anti-aging agent: 0.06 parts.

[0110] The modified microporous silica is prepared by the following steps:

[0111] A1. In parts by weight, 100 parts of 3,7-dimethyl-6-octen-1-ol were added to 250 parts of tetrahydrofuran, and 66 parts of 4-cyclohexanonecarboxylic acid and 13.6 parts of sodium hydroxide were added, and the mixture was stirred at 37° C. for 16 hours, and then salted out and dried to obtain an intermediate;

[0112] A2, adding 10 parts of microporous silica to 15.5 parts of 1.5 mol / L hydrochloric acid solution, stirring for 2 hours, filtering, and obtaining pretreated microporous silica;

[0113] A3. Add 4 parts of the intermediate to 17 parts of acetone, then add 5 parts of pretreated microporous silica, heat to 82°C, stir for 2 hours, filter and dry to obtain modified microporous silica.

[0114] The method for preparing regenerated asphalt concrete in this embodiment comprises the following steps:

[0115] S1, modified microporous silica, waste mineral oil, guaiac wood oil, dioctyl phthalate, a curing agent and an antioxidant are mixed and stirred, and heated to 105° C. to obtain a mixture;

[0116] S2, crushing the recycled asphalt mixture to an average particle size of less than 0.2 cm and heating it to 105°C;

[0117] S3, heating the SBS modified asphalt to 105°C, then adding the recycled asphalt mixture to the SBS modified asphalt, and then adding the mixture to obtain a recycled asphalt mixture;

[0118] S4. Adding the aggregate to the recycled asphalt mixture to obtain recycled asphalt concrete.

[0119] Comparative Example 1

[0120] A regenerated asphalt concrete, the other features of which are the same as those of Example 3, except that: in the regenerated asphalt concrete, in parts by weight,

[0121] SBS modified asphalt: 10 parts;

[0122] Recycled asphalt mixture: 44 parts;

[0123] Aggregate: 18 parts;

[0124] Modified microporous silica: 2 parts;

[0125] Waste mineral oil: 3 parts;

[0126] Guaiac wood oil: 0.05 parts;

[0127] Dioctyl phthalate: 0.08 parts;

[0128] Curing agent: 0.07 parts;

[0129] Anti-aging agent: 0.06 parts.

[0130] Comparative Example 2

[0131] A regenerated asphalt concrete, the other features of which are the same as those of Example 3, except that: in the regenerated asphalt concrete, in parts by weight,

[0132] SBS modified asphalt: 10 parts;

[0133] Recycled asphalt mixture: 44 parts;

[0134] Aggregate: 18 parts;

[0135] Modified microporous silica: 7 parts;

[0136] Waste mineral oil: 0.3 parts;

[0137] Guaiac wood oil: 1 part;

[0138] Dioctyl phthalate: 0.08 parts;

[0139] Curing agent: 0.07 parts;

[0140] Anti-aging agent: 0.06 parts.

[0141] Comparative Example 3

[0142] A regenerated asphalt concrete, the other features of which are the same as those of Example 3, except that no modified microporous silica is added to the raw materials of the regenerated asphalt concrete, and in the regenerated asphalt concrete, in parts by weight,

[0143] SBS modified asphalt: 10 parts;

[0144] Recycled asphalt mixture: 44 parts;

[0145] Aggregate: 18 parts;

[0146] Waste mineral oil: 4.9 parts;

[0147] Guaiac wood oil: 0.3 parts;

[0148] Dioctyl phthalate: 0.08 parts;

[0149] Curing agent: 0.07 parts;

[0150] Anti-aging agent: 0.06 parts.

[0151] The method for preparing regenerated asphalt concrete in this embodiment comprises the following steps:

[0152] S1, waste mineral oil, guaiac wood oil, dioctyl phthalate, a curing agent and an antioxidant are mixed and stirred, and heated to 105° C. to obtain a mixture;

[0153] S2, crushing the recycled asphalt mixture to an average particle size of less than 0.2 cm and heating it to 105°C;

[0154] S3, heating the SBS modified asphalt to 105°C, then adding the recycled asphalt mixture to the SBS modified asphalt, and then adding the mixture to obtain a recycled asphalt mixture;

[0155] S4. Adding the aggregate to the recycled asphalt mixture to obtain recycled asphalt concrete.

[0156] Comparative Example 4

[0157] A regenerated asphalt concrete, the other features of which are the same as those of Example 3, except that no waste mineral oil is added to the raw materials of the regenerated asphalt concrete, and in the regenerated asphalt concrete, by weight,

[0158] SBS modified asphalt: 10 parts;

[0159] Recycled asphalt mixture: 44 parts;

[0160] Aggregate: 18 parts;

[0161] Modified microporous silica: 3.8 parts;

[0162] Guaiac wood oil: 1.4 parts;

[0163] Dioctyl phthalate: 0.08 parts;

[0164] Curing agent: 0.07 parts;

[0165] Anti-aging agent: 0.06 parts.

[0166] The method for preparing regenerated asphalt concrete in this embodiment comprises the following steps:

[0167] S1, modified microporous silica, guaiac wood oil, dioctyl phthalate, a curing agent and an antioxidant are mixed and stirred, and heated to 105° C. to obtain a mixture;

[0168] S2, crushing the recycled asphalt mixture to an average particle size of less than 0.2 cm and heating it to 105°C;

[0169] S3, heating the SBS modified asphalt to 105°C, then adding the recycled asphalt mixture to the SBS modified asphalt, and then adding the mixture to obtain a recycled asphalt mixture;

[0170] S4. Adding the aggregate to the recycled asphalt mixture to obtain recycled asphalt concrete.

[0171] Comparative Example 5

[0172] A regenerated asphalt concrete, the other features of which are the same as those of Example 3, except that guaiac wood oil is not added to the raw materials of the regenerated asphalt concrete, and in the regenerated asphalt concrete, in parts by weight,

[0173] SBS modified asphalt: 10 parts;

[0174] Recycled asphalt mixture: 44 parts;

[0175] Aggregate: 18 parts;

[0176] Modified microporous silica: 3.8 parts;

[0177] Waste mineral oil: 1.4 parts;

[0178] Dioctyl phthalate: 0.08 parts;

[0179] Curing agent: 0.07 parts;

[0180] Anti-aging agent: 0.06 parts.

[0181] The method for preparing regenerated asphalt concrete in this embodiment comprises the following steps:

[0182] S1, modified microporous silica, waste mineral oil, dioctyl phthalate, a curing agent and an anti-aging agent are mixed and stirred, and heated to 105° C. to obtain a mixture;

[0183] S2, crushing the recycled asphalt mixture to an average particle size of less than 0.2 cm and heating it to 105°C;

[0184] S3, heating the SBS modified asphalt to 105°C, then adding the recycled asphalt mixture to the SBS modified asphalt, and then adding the mixture to obtain a recycled asphalt mixture;

[0185] S4. Adding the aggregate to the recycled asphalt mixture to obtain recycled asphalt concrete.

[0186] Comparative Example 6

[0187] A regenerated asphalt concrete, the other features of which are the same as those of Example 3, except that the modified microporous silica is replaced with microporous silica in the raw materials of the regenerated asphalt concrete.

[0188] Effect example

[0189] The performance of the recycled asphalt concrete prepared by Example 1 to Example 3 and Comparative Example 1 to Comparative Example 6 was tested. The penetration was tested according to GB / T4509-2010 "Asphalt Penetration Test Method". The ductility was measured according to GB / T4508-2010 "Asphalt Ductility Test Method". The dynamic stability was measured according to T0719-2011 in JTGE20-2011 "Test Procedure for Asphalt and Asphalt Mixtures in Highway Engineering", where the test size was 300mm*300mm*50mm plate specimen, the test temperature was 60°C, the wheel pressure load was 0.7MPa, and the repeated wheel pressure time was 60min. The asphalt mixture bending test procedure in JTGE20-2011 "Test Procedure for Asphalt and Asphalt Mixtures in Highway Engineering" was used to conduct the low-temperature crack resistance experiment; the specimen size was 250mm±2mm in length, 30mm±2mm in width, 35mm±2mm in height, 200mm±0.5mm in span, the test temperature was -10℃±0.5℃, and the loading rate was 50mm / min. The asphalt mixture bending tensile strength test procedure in JTGE20-2011 "Test Procedure for Asphalt and Asphalt Mixtures in Highway Engineering" was used to conduct the bending tensile strength test, in which the bending tensile strength was prepared into a rutting plate specimen with a height of 35mm, a length of 250mm, and a width of 30mm, and was tested at a temperature of -10℃ and a loading rate of 500mm / min.

[0190] The corresponding Tables 1 and 2 are obtained.

[0191] Table 1. Test results of recycled asphalt concrete performance of Examples 1 to 3

[0192]

[0193] Table 2. Performance test results of recycled asphalt concrete of Comparative Examples 1 to 6

[0194]

[0195] As can be seen from the above table, the needle penetration of the recycled concrete obtained in Examples 1 to 3 of the present invention is between 26 and 27, and its viscosity is better. The dynamic stability of the recycled concrete of the present invention is in the range of 6334 times / mm to 6456 times / mm, and can meet the use requirements of summer hot areas in terms of high temperature rutting resistance. The maximum bending and tensile strain of the recycled concrete is ≥3000με, and the low temperature crack resistance meets the use requirements of winter cold areas. The bending and tensile failure strength of the present invention is greater than 23.3MPa, and its strength is relatively large. It can be seen from Example 3 and Comparative Examples 3 to Comparative Examples 6 that the recycled concrete of the present invention can significantly improve the high temperature rutting resistance, low temperature crack resistance and bending and tensile failure strength when modified microporous silica, waste mineral oil and guaiac wood oil are present at the same time. At the same time, the above data show that the present invention can further improve the above performance through the reasonable proportion of each component and appropriate preparation conditions.

[0196] It can be seen that the recycled concrete of the present invention still has good high-temperature rutting resistance and low-temperature cracking resistance, etc., when the proportion of recycled asphalt mixture is greater than 50%, and the flexural tensile strength is relatively high.

[0197] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. A regenerated asphalt concrete, characterized in that: The raw materials include SBS modified asphalt, recycled asphalt mixture, aggregate, modified microporous silica, waste mineral oil, guaiac wood oil, dioctyl phthalate, curing agent and anti-aging agent; The modified microporous silica is prepared by the following steps: A1, adding 3,7-dimethyl-6-octen-1-ol to tetrahydrofuran, and adding 4-cyclohexanonecarboxylic acid and sodium hydroxide to obtain an intermediate; A2, adding microporous silica to hydrochloric acid, stirring and filtering to obtain pretreated microporous silica; A3. Add the intermediate to acetone, then add the pretreated microporous silica, and heat to obtain modified microporous silica.

2. The regenerated asphalt concrete according to claim 1, characterized in that: In parts by weight, SBS modified asphalt: 10 parts; Recycled asphalt mixture: 40 to 50 parts; Aggregate: 10 to 25 parts; Modified microporous silica: 3 to 5 parts; Waste mineral oil: 0.5 to 2 parts; Guaiac wood oil: 0.1 to 0.5 parts; Dioctyl phthalate: 0.05 to 0.1 parts; Curing agent: 0.05 to 0.1 parts; Anti-aging agent: 0.05 to 0.1 parts.

3. The regenerated asphalt concrete according to claim 2, characterized in that: In parts by weight, SBS modified asphalt: 10 parts; Recycled asphalt mixture: 44 parts; Aggregate: 18 parts; Modified microporous silica: 3.8 parts; Waste mineral oil: 1.1 parts; Guaiac wood oil: 0.3 parts; Dioctyl phthalate: 0.08 parts; Curing agent: 0.07 parts; Anti-aging agent: 0.06 parts.

4. The regenerated asphalt concrete according to claim 1, characterized in that: The modified microporous silica is prepared by the following steps: A1. In parts by weight, add 100 parts of 3,7-dimethyl-6-octen-1-ol to 200-300 parts of tetrahydrofuran, and add 60-80 parts of 4-cyclohexanonecarboxylic acid and 10-20 parts of sodium hydroxide, stir at 30° C. to 40° C. for 14 h to 18 h, and salt out and dry to obtain an intermediate; A2, adding 10 parts of microporous silica to 10 to 20 parts of 0.5 mol / L to 2 mol / L hydrochloric acid solution, stirring for 1 h to 3 h, filtering, and obtaining pretreated microporous silica; A3. Add 3 to 5 parts of the intermediate to 10 to 20 parts of acetone, then add 5 parts of pretreated microporous silica, heat to 70°C to 90°C, stir for 1 to 3 hours, filter and dry to obtain modified microporous silica.

5. The regenerated asphalt concrete according to claim 4, characterized in that: The modified microporous silica is prepared by the following steps: A1. In parts by weight, 100 parts of 3,7-dimethyl-6-octen-1-ol were added to 250 parts of tetrahydrofuran, and 66 parts of 4-cyclohexanonecarboxylic acid and 13.6 parts of sodium hydroxide were added, and the mixture was stirred at 37° C. for 16 hours, and then salted out and dried to obtain an intermediate; A2, adding 10 parts of microporous silica to 15.5 parts of 1.2 mol / L hydrochloric acid solution, stirring for 2 hours, filtering, and obtaining pretreated microporous silica; A3. Add 4 parts of the intermediate to 17 parts of acetone, then add 5 parts of pretreated microporous silica, heat to 82°C, stir for 2 hours, filter and dry to obtain modified microporous silica.

6. The regenerated asphalt concrete according to claim 5, characterized in that: The anti-aging agent is polyethylene naphthalate or phenyl-α-naphthylamine.

7. The regenerated asphalt concrete according to claim 6, characterized in that: The curing agent is polyetheramine or catechol.

8. A method for preparing regenerated asphalt concrete according to any one of claims 1 to 7, characterized in that: The steps include: S1, modified microporous silica, waste mineral oil, guaiac wood oil, dioctyl phthalate, a curing agent and an anti-aging agent are mixed and stirred to obtain a mixture; S2, crushing the recycled asphalt mixture; S3, heating the SBS modified asphalt, then adding the recycled asphalt mixture to the SBS modified asphalt, and then adding the mixture to obtain a recycled asphalt mixture; S4. Adding the aggregate to the recycled asphalt mixture to obtain recycled asphalt concrete.

9. The preparation method according to claim 8, characterized in that: The steps include: S1, modified microporous silica, waste mineral oil, guaiac wood oil, dioctyl phthalate, a curing agent and an anti-aging agent are mixed and stirred, and heated to 100° C. to 120° C. to obtain a mixture; S2, crushing the recycled asphalt mixture to an average particle size of less than 0.2 cm, and heating to 100°C to 110°C; S3, heating the SBS modified asphalt to 100°C to 110°C, then adding the recycled asphalt mixture to the SBS modified asphalt, and then adding the mixture to obtain a recycled asphalt mixture; S4. Adding the aggregate to the recycled asphalt mixture to obtain recycled asphalt concrete.

Citation Information

Patent Citations

  • Asphalt mastic macadam mixture and preparation method thereof

    CN109231890A

  • Recycled asphalt concrete and preparation method thereof

    CN109608093A

  • High-permeability environment-friendly medium-temperature regenerant for asphalt and preparation method thereof

    CN113999538A

  • Asphalt regenerant and preparation method thereof

    CN115353665A

  • Composite high-RAP-doping-amount efficient asphalt regenerant and preparation method thereof

    CN117024976A