Nano agglomerated rare earth doped YSZ powder and preparation method thereof

Through surface modification and multiple sintering treatments of metal ion solution, nano-agglomerated rare earth doped YSZ powder was prepared, which solved the problem of volume expansion and insufficient performance of YSZ materials at high temperatures, and improved the high-temperature performance and life of the coating. , and realizes efficient and low-cost powder preparation.

CN118993728AActive Publication Date: 2024-11-22XIAN RARE METAL MATERIALS RES INST CO LTD

Patent Information

Application Number
CN202411137296.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-11-22
Estimated Expiration
2044-08-19

AI Technical Summary

Technical Problem

The volume expansion of YSZ material due to the transformation from four-sided phase to single-climbed phase at high temperatures, resulting in cracks and failure of thermal barrier coatings. The existing rare earth doped YSZ powder preparation process is difficult to ensure that the rare earth elements completely enter the zirconia lattice, resulting in material performance. insufficient.

Method used

The metal ion solution is surface modified by dispersant, and nano-agglomerated rare earth doped YSZ powder is prepared through precipitation, ultrasonication, calcination and sintering, ensuring that the rare earth elements enter the zirconia lattice, and achieving high quality through multiple sintering treatments. Dispersibility and densification.

Benefits of technology

It improves the high-temperature performance of YSZ coating, extends the life of the coating, and realizes the preparation of high dispersion and uniform nanopowders, with high processing efficiency and low cost, which is suitable for industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118993728A_ABST
    Figure CN118993728A_ABST
Patent Text Reader

Abstract

The invention provides nano agglomerated rare earth doped YSZ powder and a preparation method thereof, and relates to the technical field of ceramic powder preparation. The preparation method comprises the following steps: carrying out surface modification treatment on a metal ion solution by using a dispersing agent to obtain a reaction solution; wherein the metal ion solution comprises zirconium salt, yttrium salt and at least one rare earth salt except the yttrium salt; performing aging treatment, ultrasonic treatment and drying treatment on the reaction solution to obtain rare earth doped YSZ precursor powder; calcining the rare earth doped YSZ precursor powder for at least two times to obtain rare earth doped YSZ nano powder; preparing the rare earth doped YSZ nano powder and deionized water into slurry, and carrying out ball milling on the slurry to obtain a rare earth doped YSZ aggregate; sintering the rare earth doped YSZ aggregate for at least two times to obtain intermediate powder; and sieving the intermediate powder to obtain the nano agglomerated rare earth doped YSZ powder. The performance of the YSZ material can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to the technical field of ceramic powder preparation, and in particular to a preparation method of nano-agglomerated rare earth-doped YSZ powder and nano-agglomerated rare earth-doped YSZ powder. Background Art

[0002] Thermal barrier coatings are widely used in high-temperature components such as aircraft engines, combustion chambers, and spacecraft. They can effectively reduce the damage to materials caused by high temperatures and extend the service life of workpieces. Yttria-Stabilized Zirconia (YSZ) is widely used in thermal barrier coatings due to its low thermal conductivity, high thermal expansion coefficient, and good chemical stability.

[0003] However, when the operating temperature is above 1200℃ for a long time, the YSZ material will undergo a transformation from tetragonal phase to monoclinic phase, causing the thermal barrier coating to expand in volume, resulting in cracks in the coating and causing it to peel off and fail.

[0004] In order to solve the above problems, some technologies have improved the life of YSZ coatings by rare earth doping. The preparation process of rare earth doped YSZ powder currently mainly relies on mixed ball milling of oxide powders and rare earth doping by solid diffusion. However, this method makes it difficult to ensure that the rare earth elements are completely incorporated into the zirconia lattice, resulting in insufficient performance of rare earth doped YSZ materials.

[0005] It should be noted that the information disclosed in the above background technology section is only used to enhance the understanding of the background of the present disclosure, and therefore may include information that does not constitute the prior art known to ordinary technicians in the field. Summary of the invention

[0006] The purpose of the present disclosure is to provide a method for preparing nano-agglomerated rare earth-doped YSZ powder and nano-agglomerated rare earth-doped YSZ powder, thereby overcoming the problem of insufficient performance of YSZ materials at least to a certain extent.

[0007] According to a first aspect of the present disclosure, a method for preparing nano-agglomerated rare earth-doped YSZ powder is provided, comprising: performing surface modification treatment on a metal ion solution using a dispersant to obtain a reaction solution; wherein the metal ion solution contains a zirconium salt, a yttrium salt and at least one rare earth salt other than the yttrium salt; performing aging treatment, ultrasonic treatment and drying treatment on the reaction solution to obtain a rare earth-doped YSZ precursor powder; performing at least two calcination treatments on the rare earth-doped YSZ precursor powder to obtain a rare earth-doped YSZ nanopowder; preparing a slurry with the rare earth-doped YSZ nanopowder and deionized water, and ball milling the slurry to obtain a rare earth-doped YSZ agglomerate; performing at least two sintering treatments on the rare earth-doped YSZ agglomerate to obtain an intermediate powder; and sieving the intermediate powder to obtain a nano-agglomerated rare earth-doped YSZ powder.

[0008] Optionally, the metal ion solution is surface modified by using a dispersant to obtain a reaction solution, including: adding the metal ion solution and the dispersant to an impinging stream reactor filled with deionized water; dripping a precipitant into the impinging stream reactor, and combining the stirring operation and ultrasonic operation of the impinging stream reactor to obtain a reaction solution; wherein the precipitant is used to adjust the pH of the solution.

[0009] Optionally, the precipitant is one or more of ammonium bicarbonate, ammonium hydroxide, and urea; wherein the pH of the reaction solution is adjusted to 8 to 11.

[0010] Optionally, the stirring speed of the impinging stream reactor is 400 r / min to 2000 r / min, and the ultrasonic power is 10 KHz to 100 KHz.

[0011] Optionally, the zirconium salt is zirconium nitrate or zirconium oxychloride, the yttrium salt is yttrium nitrate or yttrium chloride, the rare earth salt includes gadolinium salt and / or ytterbium salt, the gadolinium salt is gadolinium nitrate or gadolinium chloride, and the ytterbium salt is ytterbium nitrate or ytterbium chloride; the dispersant is a mixture of one or more of polyvinyl pyrrolidone, hexadecyltrimethylammonium bromide, polyethylene glycol ethoxylates, and polyethylene glycol.

[0012] Optionally, the reaction solution is aged, ultrasonically treated and dried to obtain a rare earth-doped YSZ precursor powder, including: aging the reaction solution to obtain a first solution; ultrasonically dispersing the first solution using an ultrasonic cell crusher to obtain a second solution; the frequency of the ultrasonic cell crusher is 10KHz to 100KHz, and the ultrasonic time is 10min to 200min; the second solution is dried using a vacuum freeze dryer to obtain a rare earth-doped YSZ precursor powder; the drying time of the vacuum freeze dryer is 10h to 24h.

[0013] Optionally, the calcination temperature of each of the at least two calcination treatments is 400° C. to 800° C., and the calcination time of each calcination treatment is 1 h to 10 h.

[0014] Optionally, the sintering temperature of each of the at least two sintering treatments is 900° C. to 1300° C., and the sintering time of each sintering treatment is 2 h to 10 h.

[0015] Optionally, sieving the intermediate powder includes: sieving the intermediate powder based on a sieving operation with a sieving mesh number of 200 mesh to 1000 mesh.

[0016] According to a second aspect of the present disclosure, a nano-agglomerated rare earth-doped YSZ powder is provided. The nano-agglomerated rare earth-doped YSZ powder is prepared by any of the above-mentioned methods for preparing nano-agglomerated rare earth-doped YSZ powder.

[0017] According to the preparation scheme of the nano-agglomerated rare earth-doped YSZ powder of the embodiment of the present disclosure, on the one hand, rare earth elements are added to YSZ by means of a metal salt solution deposition reaction, which can promote the entry of rare earth elements into the zirconia lattice, effectively improve the high temperature performance of the material, and thus help to improve the life of the coating prepared therefrom; on the other hand, the metal salt solution reaction combined with a dispersant and at least two calcination treatments of the present disclosure help to obtain highly dispersed and uniform nanopowders; on another hand, at least two sintering treatments of the present disclosure can densify the rare earth-doped YSZ nanopowder while retaining uniformity; on another hand, the preparation scheme of the present disclosure has high processing efficiency, simple operation, low cost and is easy to industrialize and apply.

[0018] It is to be understood that the foregoing general description and the following detailed description are exemplary and explanatory only and are not restrictive of the present disclosure. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] The accompanying drawings herein are incorporated into the specification and constitute a part of the specification, illustrate embodiments consistent with the present disclosure, and together with the specification are used to explain the principles of the present disclosure. Obviously, the accompanying drawings described below are only some embodiments of the present disclosure, and for ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without creative work.

[0020] Figure 1 The flowchart of the method for preparing nano-agglomerated rare earth-doped YSZ powder according to an exemplary embodiment of the present disclosure is schematically shown.

[0021] Figure 2 The XRD (X-Ray Diffractometer) diagram of the rare earth-doped YSZ nanopowder of Example 1 of the present disclosure is shown.

[0022] Figure 3 A scanning micrograph of the rare earth-doped YSZ nanopowder of Example 1 of the present disclosure is shown.

[0023] Figure 4 The XRD pattern of the nano-agglomerated rare earth-doped YSZ powder of Example 1 of the present disclosure is shown.

[0024] Figure 5 A scanning micrograph of the nano-agglomerated rare earth-doped YSZ powder of Example 1 of the present disclosure is shown. DETAILED DESCRIPTION

[0025] Example embodiments will now be described more fully with reference to the accompanying drawings. However, example embodiments can be implemented in a variety of forms and should not be construed as being limited to the examples set forth herein; on the contrary, these embodiments are provided so that the present disclosure will be more comprehensive and complete, and the concepts of the example embodiments are fully conveyed to those skilled in the art. The described features, structures, or characteristics may be combined in any suitable manner in one or more embodiments. In the following description, many specific details are provided to provide a full understanding of the embodiments of the present disclosure. However, those skilled in the art will appreciate that the technical solutions of the present disclosure may be practiced while omitting one or more of the specific details, or other methods, processes, steps, etc. may be adopted. In other cases, known technical solutions are not shown or described in detail to avoid obscuring various aspects of the present disclosure.

[0026] In addition, the accompanying drawings are only schematic illustrations of the present disclosure and are not necessarily drawn to scale. The same reference numerals in the figures represent the same or similar parts, and thus their repeated descriptions will be omitted. The flowcharts shown in the accompanying drawings are only exemplary illustrations and do not necessarily include all the steps. For example, some steps can also be decomposed, while some steps can be combined or partially combined, so the actual execution order may change according to actual conditions. In addition, all the terms "first", "second", etc. below are only for the purpose of distinction and should not be used as limitations of the present disclosure.

[0027] Figure 1 The flowchart of the method for preparing nano-agglomerated rare earth-doped YSZ powder according to an exemplary embodiment of the present disclosure is schematically shown. Figure 1 The method for preparing the nano-agglomerated rare earth-doped YSZ powder according to the embodiment of the present disclosure comprises the following steps:

[0028] S102. Performing surface modification treatment on the metal ion solution using a dispersant to obtain a reaction solution; wherein the metal ion solution comprises a zirconium salt, a yttrium salt and at least one rare earth salt other than the yttrium salt.

[0029] In an exemplary embodiment of the present disclosure, the metal ion solution may include a zirconium salt, a yttrium salt, and at least one rare earth salt other than the yttrium salt. The zirconium salt may be zirconium nitrate (Zr(NO3)4·H2O) or zirconium oxychloride (ZrOCl2·8H2O); the yttrium salt may be yttrium nitrate (Y(NO3)3·H2O) or yttrium chloride (YCl3·6H2O); the rare earth salt may include a gadolinium salt and / or a ytterbium salt, the gadolinium salt may be gadolinium nitrate (Gd(NO3)3·H2O) or gadolinium chloride (GdCl3·6H2O), and the ytterbium salt may be ytterbium nitrate (Yb(NO3)3·H2O) or ytterbium chloride (YbCl3·6H2O).

[0030] In addition, the dispersant used in the present disclosure can be a mixture of one or more of polyvinyl pyrrolidone, hexadecyltrimethylammonium bromide, polyethylene glycol ethoxylates, and polyethylene glycol.

[0031] It should be understood that the zirconium salt, yttrium salt, and at least one rare earth salt other than the yttrium salt contained in the above-mentioned dispersant and the metal ion solution are merely exemplary descriptions, and the present disclosure does not limit this.

[0032] According to some embodiments of the present disclosure, a dispersant and a metal ion solution may be added to a container and mixed by heating and ultrasonic treatment to obtain a reaction solution.

[0033] According to other embodiments of the present disclosure, the pH of the solution can be regulated by adjusting the rotation speed and ultrasonic power of the impinging stream reactor and the type of precipitant to obtain a reaction solution.

[0034] Specifically, the metal ion solution and the dispersant can be added into an impinging stream reactor filled with deionized water, and then the precipitant is added dropwise into the impinging stream reactor, and the reaction solution is obtained by combining the stirring operation and ultrasonic operation of the impinging stream reactor.

[0035] The precipitant can be used to adjust the pH of the solution, and can be a mixture of one or more of ammonium bicarbonate, ammonium hydroxide, and urea. In addition, the pH of the obtained reaction solution is adjusted to 8 to 11.

[0036] In order to achieve good high dispersibility, high purity and size uniformity, these embodiments adopt a method of combining dispersant modification, adjusting the speed of the impinging stream reactor and the ultrasonic power. Specifically, the stirring speed of the impinging stream reactor is 400r / min to 2000r / min, and the ultrasonic power is 10KHz to 100KHz.

[0037] S104. Perform aging treatment, ultrasonic treatment and drying treatment on the reaction solution to obtain rare earth-doped YSZ precursor powder.

[0038] After the reaction solution is obtained in step S102, the reaction solution may be aged. The present disclosure does not limit the aging time, for example, 10 hours to 30 hours. In the present embodiment, the solution obtained after the aging treatment is recorded as the first solution.

[0039] Next, the first solution can be ultrasonically dispersed using an ultrasonic cell pulverizer to obtain a second solution, wherein the frequency of the ultrasonic cell pulverizer is 10 KHz to 100 KHz and the ultrasonic time is 10 min to 200 min.

[0040] Subsequently, the second solution can be dried using a vacuum freeze dryer to obtain rare earth-doped YSZ precursor powder, wherein the drying time of the vacuum freeze dryer is 10 hours to 24 hours.

[0041] S106. The rare earth-doped YSZ precursor powder is calcined at least twice to obtain rare earth-doped YSZ nanopowder.

[0042] After obtaining the rare earth-doped YSZ precursor powder in step S104, the powder may be subjected to multiple calcination treatments. The present disclosure does not limit the number of calcination treatments. The calcination temperature of each calcination treatment is 400° C. to 800° C., and the calcination time of each calcination treatment is 1 h to 10 h.

[0043] It should be noted that, in some embodiments of the present disclosure, the temperature of each calcination process may be higher than the temperature of the previous calcination process, for example, the temperature of the second calcination process is higher than the temperature of the first calcination process. However, in other embodiments of the present disclosure, each calcination process is regarded as an independent process, and its temperature is not limited by the temperature of other calcination processes.

[0044] S108. Prepare a slurry by mixing rare earth-doped YSZ nanopowder with deionized water, and ball-mill the slurry to obtain rare earth-doped YSZ agglomerates.

[0045] In an exemplary embodiment of the present disclosure, the slurry concentration is configured to be 10wt% to 50wt%. The ball milling time can be configured to be 0.5h to 5h. In addition, the present disclosure does not limit the ball milling process, for example, the ball milling process is performed using alumina balls and alumina ball milling jars, and the present disclosure does not limit the diameter of the alumina balls, the ball-to-material ratio, the rotation speed of the ball milling process, the ball milling time, etc.

[0046] S110. Sintering the rare earth-doped YSZ agglomerate at least twice to obtain an intermediate powder.

[0047] After the rare earth-doped YSZ agglomerate is obtained in step S108, the agglomerate may be subjected to multiple sintering treatments. The present disclosure does not limit the number of sintering treatments. The sintering temperature of each sintering treatment is 900° C. to 1300° C., and the sintering time of each sintering treatment is 2 h to 10 h.

[0048] Taking the double sintering process as an example, the first sintering process can obtain a porous sample with a high grain growth index and good microstructure uniformity. After the second sintering process, the sintered body can be densified through grain boundary diffusion without grain growth. Therefore, by adjusting the sintering temperature and sintering time, the material can be densified while retaining uniformity.

[0049] S112. Screen the intermediate powder to obtain nano-agglomerated rare earth-doped YSZ powder.

[0050] In an exemplary embodiment of the present disclosure, the intermediate powder obtained after sintering is sieved to obtain the nano-agglomerated rare earth-doped YSZ powder of the present disclosure. Specifically, the intermediate powder can be sieved based on a sieving operation with a sieving mesh number of 200 to 1000 mesh.

[0051] Through the preparation process from step S102 to step S112, it is tested that the flowability of the powder obtained is 50s / 50g to 54s / 50g, and the bulk density is 1.8g / cc to 2.0g / cc.

[0052] The preparation process of the nano-agglomerated rare earth-doped YSZ powder disclosed in the present invention will be described in detail below through examples.

[0053] Example 1

[0054] Provided is a method for preparing a nano-agglomerated rare earth-doped YSZ powder having a material composition of 5.0 mol% Gd2O3: 6.0 mol% Yb2O3: 9 mol% Y2O3: 80.0 mol% ZrO2, abbreviated as 5Gd6Yb9YSZ, comprising the following steps:

[0055] Step 1: Calculate the mass of Gd(NO3)3·H2O, Yb(NO3)3·H2O, Y(NO3)3·H2O, and Zr(NO3)4·H2O according to the molar ratio of Gd2O3:Yb2O3:Y2O3:ZrO2 of 5:6:9:80, thereby obtaining a metal ion solution having these compositions, and adding the metal ion solution to an impinging stream reactor filled with 200 mL of deionized water to make the solution concentration 0.15 mol / L, adding 0.5 wt% polyvinyl pyrrolidone dispersant and stirring until clarified. The stirring speed of the impinging stream reactor is 800 r / min, the ultrasonic power is 20 KHz, and 0.5 mol / L ammonium hydroxide solution is added dropwise at a rate of 5 mL / min to make the solution pH 11. Thus, the reaction solution described in the present disclosure is obtained.

[0056] Step 2: The reaction solution obtained in step 1 was aged for 10 hours, then ultrasonically dispersed at a frequency of 20 kHz for 20 minutes using an ultrasonic cell crusher, and dried for 10 hours using a vacuum freeze dryer to obtain a 5Gd6Yb9YSZ precursor powder.

[0057] Step 3: The precursor powder obtained in step 2 was calcined at 400°C for 1 h and then calcined at 800°C for 1 h to obtain 5Gd6Yb9YSZ nanopowder with high dispersibility, high purity and size uniformity.

[0058] Figure 2 The XRD spectrum of the 5Gd6Yb9YSZ nanopowder is shown in Fig. Figure 2 It can be seen that the nanopowder has no diffraction peaks of Gd2O3, Yb2O3, and Y2O3, indicating that Gd 3+ , Yb 3+ and Y 3+ Evenly dispersed in the gel, and replaced Zr 4+ A substitutional solid solution is formed and exists stably in the form of a single tetragonal phase.

[0059] Figure 3 The corresponding scanning micrographs are shown in Ref. Figure 2 It can be seen that the 5Gd6Yb9YSZ nanopowder obtained in this step has high dispersibility and size uniformity.

[0060] Step 4: The 5Gd6Yb9YSZ nanopowder obtained in step 3 is prepared into a slurry with a concentration of 10 wt%, ball-milled for 0.5 h, and then spray-dried.

[0061] Step 5: The sample spray-dried in step 4 was sintered at 1200° C. for 1 h and then sintered at 1100° C. for 10 h to obtain a densified 5Gd6Yb9YSZ nano-agglomerated rare earth-doped YSZ powder.

[0062] Figure 4 The XRD spectrum of the 5Gd6Yb9YSZ nanoagglomerated powder is shown in FIG. Figure 2 It can be seen that the nanopowder still exists stably as a single tetragonal phase of ZrO2, and its crystallinity is significantly improved.

[0063] Step 6: The densified powder obtained in step 5 is sieved through 325 mesh and 800 mesh to obtain 5Gd6Yb9YSZ nano-agglomerated rare earth-doped YSZ powder with a size of 18 μm to 45 μm.

[0064] Figure 5 The scanning micrograph of the nano-agglomerated rare earth doped YSZ powder of Example 1 of the present disclosure is shown, wherein the observation scales of Figure a and Figure b are different, Figure a is at a scale of 200 μm, and Figure b is at a scale of 100 μm. Figure 5 It can be seen that the powder has good sphericity. At the same time, its fluidity is 50s / 50g and its bulk density is 2.0g / cc.

[0065] Example 2

[0066] Provided is a method for preparing a nano-agglomerated rare earth-doped YSZ powder having a material composition of 4.0 mol% Gd2O3: 5.0 mol% Yb2O3: 8 mol% Y2O3: 83.0 mol% ZrO2, abbreviated as 4Gd5Yb8YSZ, comprising the following steps:

[0067] Step 1: Calculate the mass of GdCl3·6H2O, YbCl3·6H2O, YCl3·6H2O, and ZrOCl2·8H2O according to the molar ratio of Gd2O3:Yb2O3:Y2O3:ZrO2 of 4:5:8:83, thereby obtaining a metal ion solution having these compositions, and add the metal ion solution into an impinging stream reactor filled with 200 mL of deionized water to make the solution concentration 0.3 mol / L, add 1 wt% hexadecyltrimethylammonium bromide dispersant and stir until clarified. The stirring speed of the impinging stream reactor is 1000 r / min, the ultrasonic power is 30 KHz, and 0.5 mol / L ammonium bicarbonate solution is added dropwise at a rate of 10 mL / min to make the solution pH 10. Thus, the reaction solution described in the present disclosure is obtained.

[0068] Step 2: The reaction solution obtained in step 1 was aged for 15 hours, then ultrasonically dispersed at a frequency of 30 kHz for 30 minutes using an ultrasonic cell crusher, and dried for 15 hours using a vacuum freeze dryer to obtain a 4Gd5Yb8YSZ precursor powder.

[0069] Step 3: The precursor powder obtained in step 2 was calcined at 500°C for 2 h and then calcined at 700°C for 2 h to obtain 4Gd5Yb8YSZ nanopowder with high dispersibility, high purity and size uniformity.

[0070] Step 4: The 4Gd5Yb8YSZ nanopowder obtained in step 3 is prepared into a slurry with a concentration of 40 wt%, ball-milled for 1 h, and then spray-dried.

[0071] Step 5: The sample spray-dried in step 4 was sintered at 1100° C. for 2 h and then sintered at 1000° C. for 5 h to obtain a densified 4Gd5Yb8YSZ nano-agglomerated rare earth-doped YSZ powder.

[0072] Step 6: The densified powder obtained in step 5 is sieved through 200 mesh and 600 mesh to obtain 4Gd5Yb8YSZ nano-agglomerated rare earth doped YSZ powder with a size of 23 μm to 75 μm. The flowability is 54 s / 50 g and the bulk density is 1.8 g / cc.

[0073] Example 3

[0074] Provided is a method for preparing a nano-agglomerated rare earth-doped YSZ powder having a material composition of 3.0 mol% Gd2O3: 3.0 mol% Yb2O3: 4 mol% Y2O3: 90.0 mol% ZrO2, abbreviated as 3Gd3Yb4YSZ, comprising the following steps:

[0075] Step 1: Calculate the mass of Gd(NO3)3·H2O, Yb(NO3)3·H2O, Y(NO3)3·H2O, and Zr(NO3)4·H2O according to the molar ratio of Gd2O3:Yb2O3:Y2O3:ZrO2 of 3:3:4:90, thereby obtaining a metal ion solution having these compositions, and add the metal ion solution into an impinging stream reactor filled with 200 mL of deionized water to make the solution concentration 0.5 mol / L, add 0.5 wt% of polyethylene glycol ethoxylate dispersant and stir until clarified. The stirring speed of the impinging stream reactor is 2000 r / min, the ultrasonic power is 20 KHz, and 0.5 mol / L urea solution is added dropwise at a rate of 5 mL / min to make the solution pH 8. Thus, the reaction solution described in the present disclosure is obtained.

[0076] Step 2: The reaction solution obtained in step 1 was aged for 24 hours, then ultrasonically dispersed at a frequency of 70 kHz for 40 minutes using an ultrasonic cell crusher, and dried for 24 hours using a vacuum freeze dryer to obtain a 3Gd3Yb4YSZ precursor powder.

[0077] Step 3: The precursor powder obtained in step 2 was calcined at 400°C for 1 h and then calcined at 700°C for 6 h to obtain 3Gd3Yb4YSZ nanopowder with high dispersibility, high purity and size uniformity.

[0078] Step 4: The 3Gd3Yb4YSZ nanopowder obtained in step 3 is prepared into a slurry with a concentration of 25 wt%, ball-milled for 0.5 h, and then spray-dried.

[0079] Step 5: The sample spray-dried in step 4 was sintered at 1300° C. for 1 h and then sintered at 900° C. for 10 h to obtain a densified 3Gd3Yb4YSZ nano-agglomerated rare earth-doped YSZ powder.

[0080] Step 6: The densified powder obtained in step 5 is sieved through 300 mesh and 1000 mesh to obtain 3Gd3Yb4YSZ nano-agglomerated rare earth doped YSZ powder with a size of 13 μm to 48 μm. The flowability is 52 s / 50 g and the bulk density is 1.94 g / cc.

[0081] Furthermore, the embodiment of the present disclosure also provides a nano-agglomerated rare earth-doped YSZ powder, and the nano-agglomerated rare earth-doped YSZ powder is prepared by the above-mentioned preparation method of the nano-agglomerated rare earth-doped YSZ powder.

[0082] Furthermore, the embodiments of the present disclosure also provide a thermal barrier coating, which is prepared using the above-mentioned nano-agglomerated rare earth-doped YSZ powder.

[0083] It should be noted that although the steps of the method in the present disclosure are described in a specific order in the drawings, this does not require or imply that the steps must be performed in this specific order, or that all the steps shown must be performed to achieve the desired results. Additionally or alternatively, some steps may be omitted, multiple steps may be combined into one step, and / or one step may be decomposed into multiple steps, etc.

[0084] In addition, the above-mentioned figures are only schematic illustrations of the processes included in the method according to the exemplary embodiments of the present disclosure, and are not intended to be limiting. It is easy to understand that the processes shown in the above-mentioned figures do not indicate or limit the time sequence of these processes. In addition, it is also easy to understand that these processes can be performed synchronously or asynchronously, for example, in multiple modules.

[0085] Those skilled in the art will readily appreciate other embodiments of the present disclosure after considering the specification and practicing what is disclosed herein. This application is intended to cover any variations, uses, or adaptations of the present disclosure that follow the general principles of the present disclosure and include common knowledge or customary technical means in the art that are not disclosed in the present disclosure. The specification and embodiments are to be considered merely as exemplary, and the true scope and spirit of the present disclosure are indicated by the claims.

[0086] It should be understood that the present disclosure is not limited to the exact structures that have been described above and shown in the drawings, and that various modifications and changes may be made without departing from the scope thereof. The scope of the present disclosure is limited only by the appended claims.

Claims

1. A method for preparing nano-agglomerated rare earth-doped YSZ powder, characterized in that: include: Using a dispersant to perform surface modification treatment on a metal ion solution to obtain a reaction solution; wherein the metal ion solution comprises a zirconium salt, a yttrium salt, and at least one rare earth salt other than the yttrium salt; The reaction solution is subjected to aging treatment, ultrasonic treatment and drying treatment to obtain rare earth-doped YSZ precursor powder; Calcining the rare earth-doped YSZ precursor powder at least twice to obtain rare earth-doped YSZ nanopowder; The rare earth-doped YSZ nanopowder and deionized water are mixed into a slurry, and the slurry is ball-milled to obtain rare earth-doped YSZ agglomerates; sintering the rare earth-doped YSZ agglomerate at least twice to obtain an intermediate powder; The intermediate powder is sieved to obtain nano-agglomerated rare earth-doped YSZ powder.

2. The preparation method according to claim 1, characterized in that: The metal ion solution is subjected to surface modification treatment using a dispersant to obtain a reaction solution, comprising: adding a metal ion solution and a dispersant into an impinging stream reactor filled with deionized water; Adding a precipitant dropwise to the impinging stream reactor, and combining stirring operation and ultrasonic operation of the impinging stream reactor to obtain a reaction solution; Wherein, the precipitant is used to adjust the pH value of the solution.

3. The preparation method according to claim 2, characterized in that: The precipitant is one or more of ammonium bicarbonate, ammonium hydroxide and urea; Wherein, the pH of the reaction solution is adjusted to 8 to 11.

4. The preparation method according to claim 2, characterized in that: The stirring speed of the impinging stream reactor is 400 r / min to 2000 r / min, and the ultrasonic power is 10 KHz to 100 KHz.

5. The preparation method according to any one of claims 1 to 4, characterized in that: The zirconium salt is zirconium nitrate or zirconium oxychloride, the yttrium salt is yttrium nitrate or yttrium chloride, the rare earth salt includes a gadolinium salt and / or an ytterbium salt, the gadolinium salt is gadolinium nitrate or gadolinium chloride, and the ytterbium salt is ytterbium nitrate or ytterbium chloride; The dispersant is a mixture of one or more of polyvinyl pyrrolidone, hexadecyl trimethyl ammonium bromide, polyethylene glycol ethoxylates, and polyethylene glycol.

6. The preparation method according to claim 1, characterized in that: The reaction solution is subjected to aging treatment, ultrasonic treatment and drying treatment to obtain rare earth-doped YSZ precursor powder, comprising: Performing an aging treatment on the reaction solution to obtain a first solution; Using an ultrasonic cell pulverizer to ultrasonically disperse the first solution to obtain a second solution; the frequency of the ultrasonic cell pulverizer is 10KHz to 100KHz, and the ultrasonic time is 10min to 200min; The second solution is dried using a vacuum freeze dryer to obtain a rare earth-doped YSZ precursor powder; the drying time of the vacuum freeze dryer is 10 hours to 24 hours.

7. The preparation method according to claim 1, characterized in that: The calcination temperature of each calcination treatment in the at least two calcination treatments is 400° C. to 800° C., and the calcination time of each calcination treatment is 1 hour to 10 hours.

8. The preparation method according to claim 1, characterized in that: The sintering temperature of each sintering treatment in the at least two sintering treatments is 900° C. to 1300° C., and the sintering time of each sintering treatment is 2 hours to 10 hours.

9. The preparation method according to claim 1, characterized in that: Screening the intermediate powder comprises: The intermediate powder is sieved based on a sieving operation with a sieving mesh number of 200 mesh to 1000 mesh.

10. A nano-agglomerated rare earth doped YSZ powder, characterized in that: The nano-agglomerated rare earth-doped YSZ powder is prepared by the method for preparing the nano-agglomerated rare earth-doped YSZ powder according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Preparation method for titanium-carbide-strengthened fine-grain tungsten material

    CN106011511A

  • Multi-component rare earth oxide-doped modified YSZ thermal spraying powder and preparation method thereof

    CN106380210A

  • Novel method for preparing nano-agglomerated ZrO powder through thermal spraying

    CN106518064A

  • Method for controlling sintering densification and grain sizes of metal materials

    CN109676124A

  • Ytterbium / gadolinium / yttrium ternary co-doped zirconium oxide nanostructure agglomerated sphere and production method thereof

    CN112851370A

Cited By

  • Preparation method of Sc-doped YSZ thermal spraying powder and Sc-doped YSZ thermal spraying powder

    CN119191839A

  • YSZ thermal barrier coating powder, preparation method thereof and thermal barrier coating