Crosslinking type block silicone oil for regenerated cellulose fibers and preparation method of crosslinking type block silicone oil
By introducing double-ended epoxy silicone oil and polyetheramine into the block silicone oil of regenerated cellulose fibers, the silicon methoxy groups on the branched chain are added, and the cross-linking of fibers is achieved, solving the problem of existing block silicone oil. The washing resistance and bleaching problems caused by crosslinking with fibers improve finishing performance and market prospects.
Patent Information
- Application Number
- CN202411298319.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-18
- Publication Date
- 2024-11-22
AI Technical Summary
The existing block silicone oil used for regenerating cellulose fibers is linear in structure and lacks reactive groups, which makes it impossible to cross-link with the fiber, resulting in the problem that the fiber is not resistant to water washing, is not elastic enough, and is prone to bleaching and pilling.
采用双端环氧硅油、聚醚胺、环氧基硅氧烷和溶剂等原料,通过特定的反应工艺制得交联型嵌段硅油,增加支链上的硅甲氧基团,能够与纤维上的活性基团发生交联,增强织物的整理性能。
It improves the water-washing resistance, finishing performance and anti-pilling performance of the fiber, while ensuring the excellent softness, elasticity and color change performance, and the synthesis method is simple, safe and environmentally friendly.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention relates to the field of textile auxiliaries, in particular to a cross-linked segmented silicone oil for regenerated cellulose fiber and a preparation method thereof. Background Art
[0002] Regenerated cellulose fiber is made from natural cellulose. This fiber not only has the excellent properties of natural plant fiber such as breathability and skin-friendly, but also has the characteristics of light weight and high flexibility, and is widely used in textiles, clothing, home furnishings and other fields. However, due to the looseness of its surface fibers and the particularity of its capillary structure, it is easy to cause pilling when the fibers rub against other clothes and fabrics during wearing and washing, thus affecting the appearance and comfort.
[0003] As we all know, the block silicone oil commonly used for regenerated cellulose fibers on the market is basically prepared by three process routes: 1. It is prepared by the reaction of epoxy silicone oil and alkyl tertiary amine (such as tetramethylethylenediamine, tetramethylpropylenediamine, tetramethylhexanediamine, bis(dimethylaminoethyl)ether, etc.) under the catalysis of organic acid; 2. It is prepared by the reaction of epoxy silicone oil and tertiary amine polyetheramine under the catalysis of organic acid; 3. First, epoxy silicone oil and ED series polyetheramine or D series polyetheramine are used to synthesize block polyether amino silicone oil, and then quaternary ammonium reagent (such as trimethylammonium chloride glycidyl) is added for modification, and it has a good feel style when used to finish regenerated cellulose fibers. However, from the three synthesis processes, it can be seen that the structure of the product is a linear structure and lacks effective active groups in the structure. It is mainly combined with the fabric through ionic bonds, which leads to the inability to cross-link with the active groups such as hydroxyl groups on the fiber, and it cannot cross-link itself. Therefore, when this type of structural softener is used to finish regenerated cellulose fibers, it often has problems such as poor water resistance, insufficient elasticity, and easy pilling during use. Therefore, the present invention adopts double-ended epoxy silicone oil, polyether amine, epoxy siloxane, solvent and other raw materials to prepare a cross-linked block silicone oil for regenerated cellulose fiber. This structural product not only has excellent softness, elasticity, low yellowing, low color change and water washability, but also can effectively prevent the pilling problem of the fiber. The synthesis method is simple, safe and environmentally friendly, and has good innovation. Summary of the invention
[0004] The technical problem to be solved by the present invention is to overcome the defects of the above-mentioned prior art and provide a cross-linked block silicone oil for regenerated cellulose fiber and a preparation method thereof.
[0005] In order to achieve the above object, the present invention adopts the following technical solutions: A cross-linked block silicone oil for regenerated cellulose fiber and a preparation method thereof, characterized in that the synthesis is carried out according to the following method, calculated by mass fraction: Step 1) Add 100 parts of polyetheramine D230 and 210-220 parts of 3-glycidyloxypropyltrimethoxysilane into a reaction vessel equipped with a condensation reflux device, and react at 70-90° C. for 4-6 hours to obtain a siloxane-modified polyether secondary amine, the general structural formula of which is as follows:
[0006] In the formula, 2≤n≤3.
[0007] Step 2) 1000 parts of double-terminal epoxy silicone oil with a number average molecular weight of 8000-10000, 75-95 parts of the self-made siloxane-modified polyether secondary amine in step 1), and 400-600 parts of isopropanol are added to a reaction container equipped with a condensation reflux device, and the reaction container is heated to 80-83° C. and kept in this temperature range for 6-10 hours to obtain a cross-linked block silicone oil for regenerated cellulose fiber, the general structural formula of which is as follows:
[0008] In the formula, 104≤m≤131, 2≤n≤3, 2≤a≤6.
[0009] Preferably, the number average molecular weight of the double-ended epoxy silicone oil is within a range of 8000 to 10000.
[0010] Due to the application of the above technical solution, the present invention has the following advantages: The invention prepares a cross-linked block silicone oil for regenerated cellulose fiber by reacting a self-made siloxane-modified polyether secondary amine with a double-ended epoxy silicone oil under the condition of isopropanol as a solvent. Compared with the common block silicone oil for regenerated cellulose fiber on the market, the main feature of the cross-linked block silicone oil for regenerated cellulose fiber is that while ensuring the linear structure of the main body, a branch chain is added to the main chain, and the branch chain contains a large number of silyl methoxy groups. Since the silyl methoxy group is easily hydrolyzed into silanol, under high-temperature baking, the silanol can not only undergo a cross-linking reaction with active groups such as hydroxyl groups on the fiber, but also undergo cross-linking itself, thereby enhancing the washability of the fabric after finishing, improving the adsorption performance of the finishing agent and effectively preventing the pilling problem of the fiber. The structural performance of this product is significantly better than the common block silicone oil for regenerated cellulose fiber on the market. Therefore, the cross-linked block silicone oil for regenerated cellulose fiber of the invention has good innovation and market prospects. DETAILED DESCRIPTION
[0011] The present invention is further described below through specific implementation modes. Example 1
[0012] Step 1) 100 g of polyetheramine D230 and 210 g of 3-glycidyloxypropyltrimethoxysilane were added into a reaction vessel equipped with a condensation reflux device, and reacted at 75° C. for 5 hours to obtain a siloxane-modified polyether secondary amine.
[0013] Step 2) 1000 g of double-ended epoxy silicone oil with a number average molecular weight of 8058, 92 g of the self-made siloxane-modified polyether secondary amine in step 1), and 500 g of isopropanol are added to a reaction container equipped with a condensation reflux device, and the reaction container is heated to 81° C. and kept at this temperature for 8 hours to obtain a cross-linked block silicone oil for regenerated cellulose fiber. Example 2
[0014] Step 1) 100 g of polyetheramine D230 and 212 g of 3-glycidyloxypropyltrimethoxysilane were added into a reaction vessel equipped with a condensation reflux device, and reacted at 80° C. for 5.5 hours to obtain a siloxane-modified polyether secondary amine.
[0015] Step 2) 1000 g of double-ended epoxy silicone oil with a number average molecular weight of 9020, 80 g of the self-made siloxane-modified polyether secondary amine in step 1), and 460 g of isopropanol are added to a reaction container equipped with a condensation reflux device, and the reaction container is heated to 82° C. and kept at this temperature for 9 hours to obtain a cross-linked block silicone oil for regenerated cellulose fiber. Example 3
[0016] Step 1) 100 g of polyetheramine D230 and 215 g of 3-glycidyloxypropyltrimethoxysilane were added into a reaction vessel equipped with a condensation reflux device, and reacted at 85° C. for 6 hours to obtain a siloxane-modified polyether secondary amine.
[0017] Step 2) 1000 g of double-ended epoxy silicone oil with a number average molecular weight of 10056, 78 g of the self-made siloxane-modified polyether secondary amine in step 1), and 450 g of isopropanol are added to a reaction container equipped with a condensation reflux device, and the reaction container is heated to 81° C. and kept at this temperature for 10 hours to obtain a cross-linked block silicone oil for regenerated cellulose fiber.
[0018] A cross-linked block silicone oil application finishing process for regenerated cellulose fibers: 1. Preparation of a cross-linked block silicone oil emulsion for regenerated cellulose fibers The silicone oil samples of the embodiment and the comparative sample were respectively stirred evenly with a small amount of non-ionic emulsifier (compound of XL-40 and AEO-9) and glacial acetic acid, and then water was added while stirring to obtain a silicone oil emulsion with a pH of 3-6 and a solid content of 15%.
[0019] 2. Finishing process Fabrics used: white 50S modal knitted fabric, brown 40S lyocell woven fabric, black 40S lyocell knitted fabric.
[0020] Finishing process: padding working solution (silicone oil emulsion 40g / L, one dip and one padding, padding rate (70%~80%) → baking (white 50S modal knitted fabric 165 o C×40s, brown 40S lyocell woven fabric 165 o C×50s, black 40S lyocell knitted fabric 165 o C×50s) → Cool and rehumidify for 24 hours → Test performance.
[0021] 3. Application performance testing ① Hand feel evaluation Testing the compression linearity of finished fabrics with the KES fabric style meter LC , the larger the value, the softer it is.
[0022] Testing the tensile recovery rate of finished fabrics using KES fabric style meter RT (%), the larger the value, the better the elasticity.
[0023] ②Yellowing evaluation The finished white 50S modal knitted fabric was tested by WSB-2 intelligent whiteness tester, and the average value was taken after three measurements. The blank fabric was used for comparison. The larger the whiteness value, the smaller the yellowing.
[0024] ③Color difference evaluation The finished coffee-colored 40S Lyocell woven fabric and black 40S Lyocell knitted fabric were measured using a Color-Eye7000A colorimeter. The average value was taken after three measurements and compared with a blank fabric. The smaller the △E value, the smaller the color difference.
[0025] ④Washability evaluation Refer to AATCC 135-2018 "Dimensional stability of fabrics after home washing", wash in a designated American standard washing machine according to the prescribed program, and then test the compression linearity LC and tensile work recovery RT (%).
[0026] ⑤Anti-pilling evaluation The test was carried out in accordance with GB / T 4802.1 “Textiles - Fabric Pilling Test Circular Locus Method”.
[0027] The test results of softness and elasticity of the cross-linked block silicone oil for regenerated cellulose fiber of the present invention and the comparative silicone oil are shown in Table 1: Table 1 Comparison of application performance of fabrics after finishing of example samples and comparative samples
[0028] It can be seen from Table 1 that after the fabric is finished with the finishing agent made of the cross-linked block silicone oil for regenerated cellulose fiber of the present invention, the compression linearity and the tensile power recovery rate are better than those of the control sample. After washing, the compression linearity and the tensile power recovery rate both decrease, but the decrease of the control sample is more obvious, indicating that the product of the present invention not only has a good hand feel but also has good water washing resistance.
[0029] The yellowing performance test results of the cross-linked block silicone oil for regenerated cellulose fiber of the present invention and the comparative silicone oil are shown in Table 2: Table 2 Comparison of yellowing effect of fabrics after finishing of example samples and comparative samples
[0030] It can be seen from Table 2 that the cross-linked segmented silicone oil for regenerated cellulose fibers of the present invention has little effect on the whiteness of the finished fabric, which is slightly better than the control sample, indicating that the product of the present invention has good anti-yellowing performance.
[0031] The color change performance test results of the cross-linked block silicone oil for regenerated cellulose fiber of the present invention and the comparative silicone oil are shown in Table 3: Table 3 Comparison of color change effects of fabrics after finishing of example samples and comparative samples
[0032] It can be seen from Table 3 that the cross-linked segmented silicone oil for regenerated cellulose fiber of the present invention has little effect on the color change of the fabric, which is slightly better than the control sample, indicating that the product of the present invention has good low color change performance.
[0033] The anti-pilling performance test results of the cross-linked block silicone oil for regenerated cellulose fiber of the present invention and the comparative silicone oil are shown in Table 4: Table 4 Comparison of anti-pilling effect of fabrics after finishing of example samples and comparative samples
[0034] It can be seen from Table 4 that the anti-pilling performance of the cross-linked segmented silicone oil for regenerated cellulose fiber of the present invention is significantly better than that of the control sample, indicating that the product of the present invention has good anti-pilling performance.
Claims
1. A cross-linked block silicone oil for regenerated cellulose fiber and a preparation method thereof, characterized in that The synthesis method is as follows, calculated by mass fraction: Step 1) 100 parts of polyetheramine D230 and 210-220 parts of 3-glycidyloxypropyltrimethoxysilane are added to a reaction vessel equipped with a condensation reflux device, and reacted at 70-90° C. for 4-6 hours to obtain a siloxane-modified polyether secondary amine, the general structural formula of which is as follows: Wherein 2≤n≤3; Step 2) 1000 parts of double-ended epoxy silicone oil with a number average molecular weight of 8000-10000, 75-95 parts of the self-made siloxane-modified polyether secondary amine in step 1), and 400-600 parts of isopropanol are added to a reaction container equipped with a condensation reflux device, and the reaction container is heated to 80-83° C., and the reaction is kept in this temperature range for 6-10 hours to obtain a cross-linked block silicone oil for regenerated cellulose fiber, and its general structural formula is as follows: In the formula, 104≤m≤131, 2≤n≤3, 2≤a≤6.