Large molecular weight polymer material, preparation method thereof and solar cell
By introducing a chain extender to the synthesis of polymer hole transport materials for secondary reactions, the problem of difficult molecular weight is solved, and the efficient synthesis of large molecular weight polymers is achieved, which simplifies the process and reduces costs.
Patent Information
- Application Number
- CN202411088925.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-08
- Publication Date
- 2024-11-22
AI Technical Summary
In the synthesis of polymer hole transport materials, it is difficult to control the molecular weight, especially the synthesis of large molecular weight products, resulting in large differences in polymerization degrees.
A two-stage polymerization reaction method is adopted, first the traditional one-pot polymerization reaction is carried out, and then a chain extender is added to the system to perform a secondary reaction to increase the molecular weight of the polymer.
Through this method, the polymerization degree of polymer material is significantly improved, making it easier to synthesize large molecular weights, simplifying the process, reducing production costs, and improving the error tolerance of the polymerization reaction.
Smart Images

Figure CN118994569A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of solar cell preparation, and in particular to a high molecular weight polymer and a preparation method thereof, and a solar cell. Background Art
[0002] Polymer hole transport materials have excellent conductive properties and can achieve higher electron transport than traditional conductive materials, which makes them have broad application prospects in electronic devices and solar cells.
[0003] However, in the actual synthesis process, the synthesis of polymer hole transport materials has problems such as difficulty in controlling molecular weight and difficulty in synthesizing large molecular weight products. Taking poly[bis(4-phenyl)(4-butylphenyl)amine] (Poly-TPD) and poly[bis(4-phenyl)(2,4,6-trimethylphenyl)amine] (PTAA) as examples, it can be found from the published technology and actual synthesis operations that the degree of polymerization between the synthesis batches varies greatly, and the molecular weight is mostly in the range of tens of thousands, making it difficult to synthesize products with larger molecular weights.
[0004] In view of this, the present invention is proposed. Summary of the invention
[0005] The object of the present invention is to provide a high molecular weight polymer material and a preparation method thereof and a solar cell to improve the above technical problems.
[0006] The present invention is achieved in that:
[0007] In a first aspect, the present invention provides a method for preparing a high molecular weight polymer material, comprising: according to a target polymer material, polymerizing corresponding reaction monomers according to a reaction molar ratio in the presence of a base and a catalyst;
[0008] After the polymerization reaction is completed, a chain extender is added to the product to continue the reaction, wherein the chain extender is a monomer that can undergo a chain extension reaction with at least one reactive monomer.
[0009] Optionally, the target polymer material is selected from any one of poly[bis(4-phenyl)(4-butylphenyl)amine](Poly-TPD) and poly[bis(4-phenyl)(2,4,6-trimethylphenyl)amine](PTAA).
[0010] Optionally, the target polymer material is poly[bis(4-phenyl)(4-butylphenyl)amine](Poly-TPD), and the corresponding reaction monomers include 4,4'-dibromobiphenyl or 4,4'-diiodobiphenyl and 4-n-butylaniline.
[0011] Optionally, the catalyst is a palladium catalyst, preferably tris(dibenzylideneacetone)dipalladium. Optionally, an organic phosphorus ligand is further added to the polymerization reaction system, and the organic phosphorus ligand is preferably tri-tert-butyl phosphine.
[0012] Alternatively, 4,4'-dibromobiphenyl, 4-n-butylaniline, a base and a catalyst are dissolved in an organic solvent, and then an organic phosphorus ligand is added to the system for dissolution, and then the reaction is carried out.
[0013] Optionally, the polymerization reaction temperature is 80° C. to 160° C., more preferably 150° C., the polymerization reaction is carried out under stirring, and the reaction time is 2-48 hours, more preferably 24 hours.
[0014] Optionally, the target polymer material is poly[bis(4-phenyl)(4-butylphenyl)amine], and the chain extender is selected from at least one of the following monomers:
[0015] (1) Substituted or unsubstituted aniline monomers, or other primary amine monomers;
[0016] (2) dihaloaromatic hydrocarbons;
[0017] (3) Halogenated olefins;
[0018] (4) Diisocyanate monomers.
[0019] Optionally, the target polymer material is poly[bis(4-phenyl)(4-butylphenyl)amine], and the chain extender is selected from at least one of the following monomers:
[0020] (a) alkylanilines;
[0021] (b) dihalogenated biphenyls;
[0022] (c) Bromostyrene;
[0023] (d) Hexamethylene diisocyanate (HMDC).
[0024] Optionally, the chain extender is a combination of 4-n-butylaniline and p-bromostyrene or a combination of 4-n-butylaniline and hexamethylene diisocyanate (HMDC), or any one of 4-n-butylaniline and 4,4'-diiodobiphenyl.
[0025] Optionally, the chain extender is an aniline monomer or a primary amine monomer formed by a single substitution of the amino group of the aniline monomer or a dihalogenated aromatic hydrocarbon, and the temperature for continuing the reaction by adding the chain extender is 80° C. to 160° C., more preferably 150° C., and the reaction time is 5 hours.
[0026] The chain extender is a combination of aniline monomer and halogenated olefin. The aniline monomer is first added to react at 80°C to 160°C for 2-24 hours, and then the halogenated olefin is added to react at 80°C to 160°C for 2-24 hours. The product is then post-treated and dissolved, and azobisisobutyronitrile is added to react at 60°C to 100°C for 2-24 hours.
[0027] When the chain extender is a combination of aniline monomer and diisocyanate monomer, the aniline monomer is first added to react at 80°C to 160°C for 2-24 hours, and a polymer is obtained after post-treatment. The polymer is then dissolved and the diisocyanate monomer is added to react at 50°C to 70°C for 2-24 hours.
[0028] Optionally, the amount of the chain extender is 0.15% to 15% of the molar amount of one of the reactive monomers undergoing the polymerization reaction.
[0029] In a second aspect, the present invention further provides a high molecular weight polymer material, which is prepared by the above-mentioned method for preparing a high molecular weight polymer material.
[0030] In a third aspect, the present invention further provides a solar cell comprising a hole transport layer, wherein the hole transport layer is prepared from the above-mentioned high molecular weight polymer material.
[0031] The invention has the following beneficial effects: by changing the traditional one-pot method for preparing polymer materials, on the basis of generating polymer materials by one-step polymerization reaction, a chain extender is further added to the system for a secondary reaction, thereby increasing the degree of polymerization of the synthesized polymer materials, making it easier to synthesize polymer materials with large molecular weights. The preparation method is simple and effective, increases the error tolerance of the polymerization reaction, and reduces the production cost. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.
[0033] Figure 1 It is a molecular weight comparison chart of the GPC results of Example 4 of the present invention and Comparative Example 5;
[0034] Figure 2 This is a schematic structural diagram of a perovskite solar cell according to Example 5 of the present invention;
[0035] Figure 3 : is a PCE distribution diagram of two perovskite solar cells in Example 5 of the present invention;
[0036] Figure 4 1 is a Voc distribution diagram of two perovskite solar cells in Example 5 of the present invention;
[0037] Figure 5 FF distribution diagram of two perovskite solar cells in Example 5 of the present invention;
[0038] Figure 6 This is the Jsc distribution diagram of the two perovskite solar cells in Example 5 of the present invention. DETAILED DESCRIPTION
[0039] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.
[0040] The following is a detailed description of a high molecular weight polymer material, a preparation method thereof, and a solar cell provided by the present invention.
[0041] Some embodiments of the present invention provide a method for preparing a high molecular weight polymer material, which comprises: according to the target polymer material, polymerizing the corresponding reaction monomers according to the reaction molar ratio in the presence of a base and a catalyst; and adding a chain extender to the product obtained after the polymerization reaction is completed to continue the reaction.
[0042] Chain extenders, also known as chain growth agents, are substances that can react with functional groups on linear polymer chains to extend molecular chains and increase molecular weight. They are commonly used in polymer processes such as polyurethane and polyester, but there is no relevant application in the synthesis of specific polymer materials (such as polymer hole transport layer materials). The inventor creatively proposed to introduce chain extenders in the synthesis process of specific polymer materials (such as polymer hole transport materials). However, through the practice and research of the inventor, it was found that the chain extenders used in the traditional polyurethane field and other processes are generally added to the polymerization reaction system of the reaction raw materials to promote the synthesis of products with larger molecular weights. However, in the synthesis process of specific polymer materials (such as polymer hole transport materials), the reaction monomers react with the molar ratio corresponding to the target product, and the effect is the best. Introducing chain extenders that can react with monomers or products, on the contrary, can not achieve better polymerization effects. Therefore, after further research and practice, it is creatively found that on the basis of the existing one-pot method for generating polymer materials, adding chain extenders again to the product, that is, changing a single reaction into a two-stage reaction, greatly improves the degree of polymerization of the polymer material, and is simple to operate.
[0043] It should be noted that, in some embodiments, the chain extender is a monomer that can undergo a chain extension reaction with at least one reactive monomer. That is, the chain extender has a group that reacts with the active group of the reactive monomer, for example, if the reactive monomer has an amino group, the chain extender has a halogen substituent; or if the reactive monomer has a halogen substituent, the chain extender has an amino group, etc.
[0044] For reference, the target polymer material is selected from any one of Poly-TPD and PTAA, or other polytriarylamine polymers, that is, the target polymer material is a commonly used polymer hole transport material.
[0045] Exemplarily, the target polymer material is Poly-TPD, and the corresponding reactive monomers include any one or two of 4,4'-dibromobiphenyl and 4,4'-diiodobiphenyl and 4-n-butylaniline.
[0046] Specifically, the chemical structure of Poly-TPD is:
[0047] Further, taking the synthesis of Poly-TPD as an example, its preparation method specifically includes the following steps:
[0048] S1. Poly-TPD is synthesized by a single polymerization reaction.
[0049] Specifically, in some embodiments, 4,4'-dibromobiphenyl, 4-n-butylaniline, a base and a catalyst are dissolved in an organic solvent, and then an organic phosphorus ligand is added to the system for dissolution, and then the reaction is carried out.
[0050] For reference, the catalyst is a palladium-based catalyst, and for example, tris(dibenzylideneacetone)dipalladium may be selected.
[0051] In some embodiments, the organophosphorus ligand is preferably tri-tert-butylphosphine.
[0052] In some embodiments, the polymerization temperature is 80° C. to 160° C., for example, 150° C. In order to allow the polymerization to proceed better, the polymerization is carried out under stirring conditions, and the reaction time is 2-48 hours, more preferably 24 hours.
[0053] It should be noted that after the raw materials are uniformly mixed, they can be treated multiple times by a freezing vacuum degassing method, and then reacted after being protected by nitrogen; or the raw materials can be mixed in a nitrogen environment.
[0054] Exemplarily, the synthesis route of Poly-TPD by a single polymerization reaction is as follows:
[0055]
[0056] S2. After the polymerization reaction is completed, a chain extender is added to the product to continue the reaction.
[0057] Specifically, in some embodiments, the chain extender is selected from at least one of the following monomers:
[0058] (1) Substituted or unsubstituted aniline monomers, or other primary amine monomers;
[0059] (2) dihaloaromatic hydrocarbons;
[0060] (3) Halogenated olefins;
[0061] (4) Diisocyanate monomers.
[0062] Further, in some embodiments, the chain extender is selected from at least one of the following monomers:
[0063] (a) alkylanilines;
[0064] (b) dihalogenated biphenyls;
[0065] (c) Bromostyrene;
[0066] (d) Hexamethylene diisocyanate.
[0067] For reference, the chain extender may be a combination of 4-n-butylaniline and p-bromostyrene or a combination of 4-n-butylaniline and hexamethylene diisocyanate, or any one of 4-n-butylaniline and 4,4'-diiodobiphenyl.
[0068] Depending on the selection of the chain extender, the operation process and conditions of adding the chain extender for the continued reaction will also be different. In some specific embodiments, the chain extender is selected from aniline monomers or primary amine monomers formed by the mono-substitution of the amino group of aniline monomers or dihaloaromatic hydrocarbons, and the chain extender is directly added to the reaction system after the polymerization reaction is completed to continue the reaction, and the temperature of the continued reaction is 80°C to 160°C, for example, 150°C, and the time of the continued reaction is 2-24 hours.
[0069] When the chain extender is a combination of aniline monomer and halogenated olefin, the aniline monomer is first directly added to the reaction system after the polymerization reaction is completed, and the reaction is carried out at 80°C to 160°C for 2-24 hours to achieve the synthesis of amino terminal groups. Thereafter, the halogenated olefin is added and the reaction is carried out at 80°C to 160°C for 2-24 hours to achieve the synthesis of vinyl terminal groups. After the reaction product is post-treated, the obtained polymer is dissolved and then azobisisobutyronitrile is added and the reaction is carried out at 60°C to 100°C for 2-24 hours.
[0070] After the chain extender is selected and the chain extender reaction is completed, the reaction system is cooled to room temperature, cooled to room temperature, the solvent is removed by rotary evaporation under reduced pressure, chloroform is added to dissolve, methanol is used to slurry and precipitate, filtered, and the solid is washed with methanol, water, and acetone. The obtained solid and palladium-removing silica gel are mixed, chloroform is added, stirred overnight, and the palladium-removing silica gel is removed by filtration. The filtrate is spin-dried and dried in an oven.
[0071] Furthermore, the chain extender is a combination of aniline monomer and diisocyanate monomer. The aniline monomer is first added to react at 80°C to 160°C for 2-24 hours, and the polymer is obtained by post-treatment, that is, the reaction system is cooled to room temperature, cooled to room temperature, the solvent is removed by rotary evaporation under reduced pressure, chloroform is added to dissolve, methanol is used for pulping and precipitation, and the solid is washed with methanol, water, and acetone. The obtained solid is mixed with palladium-removing silica gel, chloroform is added, stirred overnight, the palladium-removing silica gel is filtered to remove the palladium-removing silica gel, the filtrate is spin-dried, and dried in an oven. Then the obtained polymer is dissolved and the diisocyanate monomer is added to react at 50°C to 70°C for 2-24 hours.
[0072] It should be noted that when the chain extender is selected, for example, a combination of 4-n-butylaniline and p-bromostyrene or a combination of 4-n-butylaniline and hexamethylene diisocyanate, that is, other functional groups are introduced while expanding the molecular weight, which can effectively passivate HTL / perovskite interface defects, improve perovskite crystallization, and regulate energy level matching, thereby effectively improving the photoelectric performance parameters of the battery.
[0073] Furthermore, in the above embodiment, the amount of the chain extender is 0.15% to 15% of the molar amount of one of the reactive monomers undergoing the polymerization reaction.
[0074] Some embodiments of the present invention further provide a high molecular weight polymer material, which is prepared by the above-mentioned method for preparing a high molecular weight polymer material.
[0075] Furthermore, some embodiments of the present invention also provide a solar cell, which includes a hole transport layer, wherein the hole transport layer is made of the above-mentioned high molecular weight polymer material. The solar cell may be a perovskite solar cell.
[0076] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.
[0077] Example 1
[0078] This embodiment provides a method for preparing a high molecular weight polymer material, which comprises the following steps:
[0079] In a nitrogen glove box, add 4,4'-diiodobiphenyl (1221.2 mg, 3.01 mmol), 4-n-butylaniline (448.9 mg, 3.01 mmol), sodium tert-butoxide (870.0 mg, 9.05 mmol), tris(dibenzylideneacetone)dipalladium (14.0 mg, 0.015 mmol) to the reaction bottle, add 40 mL of xylene to dissolve, then add tri-tert-butylphosphine (1M toluene solution, 60 μL, 0.06 mmol) to the system, seal it well, take out the glove box, heat to 150°C and stir for 24 hours.
[0080] 0.015 eq of 4-n-butylaniline (6.7 mg, 0.045 mmol) was added, and the reaction was continued to be heated at 150° C. for 5 h.
[0081] Cool to room temperature, remove the solvent by rotary evaporation under reduced pressure, add chloroform to dissolve, use methanol to slurry and precipitate, filter, and rinse the solid with methanol, water, and acetone. Mix the obtained solid with palladium-removing silica gel, add chloroform and stir overnight, filter to remove palladium-removing silica gel, spin dry the filtrate, and dry in an oven to obtain 740 mg (yield 82.2%). GPC (chloroform): Mw = 136.9k, PDI = 9.73.
[0082] Example 2
[0083] This embodiment provides a method for preparing a high molecular weight polymer material, which comprises the following steps:
[0084] In a nitrogen glove box, add 4,4'-diiodobiphenyl (1221.2 mg, 3.01 mmol), 4-n-butylaniline (448.9 mg, 3.01 mmol), sodium tert-butoxide (870.0 mg, 9.05 mmol), tris(dibenzylideneacetone)dipalladium (14.0 mg, 0.015 mmol) to the reaction bottle, add 40 mL of xylene to dissolve, then add tri-tert-butylphosphine (1M toluene solution, 60 μL, 0.06 mmol) to the system, seal it well, take out the glove box, heat to 150°C and stir for 24 hours.
[0085] Then, 122 mg of diiodobiphenyl (0.3 mmol, 0.1 eq) was added and the reaction was continued by heating at 150° C. for 5 h.
[0086] Cool to room temperature, remove the solvent by rotary evaporation under reduced pressure, add chloroform to dissolve, use methanol to slurry and precipitate, filter, and rinse the solid with methanol, water, and acetone. Mix the obtained solid with palladium-removing silica gel, add chloroform and stir overnight, filter to remove palladium-removing silica gel, spin dry the filtrate, and dry in an oven to obtain 762 mg (yield 85%). GPC (chloroform): Mw = 115.2k, PDI = 4.58.
[0087] Example 3
[0088] This embodiment provides a method for preparing a high molecular weight polymer material, which comprises the following steps:
[0089] In a nitrogen glove box, add 4,4'-diiodobiphenyl (1221.2 mg, 3.01 mmol), 4-n-butylaniline (448.9 mg, 3.01 mmol), sodium tert-butoxide (870.0 mg, 9.05 mmol), tris(dibenzylideneacetone)dipalladium (14.0 mg, 0.015 mmol) to the reaction bottle, add 40 mL of xylene to dissolve, then add tri-tert-butylphosphine (1M toluene solution, 60 μL, 0.06 mmol) to the system, seal it well, take out the glove box, heat to 150°C and stir for 24 hours.
[0090] Synthesis of amino terminal group: 22.4 mg (0.15 mmol, 0.05 eq) of 4-n-butylaniline was added, and the reaction was continued to heat at 150° C. for 5 h.
[0091] Synthesis of vinyl end group: Add 54.9 mg (0.3 mmol, 0.1 eq) of p-bromostyrene and continue heating the reaction at 150°C for 5 h.
[0092] Cool to room temperature, remove the solvent by rotary evaporation under reduced pressure, add chloroform to dissolve, use methanol to slurry and precipitate, filter, and rinse the solid with methanol, water, and acetone. Mix the obtained solid with palladium-removing silica gel, add chloroform and stir overnight, filter to remove palladium-removing silica gel, spin dry the filtrate, and dry in an oven to obtain 760 mg (yield 85%). GPC (chloroform): Mw = 38.9k, PDI = 2.07.
[0093] Take 0.3148g of the above compound, add 3.1mg of AIBN, add 10mL of toluene, heat at 65℃ for 1h, the reaction solution is clear, heat to 95℃, and react overnight. Cool to room temperature, remove the solvent by rotary evaporation under reduced pressure, add chloroform to dissolve, use methanol to slurry and precipitate, filter, and rinse the solid with methanol, water, and acetone. GPC (chloroform): Mw = 86.4k, PDI = 3.37.
[0094] Example 4
[0095] This embodiment provides a method for preparing a high molecular weight polymer material, which comprises the following steps:
[0096] Take 104.0 mg of the target polymer in Example 1 and add it to 4 mL of chloroform to dissolve. Take 6.2 mg of HMDC and add it to 2 mL of chloroform to obtain a 3.1 mg / mL solution. Take 0.1 mL and add it to a reaction tube. React at 60°C overnight. Cool to room temperature, remove the solvent by rotary evaporation under reduced pressure, add chloroform to dissolve, use methanol to slurry and precipitate, filter, and rinse the solid with methanol, water, and acetone. GPC (chloroform): Mw = 171.2k, PDI = 4.55.
[0097] Comparative Example 1
[0098] This comparative example provides a method for preparing a high molecular weight polymer material, which comprises the following steps:
[0099] Add 4,4'-dibromobiphenyl (938.2mg, 3.01mmol), 4-n-butylaniline (938.2mg, 3.01mmol), sodium tert-butoxide (870.0mg, 9.05mmol), tri(dibenzylideneacetone)dipalladium (14.0mg, 0.015mmol) to the reaction bottle, add 40mL of xylene to dissolve, then add tri-tert-butylphosphine (1M toluene solution, 60μL, 0.06mmol) to the system, and repeat the freezing vacuum degassing method three times, nitrogen protection, and heat to 150℃ and stir for 24h. Cool to room temperature, remove the solvent by rotary evaporation under reduced pressure, add chloroform to dissolve, use methanol to beat the precipitation, filter, and rinse the solid with methanol, water, and acetone. The obtained solid and palladium-removing silica gel are mixed and stirred overnight with chloroform, and the palladium-removing silica gel is removed by filtration. The filtrate is spin-dried and dried in an oven to obtain a yellow-green solid with a yield of 731.8mg (81.3%). GPC (chloroform): Mw=14k, PDI=1.99.
[0100] Comparative Example 2 to Comparative Example 5
[0101] Comparative Example 2 is a direct repetition of the operation of Comparative Example 1; the only difference between Comparative Example 3 and Comparative Example 1 is that the raw materials are directly weighed and mixed in a nitrogen glove box; Comparative Examples 4 and Comparative Examples 5 are compared with Comparative Example 1, and the only difference is that the raw materials are directly weighed and mixed in a nitrogen glove box, and 4,4'-diiodobiphenyl is used instead of 4,4'-dibromobiphenyl in the same molar ratio.
[0102] Table 1 shows the comparison of GPC results of the target polymers of Comparative Examples 1 to 5 and Examples 1 to 4.
[0103] Table 1
[0104] serial number M PDI Comparative Example 1 14.1k 1.99 Comparative Example 2 14.4k 2.30 Comparative Example 3 17.2k 2.88 Comparative Example 4 21.7k 2.32 Comparative Example 5 36.0k 3.96 Example 1 136.9k 9.37 Example 2 115.2k 4.58 Example 3 86.3k 3.37 Example 4 171.2k 4.55
[0105] From the comparison of the results of Comparative Examples 1 to 5 in Table 1, it can be seen that the molecular weight distribution of Poly-TPD synthesized each time is different, and the best Mw can reach 36,000, but most of them are concentrated in 10,000 to 20,000. From the results of Examples 1 to 4, it can be seen that by further introducing a chain extender to continue the reaction, the molecular weight of the polymer material is greatly increased. The GPC molecular weight comparison of Comparative Example 5 and Example 4 is as follows: Figure 1 As shown (the red line is the spectrum of Example 4).
[0106] Example 5
[0107] This embodiment provides a perovskite solar cell, and the specific preparation method thereof is as follows:
[0108] ① Substrate preparation: The etched ITO substrate was ultrasonically cleaned with detergent, deionized water, acetone and isopropanol for 15 minutes in sequence, dried in a nitrogen atmosphere, and then treated with ultraviolet ozone for 30 minutes to remove organic impurities on the surface of the ITO substrate.
[0109] ② Preparation of hole transport layer: The polymer material prepared in Example 4 and commercially available Poly-TPD (Mw = 200,000) were dissolved in a mixed solvent of chlorobenzene to prepare a 2 mg / ml solution, and each solution was coated on the surface of the ITO substrate and annealed and dried.
[0110] ③ Preparation of perovskite layer: 1.4M Cs 0.22 FA 0.78 Pb(I 0.865 Br 0.135 )3's DMF:DMSO (4:1) precursor solution was deposited on the hole transport layer by spin coating at 3000 rpm for 25 s to prepare a perovskite layer, and the perovskite film was treated by a vacuum method and annealed at 100°C for 10 min to obtain the perovskite layer.
[0111] ④ Preparation of electron transport layer: A 20 nm thick C60 layer was deposited as the electron transport layer by thermal evaporation at a rate of 0.1 A° / s, followed by a 5 nm thick BCP deposition at a rate of 0.1 A° / s.
[0112] ⑤ Preparation of electrodes: In a vacuum chamber with 5×10 4 Pa high vacuum conditions to deposit a 100nm thick copper electrode to obtain a structure such as Figure 2 The battery shown.
[0113] The intensity calibrated on a standard silicon cell is 100 mW cm -2 The current-voltage (JV) characteristics of the battery measured under AM 1.5G simulated sunlight are as follows Figures 3 to 6As shown, it can be seen that compared with commercial Poly-TPD, using Example 4 as the hole material can significantly improve the VOC (median Voc: 1.24→1.26V), FF (median: 84.18→84.70), and Jsc (median: 19.97→20.16) of the perovskite battery, thereby effectively improving the PCE of the battery (median PCE: 21.03→21.36%).
[0114] In summary, the embodiments of the present invention solve the problem of difficulty in synthesizing high molecular weight polymer materials, and effectively and simply achieve the synthesis of high molecular weight polymer triarylamine hole transport materials by using a chain extender. While the chain extender increases the molecular weight, it can also introduce other functional groups, which can effectively passivate HTL / perovskite interface defects, improve perovskite crystallization, and regulate energy level matching, thereby effectively improving the photoelectric performance parameters of the battery.
[0115] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a high molecular weight polymer material, characterized in that: It includes: According to the target polymer material, the corresponding reaction monomers are subjected to polymerization reaction in the presence of a base and a catalyst according to a reaction molar ratio; After the polymerization reaction is completed, a chain extender is added to the product to continue the reaction, wherein the chain extender is a monomer that can undergo a chain extension reaction with at least one reactive monomer.
2. The preparation method according to claim 1, characterized in that: The target polymer material is selected from any one of poly[bis(4-phenyl)(4-butylphenyl)amine] and poly[bis(4-phenyl)(2,4,6-trimethylphenyl)amine].
3. The preparation method according to claim 1, characterized in that: The target polymer material is poly[bis(4-phenyl)(4-butylphenyl)amine], and the corresponding reaction monomers include any one of 4,4'-dibromobiphenyl and 4,4'-diiodobiphenyl, and 4-n-butylaniline.
4. The preparation method according to claim 3, characterized in that: The catalyst is a palladium catalyst. 4,4'-dibromobiphenyl, 4-n-butylaniline, a base and a catalyst are dissolved in an organic solvent, and then an organic phosphorus ligand is added to the system for dissolution, and then a reaction is carried out. The polymerization reaction temperature is 80 to 160 degrees Celsius, and the polymerization reaction is carried out under stirring conditions, and the reaction time is 2 to 48 hours.
5. The preparation method according to claim 4, characterized in that: The organic phosphorus ligand is tri-tert-butyl phosphine.
6. The preparation method according to any one of claims 1 to 5, characterized in that: The target polymer material is poly[bis(4-phenyl)(4-butylphenyl)amine], and the chain extender is selected from at least one of the following monomers: (1) Substituted or unsubstituted aniline monomers, or other primary amine monomers; (2) dihaloaromatic hydrocarbons; (3) Halogenated olefins; (4) Diisocyanate monomers.
7. The preparation method according to claim 6, characterized in that: The target polymer material is poly[bis(4-phenyl)(4-butylphenyl)amine], and the chain extender is selected from at least one of the following monomers: (a) alkylanilines; (b) dihalogenated biphenyls; (c) Bromostyrene; (d) Hexamethylene diisocyanate.
8. The preparation method according to claim 5, characterized in that: The chain extender is a combination of 4-n-butylaniline and p-bromostyrene or a combination of 4-n-butylaniline and hexamethylene diisocyanate, or any one of 4-n-butylaniline and 4,4'-diiodobiphenyl; The chain extender is selected from aniline monomers / other primary amine monomers or dihalogenated aromatic hydrocarbons, and the temperature for continuing the reaction after adding the chain extender is 80°C to 160°C, more preferably 150°C, and the reaction time is preferably 5 hours; The chain extender is a combination of aniline monomer and halogenated olefin. The aniline monomer is first added to react at 80°C to 160°C for 2-24 hours, and then the halogenated olefin is added to react at 80°C to 160°C for 2-24 hours. The product is then post-treated and dissolved, and azobisisobutyronitrile is added to react at 60°C to 100°C for 2-24 hours. The chain extender is a combination of aniline monomer and diisocyanate monomer. The aniline monomer is first added to react at 80°C to 160°C for 2-24 hours, and then the polymer is post-treated to obtain a polymer. The polymer is then dissolved and the diisocyanate monomer is added to react at 50°C to 70°C for 2-24 hours. The amount of the chain extender used is 0.15% to 15% of the molar amount of one of the reactive monomers in the polymerization reaction.
9. A high molecular weight polymer material, characterized in that: The compound is prepared by the preparation method according to any one of claims 1 to 8.
10. A solar cell, characterized in that: The hole transport layer comprises a hole transport layer, wherein the hole transport layer is prepared from the high molecular weight polymer material according to claim 9.
Citation Information
Cited By
Polytriarylamine hole transport material, preparation method thereof and perovskite battery
CN121609910A