Biomass thermochromic porous membrane with adhesive single surface and preparation method of biomass thermochromic porous membrane

By using biomass materials and gradient crosslinking structures in thermochromic dyes, the safety hazards of bisphenol A color developer and the leakage problems caused by solid-liquid phase change characteristics are solved, and a safe and environmentally friendly temperature response discoloration and Thermal energy storage performance broadens the range of color variation and improves stability.

CN118994718AActive Publication Date: 2024-11-22JIANGNAN UNIV

Patent Information

Application Number
CN202411053275.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-02
Publication Date
2024-11-22
Estimated Expiration
2044-08-02

AI Technical Summary

Technical Problem

The bisphenol A color developer used in existing thermochromic dyes has safety risks, and the solid-liquid phase transition characteristics lead to solid-state rigidity and molten state leakage problems, limiting its application.

Method used

Using a single-sided sticky biomass thermochromic porous membrane preparation method, biomass is prepared by heating the solid-liquid phase change solvent, weakly acidic polyhydroxy biomass or biomass derivatives and cryptosomal dyes in a vacuum environment. Thermal discoloration dye is encapsulated using a gradient crosslinking structure and a porous gel film to form a biomass thermochromic porous film with high thermal conductivity and good stability.

Benefits of technology

It achieves safe and environmentally friendly dual properties of temperature-responsive color change performance and thermal energy storage, avoids solvent leakage, broadens the color change range, and has good reversibility and self-support flexibility.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118994718A_ABST
    Figure CN118994718A_ABST
Patent Text Reader

Abstract

The invention discloses a single-sided adhesive biomass thermochromic porous membrane and a preparation method thereof, and belongs to the field of intelligent stimulation response materials. According to the method, weakly acidic polyhydroxy biomass or a biomass derivative is used for replacing a toxic bisphenol A color developing agent and is used for preparing the biomass thermochromic dye; a polydimethylsiloxane gel film with a large number of pore structures is prepared through a salt template method, and meanwhile, a gradient cross-linking strategy is introduced to endow the gel film with single-sided adhesion; the porous structure of the porous gel film is filled with the biomass thermochromic dye through a vacuum pressure impregnation technology, and the single-face-adherable biomass thermochromic porous film with shape stability is obtained. The biomass thermochromic porous membrane prepared by the preparation method disclosed by the invention shows good temperature response discoloration performance and cyclic reversibility, and has single-sided adhesiveness, shape stability, excellent self-supporting flexibility and solid-solid phase change characteristics.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of intelligent stimulus response materials, and in particular to a single-sided adhesive biomass thermochromic porous film and a preparation method thereof. Background Art

[0002] Thermochromic dyes composed of leuco dyes, developers and phase change solvents have excellent temperature-responsive color change and phase change properties, and can provide real-time and intuitive response to temperature through color. They have attracted the attention of many researchers due to their high color saturation, suitable color change temperature and easy availability. However, they also have problems with color uniformity and the safety of developers. Developers, as the key component of three-component thermochromic dyes, are usually weakly acidic compounds with electron-withdrawing ability. Among them, bisphenol A (BPA) is used as the main source of thermochromic dye developers due to its high color formation efficiency and low cost, such as bank printing slips, supermarket shopping receipts and other thermal papers. Although bisphenol A is the most widely used high-efficiency developer in current research and application, it is an organic compound with 96 toxicities, endocrine disruptors and possible carcinogenicity. Long-term exposure to bisphenol A may cause various health hazards to the human body, including breast cancer, heart disease, infertility and neurodevelopmental disorders. Widespread exposure to bisphenol A has become an important public health issue. For this reason, safer analogs such as bisphenol S (BPS), bisphenol F (BPF) and bisphenol AF (BPAF) have been introduced into the market as substitutes. Studies have found that although similar substitutes such as bisphenol S and bisphenol F are less destructive to the electrophysiological balance of the heart and the endocrine system than bisphenol A, they are not completely safe. Given the harm of bisphenol color developers to the human body, the development of green and healthy bisphenol A alternative color developers remains a challenge.

[0003] In addition, thermochromic dyes with phase change properties can show corresponding color changes while absorbing or releasing a large amount of latent heat. They are considered to be ideal carriers for temperature visualization and thermal energy storage composite materials, and have broad application prospects in functional textiles, smart temperature-regulating clothing, wearable temperature control, building energy saving, flexible electronic devices, etc. However, due to their solid-liquid phase change properties, thermochromic dyes mainly exist in the form of low-temperature solid or high-temperature molten state, and have the problems of solid rigidity and molten state leakage, which greatly limits their application.

[0004] Most of the thermochromic materials with temperature indication function that have been widely studied use materials that respond to temperature-responsive solid-liquid phase transitions. The materials change transparency while the phase state changes, and use the temperature-responsive transparency change to indicate the temperature. In patent EP1281946, paraffin is used as a temperature-indicating phase change material to prepare a regular composite material. When the temperature rises above the melting point of paraffin, the crystal state of paraffin changes from a white opaque state to a transparent state, thereby indicating the temperature. Since paraffin changes from white to colorless under the influence of temperature, the composite material using paraffin as a temperature-indicating phase change material can only change from white to colorless, and the color change is relatively single. Patent US4428321 designs a temperature indicating label with a three-layer structure. The top layer is a transparent blended coating containing rubber and a crystallizable material. At a certain temperature, this coating has fluidity. The middle layer is a porous film shielding layer used to shield the color of the bottom layer. The bottom layer is a colored layer. When a certain temperature is reached, the top layer material begins to flow and penetrates into the porous shielding layer, making the shielding layer transparent, thereby revealing the bottom layer color and playing an indicating effect. Since the physical behavior of the top layer material penetrating into the porous shielding layer is not only related to temperature, but also to time. Therefore, even if the color is observed, it is impossible to estimate the temperature indicated by the label. Summary of the invention

[0005] In order to solve the above problems, the present invention provides a method for preparing a single-sided adhesive biomass thermochromic porous membrane. The prepared biomass thermochromic porous membrane has good temperature responsive color change performance and cyclic reversibility, can effectively prevent solvent leakage and is environmentally friendly.

[0006] The present invention provides a method for preparing a single-sided adhesive biomass thermochromic porous film, which specifically comprises the following steps:

[0007] (1) heating a solid-liquid phase change solvent to a molten state, adding weakly acidic polyhydroxy biomass or a biomass derivative, boron nitride nanosheets, and a leuco dye, and heating the reaction in a vacuum environment to prepare a biomass thermochromic dye;

[0008] (2) 3-(2-aminoethyl)-aminopropyltrimethoxysilane (AEAPS) is used to modify the surface of the cleaned glass sheet to obtain AEAPS modified glass; vinyl dimethyl silane, salt template agent, hydrogenated silicone oil and platinum catalyst are uniformly mixed by the salt template method, and the bubbles are removed by vacuum to obtain a film-forming liquid; using a gradient cross-linking strategy, the film-forming liquid is poured on the surface of the AEAPS modified glass, and the platinum catalyst diffuses toward the modified glass and solidifies to form a gradient cross-linking structure, followed by ultrasonic desalination to obtain a porous structure, and after drying, a polydimethylsiloxane porous gel membrane is obtained;

[0009] (3) The biomass thermochromic dye prepared in step (1) is heated and melted, and filled into the pore structure of the polydimethylsiloxane porous gel membrane in step (2) through a vacuum pressure impregnation process to obtain a single-sided adhesive biomass thermochromic porous membrane, which can change color from colored to colorless as the temperature increases.

[0010] In one embodiment of the present invention, in step (1), the weakly acidic polyhydroxy biomass or biomass derivative is an organic weakly acidic biomass or biomass derivative compound with electron accepting property, which is one of L-ascorbic acid, L-ascorbyl palmitate, tea polyphenols, lauryl gallate, and tannic acid.

[0011] In one embodiment of the present invention, in step (1), the leuco dye is an electron-donating organic compound, which is one of crystal violet lactone, methyl red, bromocresol green, bromocresol purple, phenol red, 1′,3′-dimethyl-6′-diethylaminofluoran, 3′,6′-dimethoxyfluoran, 3,3-bis(4-diethylamino-2-ethoxyphenyl)-4-azaphthalide, and 7,7-bis(4-(diethylamino)-2-ethoxyphenyl)furano[3,4-b]pyridine-5(7H)-one.

[0012] In one embodiment of the present invention, in step (1), the solid-liquid phase change solvent refers to a solid-liquid phase change solvent that can change from a solid state to a molten state when heated above the phase change temperature of the phase change solvent, and the solid-liquid phase change solvent is one or more of lauryl alcohol, myristyl alcohol, cetyl alcohol, stearyl alcohol, tetradecanol, hexadecanol, octadecyl alcohol, behenyl alcohol, and oleyl alcohol.

[0013] In one embodiment of the present invention, in step (1), the amount of boron nitride nanosheets added is 0.1% to 15% of the total mass of the solid-liquid phase change solvent, the weakly acidic polyhydroxy biomass or biomass derivative, the boron nitride nanosheets, and the leuco dye.

[0014] In one embodiment of the present invention, in step (1), the biomass thermochromic dye is prepared by heating the reaction in a vacuum environment, wherein the vacuum degree is -0.1 MPa to -0.06 MPa and the heating temperature is 40 to 120°C.

[0015] In one embodiment of the present invention, in step (1), the mass ratio of the leuco dye to the weakly acidic polyhydroxy biomass or biomass derivative is 1:0.2-15; the mass ratio of the leuco dye to the solid-liquid phase change solvent is 1:50-1:300.

[0016] In one embodiment of the present invention, in step (2), the salt template is one or more of sodium nitrate, potassium nitrate, sodium chloride, potassium chloride, and sodium sulfate; and the ultrasonic desalting time is 6 h to 72 h.

[0017] In one embodiment of the present invention, in step (2), the total mass ratio of vinyldimethylsilane to hydrogenated silicone oil and platinum catalyst is 5 to 30:1; the total mass ratio of salt template to vinyldimethylsilane, hydrogenated silicone oil and platinum catalyst is 0.1 to 1.2:1.

[0018] In one embodiment of the present invention, in step (2), the curing temperature is 70°C to 150°C.

[0019] The invention provides a single-sided adhesive biomass thermochromic porous film prepared by the method described above.

[0020] The single-sided adhesive biomass thermochromic porous film of the present invention is used in the fields of wearable sensors, surface temperature indicators of instruments and equipment, and flexible electronic devices.

[0021] [Beneficial Effects]

[0022] (1) The present invention introduces safe and renewable weakly acidic polyhydroxy biomass or biomass derivatives as a color developer for thermochromic dyes, replacing the bisphenol A color developer commonly used in the market, and is used for the preparation of biomass thermochromic dyes, which can effectively avoid the harm of bisphenol A and improve the safety of thermochromic dyes;

[0023] (2) The present invention introduces boron nitride nanosheets in the preparation of thermochromic dyes, which can improve the thermal conductivity of the thermochromic dyes, thereby improving the color change sensitivity of the thermochromic porous membrane; at the same time, the two-dimensional structure of the boron nitride nanosheets in the thermochromic porous membrane is conducive to preventing the leakage of the thermochromic dyes under high temperature conditions, thereby improving the stability of the biomass thermochromic porous membrane;

[0024] (3) The present invention uses 3-(2-aminoethyl)-aminopropyltrimethoxysilane (AEAPS) to modify the surface of the cleaned glass sheet, mainly because the AEAPS-modified glass can capture the platinum catalyst close to the modified glass, so that the platinum catalyst forms a gradient concentration, and then constructs a film with a gradient cross-linked structure. The two amine groups in the AEAPS molecular structure can coordinate with the platinum atom to form a stable five-membered ring. Therefore, the platinum catalyst close to the surface of the AEAPS-modified glass is captured and loses its catalytic ability. Then, the platinum catalyst in the uniform film-forming liquid diffuses toward the modified glass due to the concentration difference, forming a platinum concentration gradient; the film-forming liquid begins to gel in a high-temperature environment, which can prevent the diffusion movement of the platinum catalyst and produce a gradient cross-linked polysiloxane film;

[0025] (4) The present invention uses vinyl dimethyl silane and hydrogenated silicone oil to prepare a polydimethylsiloxane gel film with a large number of pore structures through a salt template method, and introduces a gradient cross-linking strategy to give the gel film single-sided adhesion;

[0026] (5) The single-sided adhesive biomass thermochromic porous membrane prepared by the present invention can indicate temperature changes through color. As the temperature rises, the shape-stable biomass thermochromic porous membrane changes from a colored solid state (any one of blue, red, green, purple, and yellow) to a white solid state, broadening the color spectrum range of the color change, showing good temperature-responsive color change performance, and having no solvent leakage problem; and having reversible cyclicity and can be reused;

[0027] (6) The present invention utilizes the spatial threshold effect of the pore structure in the porous gel membrane to encapsulate the biomass thermochromic dye with solid-liquid phase change characteristics, wherein the smaller pores in the porous gel membrane can provide sufficient capillary force for the thermochromic dye in liquid state, and have a strong adsorption effect on the phase change solvent, which can effectively solve the problem of easy leakage of the liquid state dye; and the large pore structure interconnected in the porous gel membrane can be filled with more biomass thermochromic dye, which greatly increases the amount of dye used and improves the thermal energy storage performance, which is conducive to giving full play to the dual properties of temperature response color change and thermal energy storage of the biomass thermochromic dye. By establishing the relationship between color and stored heat, the state of thermal energy storage can be intuitively reflected in real time, and the visualization of thermal energy storage can be realized;

[0028] (7) The preparation method of the present invention is simple and easy to operate. Compared with the traditional microcapsule encapsulation method, the preparation cost is greatly saved. The prepared single-sided adhesive biomass thermochromic porous film can indicate the ambient temperature by color change, which overcomes the disadvantage of complicated steps in the traditional encapsulation process and has good application prospects.

[0029] (8) The biomass thermochromic porous membrane prepared by the present invention has excellent self-supporting flexibility. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 It is a schematic flow chart of a method for preparing a single-sided adhesive biomass thermochromic porous membrane of the present invention;

[0031] Figure 2 is the temperature response color change diagram of the biomass thermochromic dye in Example 1 of the present invention;

[0032] Figure 3 is a temperature response color change diagram of the biomass thermochromic porous membrane in Example 1 of the present invention;

[0033] Figure 4 is the color difference value change of the biomass thermochromic porous membrane at different temperatures in Example 1 of the present invention;

[0034] Figure 5 is the differential scanning calorimetry (DSC) curve of the biomass thermochromic porous membrane in Example 1;

[0035] Figure 6 is a color difference value change (ΔE) curve of the biomass thermochromic porous membrane in Example 1 of the present invention under 25 alternating cycles of heating and cooling;

[0036] Figure 7 Optical images of the biomass thermochromic porous membrane in Example 1 in the initial state, folded state and curled state;

[0037] Figure 8 is the temperature response color change diagram of the biomass thermochromic dye in Example 2 of the present invention;

[0038] Fig. 9 is a cross-sectional SEM image of the porous gel membrane in Example 2 of the present invention;

[0039] Fig.10 is a cross-sectional SEM image of the biomass thermochromic porous membrane in Example 2 of the present invention;

[0040] Fig.11 The temperature response color change of the four colors of blue, red, yellow and green biomass thermochromic porous membrane in Example 3 of the present invention;

[0041] Fig.12 This is the temperature response color change diagram of the biomass thermochromic dye in Comparative Example 2 of the present invention. DETAILED DESCRIPTION

[0042] Example 1

[0043] A method for preparing a single-sided adhesive biomass thermochromic porous membrane Figure 1 As shown, the specific steps include:

[0044] (1) heating the solid-liquid phase change solvent tetradecanol to a molten state, adding weakly acidic polyhydroxy biomass or biomass derivatives tea polyphenols, leuco dye crystal violet lactone, and boron nitride nanosheets, wherein the mass ratio of crystal violet lactone, tea polyphenols, and tetradecanol is 1:0.3:100, and the amount of boron nitride nanosheets is 3% of the total mass (3% of the total mass of the solid-liquid phase change solvent, weakly acidic polyhydroxy biomass or biomass derivatives, boron nitride nanosheets, and leuco dye); heating to 120° C. and stirring for reaction for 3 hours, and then placing in a vacuum box at 80° C. with a vacuum degree of -0.1 MPa for 3 hours to obtain a biomass thermochromic dye;

[0045] Figure 2 This is the temperature response color change diagram of the biomass thermochromic dye in Example 1. When the ambient temperature is lower than the melting point of the phase change solvent, the biomass thermochromic dye is in a blue solid state. As the temperature rises, when the ambient temperature is higher than the melting point of the phase change solvent, the biomass thermochromic dye is in a colorless liquid state, showing significant temperature response color change performance.

[0046] (2) AEAPS was used to modify the surface of the cleaned glass sheet to obtain an AEAPS-modified glass sheet; 3.0 g of vinyl dimethyl silane was mixed with 2.64 g of sodium chloride, a salt template agent, by a salt template method, and after uniform dispersion, 0.3 g of a mixture of a platinum catalyst and hydrogenated silicone oil was added, and the mixture was quickly stirred until uniformly dispersed, and then the bubbles in the solution were removed under vacuum for 10 min to obtain a film-forming solution; using a gradient crosslinking strategy, the film-forming solution was cast on the surface of the AEAPS-modified glass sheet, and the platinum catalyst diffused in the direction of the modified glass for 30 min, and then cured at 80°C for 3 h to obtain a polysiloxane gel film containing a template agent, and the gel film was immersed in deionized water and ultrasonicated at 25°C for 24 h, wherein the water was changed every 2 h to remove the template agent in the gel film, and then the film was taken out and placed in a 65°C forced air drying oven for 2 h to remove the moisture in the gel film to obtain a monopolydimethylsiloxane porous gel film;

[0047] (3) The biomass thermochromic dye prepared in step (1) is heated and melted, and the solution is used as an impregnation phase solution. The porous gel membrane prepared in step (2) is immersed in the molten thermochromic dye, and immersed in a vacuum condition of 80° C. for 5 hours to allow the dye to fully fill the pore structure of the porous gel membrane. The gel membrane is then taken out and placed in an oven at 60° C., and the thermochromic dye on the surface of the gel membrane is repeatedly absorbed with oil-absorbing paper until no dye leaks after repeated heating, thereby obtaining a shape-stable biomass thermochromic porous membrane with a thermal conductivity of 0.36 W / (m·K). As the temperature increases, a color change from blue to white occurs.

[0048] Figure 3 This is the temperature response color change diagram of the biomass thermochromic porous membrane in Example 1. As the temperature increases, the shape-stable biomass thermochromic porous membrane changes from a blue solid state to a white solid state, showing good temperature response color change performance and no solvent leakage problem.

[0049] Figure 4 The color difference value of the biomass thermochromic porous film at different temperatures in Example 1 of the present invention increases with the increase of temperature. When the temperature increases from 41°C to 43°C, the color difference value increases from 2.7 to 16.7, and the color of the film changes from blue to white.

[0050] Figure 5The differential scanning calorimetry (DSC) curve of the biomass thermochromic porous membrane in Example 1 shows that the phase transition temperature of the thermochromic porous membrane in Example 1 is 40°C, the temperature at the end of endothermic absorption is 43°C, and the thermal energy storage density is 48 J / g. The color performance test of the biomass thermochromic porous membrane is compared. The results show that as the temperature increases, the thermochromic porous membrane absorbs heat and changes from blue to white. The color change temperature range is 41-43°C, and the temperature at the end of endothermic absorption is 43°C. When the temperature is higher than 43°C, the film color is white, and the thermal energy storage density is 48 J / g.

[0051] Figure 6 The color difference value change (ΔE) curve of the biomass thermochromic film in Example 1 under 25 alternating cycles of heating and cooling is shown in FIG. Figure 6 It can be seen that the prepared biomass thermochromic film has good temperature-responsive color-changing performance and cyclic reversibility.

[0052] Figure 7 These are optical images of the biomass thermochromic porous membrane in the initial state, folded state, and curled state in Example 1. When in the original, folded, and curled states during the heating / cooling cycle, the thermochromic porous membrane exhibits good flexibility and mechanical toughness, indicating that it has good self-supporting flexibility. At the same time, the good self-supporting performance of the thermochromic porous membrane does not affect its temperature-responsive color-changing performance.

[0053] Example 2

[0054] (1) The solid-liquid phase change solvent octadecyl alcohol is heated to a molten state, and the weakly acidic polyhydroxy biomass or biomass derivative L-antihypocyanic acid and the leuco dye 1′,3′-dimethyl-6′-diethylaminofluoran and boron nitride nanosheets are added to the molten phase change solvent octadecyl alcohol, wherein the mass ratio of 1′,3′-dimethyl-6′-diethylaminofluoran, L-antihypocyanic acid and octadecyl alcohol is 1:12:80, and the amount of boron nitride nanosheets is 10% (10% of the total mass of the solid-liquid phase change solvent, the weakly acidic polyhydroxy biomass or biomass derivative, the boron nitride nanosheets and the leuco dye), heated to 120° C. and stirred for reaction for 3 h, and then placed in a vacuum box at 80° C. with a vacuum degree of -0.1 MPa for 3 h to obtain a biomass thermochromic dye;

[0055] Figure 8 This is the temperature response color change diagram of the biomass thermochromic dye in Example 2. When the ambient temperature is lower than the melting point of the dye, the biomass thermochromic dye is in a red solid state. As the temperature rises, when the ambient temperature is higher than the melting point of the dye, the thermochromic dye is in a colorless liquid state, showing significant temperature response color change performance.

[0056] (2) AEAPS was used to modify the surface of the cleaned glass sheet to obtain an AEAPS-modified glass sheet; 2.0 g of vinyl dimethyl silane was mixed with 2.0 g of salt template agent potassium chloride by the salt template method, and after uniform dispersion, 0.1 g of a mixture of a platinum catalyst and hydrogenated silicone oil was added, and the mixture was quickly stirred until uniformly dispersed, and then the bubbles in the solution were removed under vacuum conditions at 25°C for 30 minutes to obtain a film-forming solution; using a gradient crosslinking strategy, the film-forming solution was cast on the surface of the AEAPS-modified glass sheet, and the platinum catalyst diffused in the direction of the modified glass for 30 minutes, and then cured at 70°C for 6 hours to obtain a polysiloxane gel film containing a template agent, and the gel film was immersed in deionized water and ultrasonicated at 40°C for 10 hours, wherein the water was changed every 2 hours to remove the template agent sodium chloride in the gel film, and then the gel film was taken out and placed in a 65°C forced air drying oven for 2 hours to remove the moisture in the gel film to obtain a polydimethylsiloxane porous gel film;

[0057] Fig. 9 This is a cross-sectional SEM image of the porous gel membrane in Example 2. After removing the salt template, the single-sided adhesive porous gel membrane has a relatively large number of micron-scale pore structures, which provide space for the filling of the biomass thermochromic dye and the volume expansion after melting.

[0058] (3) The biomass thermochromic dye prepared in step (1) is heated and melted, and the solution is used as an impregnation phase solution. The porous gel membrane prepared in step (2) is immersed in the molten thermochromic dye, and immersed in a vacuum condition of 120° C. for 5 hours to allow the dye to fully fill the pore structure of the porous gel membrane. The gel membrane is then taken out and placed in an oven at 80° C., and the thermochromic dye on the surface of the gel membrane is repeatedly absorbed with oil-absorbing paper until no dye leaks after repeated heating, thereby obtaining a biomass thermochromic flexible membrane, which can undergo a color change from red to white as the temperature increases.

[0059] Fig.10 is a cross-sectional SEM image of the shape-stable biomass thermochromic porous membrane in Example 2, Fig.10 It can be seen that the thermochromic dye has been filled into the pore structure of the porous gel membrane, and its crystalline thermochromic dye is tightly wrapped by the porous gel membrane supporting material. This is mainly because the micron-scale pore structure has a strong capillary force and surface tension on the molten dye, which is beneficial to the stability of the molten thermochromic dye and prevents leakage.

[0060] Example 3

[0061] (1) heating the solid-liquid phase change solvent octadecyl alcohol to a molten state, adding weakly acidic polyhydroxy biomass or biomass derivative tannic acid and leuco dye crystal violet lactone and boron nitride nanosheets to the molten phase change solvent octadecyl alcohol, wherein the mass ratio of crystal violet lactone, tannic acid and octadecyl alcohol is 1:12:80, and the amount of boron nitride nanosheets is 1% (1% of the total mass of the solid-liquid phase change solvent, weakly acidic polyhydroxy biomass or biomass derivative, boron nitride nanosheets and leuco dye), heating to 120° C. and stirring for reaction for 3 h, and then placing in a vacuum box at 80° C. with a vacuum degree of -0.1 MPa for 3 h to obtain a biomass thermochromic dye;

[0062] (2) AEAPS was used to modify the surface of the cleaned glass sheet to obtain an AEAPS-modified glass sheet; 3.0 g of vinyl dimethyl silane was mixed with 1.32 g of sodium chloride, a salt template agent, by a salt template method, and after uniform dispersion, 0.3 g of a mixture of a platinum catalyst and hydrogenated silicone oil was added, and the mixture was rapidly stirred until uniformly dispersed, and then the bubbles in the solution were removed under vacuum conditions at 25°C for 30 minutes to obtain a film-forming solution; using a gradient crosslinking strategy, the film-forming solution was cast on the surface of the AEAPS-modified glass sheet, and the platinum catalyst diffused in the direction of the modified glass for 30 minutes, and then cured at 100°C for 2 hours to obtain a polysiloxane gel film containing a template agent, and the gel film was immersed in deionized water and ultrasonicated at 40°C for 12 hours, wherein the water was changed every 2 hours to remove the template agent sodium chloride in the gel film, and then the gel film was taken out and placed in a 65°C forced air drying oven for 2 hours to remove the moisture in the gel film to obtain a polydimethylsiloxane porous gel film;

[0063] (3) The biomass thermochromic dye prepared in step (1) is heated and melted, and the solution is used as an impregnation phase solution. The porous gel membrane prepared in step (2) is immersed in the molten thermochromic dye, and immersed in a vacuum condition of 80° C. for 5 hours to allow the dye to fully fill the pore structure of the porous gel membrane. The gel membrane is then taken out and placed in an oven at 60° C., and the thermochromic dye on the surface of the gel membrane is repeatedly absorbed with oil-absorbing paper until no dye leaks after repeated heating, thereby obtaining a yellow biomass thermochromic porous membrane with a color change temperature of 60° C.

[0064] Example 4

[0065] The preparation method is consistent with that of Example 1, except that the leuco dye is 3',6'-dimethoxyfluoran, and a yellow biomass thermochromic porous membrane is obtained.

[0066] Example 5

[0067] The preparation method is consistent with that in Example 1, except that the leuco dye is 7,7-bis(4-(diethylamino)-2-ethoxyphenyl)furano[3,4-b]pyridine-5(7H)-one, and a green biomass thermochromic porous membrane is obtained.

[0068] Fig.11 The temperature response color change diagrams of the four colors of blue, red, yellow and green biomass thermochromic porous membranes in Examples 1, 2, 4 and 5 are as follows. As the temperature increases, the biomass thermochromic porous membrane changes from color to white, showing good temperature response color change performance, and there is no solvent leakage problem.

[0069] Comparative Example 1

[0070] (1) The solid-liquid phase change solvent octadecyl alcohol is heated to a molten state, and the weakly acidic polyhydroxy biomass or biomass derivative L-antihypocyanic acid and the leuco dye 1′,3′-dimethyl-6′-diethylaminofluoran and boron nitride nanosheets are added to the molten fatty alcohol phase change solvent octadecyl alcohol, wherein the mass ratio of 1′,3′-dimethyl-6′-diethylaminofluoran, L-antihypocyanic acid and octadecyl alcohol is 1:12:80, and the amount of boron nitride nanosheets is 10% (10% of the total mass of the solid-liquid phase change solvent, the weakly acidic polyhydroxy biomass or biomass derivative, the boron nitride nanosheets and the leuco dye), heated to 120° C. and stirred for reaction for 3 h, and then placed in a vacuum box at 80° C. with a vacuum degree of -0.1 MPa for 3 h to obtain a biomass thermochromic dye;

[0071] (2) AEAPS was used to modify the surface of the cleaned glass sheet to obtain an AEAPS-modified glass sheet, 2.0 g of vinyl dimethyl silane was added to 0.1 g of a mixture containing a platinum catalyst and hydrogenated silicone oil, and the mixture was quickly stirred until uniformly dispersed, and then the bubbles in the solution were removed under vacuum conditions at 25° C. for 30 minutes to obtain a film-forming solution; the film-forming solution was cast on the surface of the AEAPS-modified glass sheet, and the platinum catalyst diffused in the direction of the modified glass for 30 minutes, and then cured at 70° C. for 6 hours to obtain a polysiloxane gel film;

[0072] (3) The biomass thermochromic dye prepared in step (1) is heated and melted, and the solution is used as an impregnation phase solution. The polysiloxane gel membrane prepared in step (2) is immersed in the molten thermochromic dye, and immersed in a vacuum condition of 120° C. for 5 hours to allow the dye to fully fill the pore structure of the porous gel membrane. The gel membrane is then taken out and placed in an oven at 80° C., and the thermochromic dye on the surface of the gel membrane is repeatedly absorbed with oil-absorbing paper until no dye leaks after repeated heating, thereby obtaining a shape-stable biomass thermochromic membrane.

[0073] The biomass thermochromic dye prepared in step (1) can change from red to colorless as the temperature rises. The thermochromic film changes from white to colorless when the temperature rises, and the color change temperature is 60°C. Although the film shows temperature-responsive color change performance, it is only a change in transparency. When the temperature is below 60°C, it is white and cannot show color. This is mainly because the amount of salt template added during the preparation of the polysiloxane gel film in step (2) is 0, and there is no pore structure inside the film. The polysiloxane gel film without a pore structure is not conducive to the biomass thermochromic dye filling the film according to the original proportion, so it cannot show a colored state.

[0074] Comparative Example 2

[0075] (1) The solid-liquid phase change solvent tetradecanol is heated to a molten state, and weakly acidic polyhydroxy biomass or biomass derivative tannic acid and leuco dye crystal violet lactone and boron nitride nanosheets are added to the molten phase change solvent tetradecanol, wherein the mass ratio of crystal violet lactone, tannic acid and octadecanol is 1:30:100, and the amount of boron nitride nanosheets is 10% (10% of the total mass of the solid-liquid phase change solvent, weakly acidic polyhydroxy biomass or biomass derivative, boron nitride nanosheets and leuco dye), heated to 120° C. and stirred for reaction for 3 h, and then placed in a vacuum box at 80° C. with a vacuum degree of -0.1 MPa for 3 h to obtain a biomass thermochromic dye;

[0076] (2) AEAPS was used to modify the surface of the cleaned glass sheet to obtain an AEAPS-modified glass sheet. By using the salt template method, 3.0 g of vinyl dimethyl silane was mixed with 1.32 g of salt template agent potassium chloride. After uniform dispersion, 0.3 g of a mixture of a platinum catalyst and hydrogenated silicone oil was added, and the mixture was quickly stirred until uniformly dispersed. The bubbles in the solution were then removed under vacuum conditions at 25°C for 30 minutes to obtain a film-forming solution. The film-forming solution was cast on the surface of the AEAPS-modified glass sheet using a gradient crosslinking strategy. After the platinum catalyst diffused toward the modified glass for 30 minutes, the solution was cured at 100°C for 2 hours to obtain a template-containing polysiloxane gel film. The gel film was immersed in deionized water and ultrasonicated at 40°C for 12 hours, with the water changed every 2 hours to remove the template agent sodium chloride in the gel film. The gel film was then taken out and placed in a 65°C forced air drying oven for 2 hours to remove moisture from the gel film to obtain a porous gel film.

[0077] (3) The biomass thermochromic dye prepared in step (1) is heated and melted, and the solution is used as an impregnation phase solution. The porous gel membrane prepared in step (2) is immersed in the molten thermochromic dye, and immersed in a vacuum condition of 80° C. for 5 hours to allow the dye to fully fill the pore structure of the porous gel membrane. The gel membrane is then taken out and placed in an oven at 60° C., and the thermochromic dye on the surface of the gel membrane is repeatedly absorbed with oil-absorbing paper until no dye leaks after repeated heating, thereby obtaining a shape-stable biomass thermochromic porous membrane, which is blue under both high and low temperature conditions and does not have temperature-responsive color-changing properties.

[0078] Fig.12 The temperature response color change diagram of the biomass thermochromic dye in comparative example 2 shows that when the ambient temperature is lower than the melting point of the dye, the biomass thermochromic dye is in a blue solid state. As the temperature rises, when the ambient temperature is higher than the melting point of the dye, the biomass thermochromic dye is in a blue liquid state. Only solid-liquid phase transition occurs, but no color change occurs, and the biomass thermochromic dye does not have temperature response color change performance. In the process of preparing a single-sided adhesive biomass thermochromic porous membrane in the present invention, a thermochromic dye based on a three-component color change system is used as a filling material for the porous gel membrane. In the preparation process, the mass ratio of the leuco body, the weakly acidic polyhydroxy biomass or biomass derivative, and the phase change solvent is crucial to the presentation of the thermochromic performance of the dye. It is necessary to control the appropriate ratio to prepare a thermochromic dye with good temperature response color change performance. In Comparative Example 2, because the proportion of the weakly acidic polyhydroxy biomass or biomass derivative developer in the three-component ratio is too high, the leuco body / developer colored complex cannot be separated after formation, the leuco body / developer complex continues to exist, and the crystal violet lactone always exists in an open-ring conjugated form, thus showing a temperature-independent continuous blue color, resulting in the failure of the preparation of the biomass thermochromic porous membrane.

[0079] Comparative Example 3

[0080] The preparation method is the same as that of Example 1, except that no boron nitride nanosheets are added in step (1), and a shape-stable biomass thermochromic porous membrane is prepared, with a thermal conductivity of 0.23 W / (m·K), and a color change from blue to white occurs with increasing temperature. Compared with the thermochromic porous membrane introduced with 3% boron nitride thermal conductive material in Example 1, the thermal conductivity decreases from 0.36 W / (m·K) to 0.23 W / (m·K), indicating that the introduction of boron nitride can improve the thermal conductivity of the thermochromic porous membrane.

[0081] The embodiments provided above are not intended to limit the scope of the present invention, and the steps described are not intended to limit the execution order thereof. Those skilled in the art may make obvious improvements to the present invention in combination with existing common knowledge, which also fall within the scope of protection defined by the claims of the present invention.

Claims

1. A method for preparing a thermochromic porous membrane, characterized in that: The steps include: (1) heating a solid-liquid phase change solvent to a molten state, adding weakly acidic polyhydroxy biomass or a biomass derivative, boron nitride nanosheets, and a leuco dye, and heating the reaction in a vacuum environment to prepare a biomass thermochromic dye; (2) modifying the surface of a glass sheet with 3-(2-aminoethyl)-aminopropyltrimethoxysilane to obtain a modified glass; uniformly mixing vinyldimethylsilane, a salt template agent, hydrogenated silicone oil, and a platinum catalyst by a salt template method, and removing bubbles by vacuum to obtain a film-forming liquid; using a gradient crosslinking strategy, casting the film-forming liquid on the modified glass, curing, ultrasonically desalting, and drying to obtain a polydimethylsiloxane porous gel membrane; (3) The biomass thermochromic dye prepared in step (1) is heated and melted, and filled into the pores of the polydimethylsiloxane porous gel membrane in step (2) by a vacuum pressure impregnation process to obtain a single-sided adhesive biomass thermochromic porous membrane with a porous structure.

2. The method for preparing a thermochromic porous membrane according to claim 1, characterized in that: In step (1), the weakly acidic polyhydroxy biomass or biomass derivative is an organic weakly acidic biomass or biomass derivative compound with electron accepting property, and is one of L-ascorbic acid, L-ascorbyl palmitate, tea polyphenols, lauryl gallate, and tannic acid.

3. The method for preparing a thermochromic porous membrane according to claim 1, characterized in that: In step (1), the leuco dye is an electron-donating organic compound, which is one of crystal violet lactone, methyl red, bromocresol green, bromocresol purple, phenol red, 1′,3′-dimethyl-6′-diethylaminofluoran, 3′,6′-dimethoxyfluoran, 3,3-bis(4-diethylamino-2-ethoxyphenyl)-4-azaphthalide, and 7,7-bis(4-(diethylamino)-2-ethoxyphenyl)furano[3,4-b]pyridine-5(7H)-one.

4. The method for preparing a thermochromic porous membrane according to claim 1, characterized in that: In step (1), the solid-liquid phase change solvent refers to a solid-liquid phase change solvent that can change from a solid state to a molten state when heated above the phase change temperature of the phase change solvent, and the solid-liquid phase change solvent is one or more of lauryl alcohol, myristyl alcohol, cetyl alcohol, stearyl alcohol, tetradecanol, hexadecanol, octadecyl alcohol, behenyl alcohol, and oleyl alcohol.

5. The method for preparing a thermochromic porous membrane according to claim 1, characterized in that: In step (1), the amount of boron nitride nanosheets added is 0.1% to 15% of the total mass of the solid-liquid phase change solvent, the weakly acidic polyhydroxy biomass or biomass derivative, the boron nitride nanosheets, and the leuco dye.

6. The method for preparing a thermochromic porous membrane according to claim 1, characterized in that: In step (1), the mass ratio of the leuco dye to the weakly acidic polyhydroxy biomass or biomass derivative is 1:0.2-15; the mass ratio of the leuco dye to the solid-liquid phase change solvent is 1:50-300.

7. The method for preparing a thermochromic porous membrane according to claim 1, characterized in that: In step (2), the salt template is one or more of sodium nitrate, potassium nitrate, sodium chloride, potassium chloride, and sodium sulfate; and the ultrasonic desalting time is 6 h to 72 h.

8. The method for preparing a thermochromic porous membrane according to claim 1, characterized in that: In step (2), the mass ratio of vinyldimethylsilane to the total mass of hydrogenated silicone oil and platinum catalyst is 5 to 30:1; the mass ratio of the salt template to the total mass of vinyldimethylsilane, hydrogenated silicone oil and platinum catalyst is 0.1 to 1.2:

1.

9. A single-sided adhesive biomass thermochromic porous film prepared by the method of any one of claims 1 to 8.

10. Application of the single-sided adhesive biomass thermochromic porous film according to claim 9 in the fields of wearable sensors, surface temperature indicators of instruments and equipment, and flexible electronic devices.

Citation Information

Patent Citations

  • Strawberry-like thermochromic energy storage material and preparation method and application thereof

    CN109575911A

  • Thermochromic capsule and preparation method thereof

    CN110964498A

  • Thermotropic bionic color-changing fiber, yarn and fabric and preparation method of thermotropic bionic color-changing fiber, yarn and fabric

    CN114457456A

  • Reversible thermochromic functional composite phase change material as well as preparation method and application thereof

    CN114716980A

  • Double-layer thermal response photonic crystal thin film device and preparation method thereof

    CN115785496A

Cited By

  • Wide-temperature-range pressure heating silicone rubber material for vehicle and preparation method of wide-temperature-range pressure heating silicone rubber material

    CN122080639A