Method for preparing tracer and recoverable irregular nano plastic through internal strong oxidative disintegration

Through internal strong oxidation and disintegration reaction and nanomagnetic powder labeling technology, the problem of difficulty in preparing irregular plastics in the existing technology is solved, and efficient and simple preparation and recycling of nanoplastics is achieved, which enhances environmental representativeness and research convenience.

CN118994756APending Publication Date: 2024-11-22ZHEJIANG UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410785960.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-18
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The prior art is difficult to efficiently and simply prepare and recover irregularly shaped nanoplastics, and their toxic effects and migration and transformation mechanisms in the environment are still unclear.

Method used

Using internal strong oxidation and disintegration reaction combined with SiO2-coated nanomagnetic powder and fluorescein labels, the traceable and recyclable irregular nano-nanomagnetic powder is prepared by extruded plastic pelletization, pressure forming, ultraviolet aging and catalytic oxidation and disintegration reactions. plastic.

Benefits of technology

The preparation of irregularly shaped nanoplastics with environmentally representative characteristics has been achieved, which simplifies operation, improves yield, and facilitates identification and recycling through fluorescent markers, enhancing the research ability of nanoplastic pollutants migration and transformation and chemical effects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118994756A_ABST
    Figure CN118994756A_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing tracer and recoverable irregular nano-plastics through internal strong oxidative disintegration, and belongs to the technical field of micro-plastics. And carrying out melt blending on plastic master batches, an oxidizing agent and the SiO2-coated nano magnetic powder, then carrying out pelletizing, and carrying out film forming by rolling so as to obtain the plastic film. After being subjected to ultraviolet aging, the plastic film is placed in a reducing agent solution to be subjected to catalytic oxidation disintegration reaction. After the reaction, centrifuging to retain precipitate, and repeatedly pickling the precipitate to remove ferric salt; and ultrasonically dispersing the pickled precipitate in the aqueous solution again, adjusting the pH value to be neutral, and terminating the catalytic oxidation disintegration reaction. And adding FITC into the nano-plastic suspension, reacting at room temperature under a dark condition, dialyzing the reaction solution in a dialysis bag to remove the unreacted FITC, retaining the dialysate, and performing vacuum freeze-drying to obtain the traceable and recyclable irregular nano-plastic. Compared with the spherical nano-plastic prepared by the traditional method, the nano-plastic with the irregular shape has more environmental representativeness.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of microplastics, and in particular relates to a method for preparing traceable and recyclable irregular nanoplastics through internal strong oxidative disintegration. Background Art

[0002] Micro-nano plastics have the characteristics of wide distribution, small particle size, difficult degradation, and adsorption of toxic substances. Their removal effect and the current status of environmental pollution are still unclear, which is a hot spot and difficulty in current research. Due to long-term exposure to the environment, micro-nano plastics are subjected to mechanical and oxidative weathering, resulting in a rough surface and many cracks; most micro-nano plastics in the environment are fragmented, including fibrous, elliptical, spherical, triangular, free form and unrecognizable shapes. Due to the smaller particle size, size and specific colloidal properties of nanoplastics, they will have a greater environmental impact than microplastics, cause more complex toxic effects, and are more likely to penetrate biological surfaces.

[0003] According to the study, irregular microplastic (PE) particles with sharp edges and higher curvature variations are more toxic than spherical microplastic beads with smooth surface morphology, and this finding also applies to nanoplastics. The difference in metabolism of irregular and spherical plastics after entering the organism can be attributed to the polymer type, size distribution, and particle shape and morphology, which may affect the formation of the corona and the interaction with proteins and cell membrane receptors. In addition, a study found through molecular dynamics simulation that irregular plastics with lower hydrophobicity can easily penetrate cell membranes due to less lipid absorption compared to spheres, so there is a difference between the actual situation when using spherical nanoplastics to study metabolism in organisms.

[0004] At present, the preparation methods of nanoplastic products include thermal degradation, laser ablation, low-temperature grinding, etc., but these methods are complicated to operate, the product shape is mostly regular spherical, and the yield is relatively low. In addition, due to the small size of nanoplastics, their detection and recycling are extremely difficult. Therefore, it is particularly important to develop a new method for irregularly shaped nanoplastics that is efficient, simple to operate, low-cost, traceable and recyclable. Summary of the invention

[0005] The purpose of the present invention is to solve the deficiencies in the prior art and provide a method for preparing traceable and recyclable irregular nanoplastics by internal strong oxidative disintegration.

[0006] The specific technical solutions adopted by the present invention are as follows:

[0007] The present invention provides a method for preparing traceable and recyclable irregular nanoplastics by internal strong oxidative disintegration, and the specific steps are as follows:

[0008] S1: Melt and blend the dried plastic masterbatch, oxidant and SiO2-coated nano magnetic powder, extrude the plastic pellets, and then roll-press them into a film to obtain a plastic film;

[0009] S2: after ultraviolet aging, the plastic film obtained in step S1 is placed in a reducing agent solution to form a reaction system, and a catalytic oxidation disintegration reaction is performed to obtain a first nanoplastic suspension; after centrifuging the first nanoplastic suspension, a precipitate is retained, an acid solution is added to the precipitate, and the precipitate is repeatedly acid-washed to remove the iron salt; the precipitate after acid washing is ultrasonically dispersed in an aqueous solution again to obtain a second nanoplastic suspension, and the pH value of the second nanoplastic suspension is adjusted to neutral to terminate the catalytic oxidation disintegration reaction;

[0010] S3: adding fluorescein isothiocyanate to the second nanoplastic suspension obtained in step S2, stirring evenly to fully dissolve the fluorescein isothiocyanate, reacting at room temperature and in the dark to obtain a reaction solution; placing the reaction solution in a dialysis bag for dialyzing to remove unreacted fluorescein isothiocyanate, taking the dialysate in the dialysis bag, and performing vacuum freeze-drying to obtain the irregular nanoplastic.

[0011] Preferably, the plastic masterbatch in step S1 is made of biodegradable polybutylene succinate PBS, polybutylene adipate terephthalate PBAT, polylactic acid PLA or polycaprolactone PCL, or traditional plastics polyethylene PE, polystyrene PS, polyvinyl chloride PVC or polypropylene PP.

[0012] Preferably, in step S1, the plastic masterbatch and the oxidant are dried in a vacuum drying oven at 60° C. for 12 to 24 hours; the plastic pellets are placed in a vacuum drying oven at 60° C. for 3 to 5 hours and then pressed into film.

[0013] Preferably, the oxidant is calcium peroxide powder, and the particle size of the oxidant is 200 mesh; the mass ratio of the plastic masterbatch, the oxidant and the SiO2-coated nano-magnetic powder is 1000:5:1.

[0014] Preferably, the preparation method of SiO2-coated nano magnetic powder is as follows:

[0015] The nano magnetic powder is dissolved in anhydrous ethanol, and after ultrasonic dispersion, 25% concentrated ammonia water is added to react for 30 minutes; then tetraethoxysilane is added to continue the reaction for 3 to 4 hours, and a precipitate is obtained by centrifugation; the precipitate is first washed twice with alcohol under magnetic field attraction, and then repeatedly washed three times with distilled water, and the precipitate is dried to obtain SiO2-coated nano magnetic powder; the nano magnetic powder adopts oleic acid-modified ferroferric oxide magnetic nanoparticles, with a concentration of 1 mg / mL, a particle size of 10 nm, and a saturation magnetization intensity of 75emu / g Fe.

[0016] Preferably, in step S1, a twin-screw extruder is used to prepare plastic pellets, and the preset temperatures of the twin-screw extruder are set to 180°C, 190°C, and 200°C in each section from feeding to discharging, respectively, the head temperature is set to 190°C, and the rotation speed is set to 75-100r / min; in step S1, a flat-plate vulcanizing press is used to roll-press the plastic pellets into films, and the rolling heating temperature is set to 120°C to obtain a plastic film with a thickness of 10-150μm.

[0017] Preferably, in step S2, the plastic film is aged under ultraviolet light for 1 to 15 days.

[0018] Preferably, the reducing agent solution in step S2 is a ferrous chloride solution with a concentration of 15 to 120 mg / L; the molar ratio of ferrous ions and calcium peroxide in the catalytic oxidation disintegration reaction system is controlled to be 1:2; and the acid solution in step S2 is a hydrochloric acid solution with a pH value of 1 to 3.

[0019] Preferably, the pH value of the reaction system in step S2 is 1 to 3 to avoid the formation of trivalent iron salt precipitation interfering with the catalytic oxidation disintegration reaction; the catalytic oxidation disintegration reaction time is 4 to 8 hours; the first nanoplastic suspension is centrifuged at 4°C at a speed of 20,000 to 30,000 rpm for 10 to 20 minutes to obtain a precipitate.

[0020] Preferably, in step S3, the concentration of fluorescein isothiocyanate in the second nanoplastic suspension is 0.8-2 mg / L; the reaction solution is placed in a 500-1000 Da dialysis bag for 3-5 days.

[0021] Compared with the prior art, the present invention has the following beneficial effects:

[0022] (1) The present invention uses nanomagnetic powder @SiO2 and fluorescein for dual labeling to prepare irregular nanoplastics that can be traced and magnetically recovered. Fluorescein isothiocyanate (FITC) is used as a fluorescent marker. The isothiocyanate group in FITC can react with the hydroxyl group on the plastic to obtain a stable fluorescent plastic. Compared with other fluorescent molecular dyes, it is better in efficiency, stability and molecular binding force, and can eliminate the interference of other particles during identification.

[0023] (2) The present invention utilizes an internal strong oxidative disintegration reaction to prepare irregularly shaped nanoplastics, which are closer to the morphology of nanoplastics after weathering and light-induced fragmentation in the natural environment. Compared with the spherical regular nanoplastic standard products prepared by traditional methods, this irregularly shaped nanoplastic is more representative of the environment. Ultraviolet aging accelerates the gradual degradation of the plastic, which not only reduces the particle size, but also shortens the reaction degradation time, and quickly obtains plastic particles of the desired particle size. This is of great significance for verifying the migration and transformation of nanoplastic pollutants in the environment and their chemical effects. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 This is a scanning electron microscopy image of PE@Fe3O4-FITC prepared in Example 1;

[0025] Figure 2 This is the fluorescence imaging image of PE@Fe3O4-FITC prepared in Example 1;

[0026] Figure 3 This is a scanning electron microscope image of PBAT@Fe3O4-FITC prepared in Example 2;

[0027] Figure 4 This is the fluorescence imaging image of PBAT@Fe3O4-FITC prepared in Example 2;

[0028] Figure 5 This is a scanning electron microscopy image of PBS@Fe3O4-FITC prepared in Example 3;

[0029] Figure 6 This is the fluorescence imaging image of PBS@Fe3O4-FITC prepared in Example 3. DETAILED DESCRIPTION

[0030] The present invention is further described and illustrated below in conjunction with the accompanying drawings and specific embodiments. The technical features of each embodiment of the present invention can be combined accordingly without conflicting with each other. Three groups of parallel are set in each embodiment.

[0031] Example 1

[0032] This embodiment provides a method for preparing traceable and recyclable irregular nanoplastics using polyethylene (PE) as a plastic masterbatch. The specific method is as follows:

[0033] (1) Preparation of SiO2-coated nanomagnetic powder:

[0034] Take 100μL of 1mg / mL oleic acid-modified ferroferric oxide magnetic nanoparticle suspension and dilute it 100 times to 10mg / L to obtain Fe3O4 suspension. Take 0.5mL of 10mg / L Fe3O4 suspension, dissolve it in 45mL of anhydrous ethanol, transfer it to a 100mL conical flask after ultrasonic dispersion for 30min, add 1.334mL of 25% concentrated ammonia water, and stir vigorously for 30min. Then add 2.233mL of tetraethoxysilane (TEOS) and stir the reaction for 3-4h. After the reaction is completed, centrifuge and wash the precipitate until the washed solution is no longer turbid. Washing method: Wash twice with alcohol under magnetic field attraction, and then wash repeatedly with distilled water three times.

[0035] The washed precipitate was placed in an oven and dried at 70°C to obtain SiO2-coated nanomagnetic powder, which was recorded as nanomagnetic powder@SiO2. The nanomagnetic powder@SiO2 was re-ultrasonicated and dispersed in an ethanol solution for later use.

[0036] (2) In order to prevent the hydrolysis and carbonization of plastic masterbatch caused by the water generated by melting at high temperature, PE and calcium peroxide powder (particle size of 200 mesh) were first dried in a vacuum drying oven at 60°C for 24 hours. The dried PE, calcium peroxide and SiO2-coated nanomagnetic powder were added to the feed port of the twin-screw extruder. The mass ratio of PE, calcium peroxide and SiO2-coated nanomagnetic powder was 1000:5:1.

[0037] The die diameter of the twin screw is 20 mm, and the aspect ratio of the screw is 40:1. The preset temperature of the twin screw extruder is set to 180°C, 190°C, and 200°C from feeding to discharging, the die head temperature is set to 190°C, and the speed is set to 75-100r / min. After melt blending in the twin screw extruder, the plastic pellets are extruded. The plastic pellets are placed in a vacuum drying oven at 60°C and dried for 3 hours.

[0038] The dried plastic pellets were placed in a flat vulcanizer, and the plastic pellets were rolled into films. The rolling heating temperature was set to 120° C. to obtain a plastic film with a thickness of 100 μm.

[0039] (3) After the plastic film obtained in step (2) was subjected to UV aging for 15 days, 0.3636 g of the plastic film was added to a ferrous chloride solution with a concentration of 117.88 mg / L to form a reaction system, and a catalytic oxidation disintegration reaction was performed. Referring to the optimal addition ratio of the Fenton reaction catalyst to the oxidant, the n(Fe 2+ ): n(CaO2) = 1:2. The pH value of the reaction system is controlled to be 1-2 to avoid the formation of trivalent iron salt precipitation to interfere with the catalytic oxidation disintegration reaction. The catalytic oxidation disintegration reaction time is 4 hours to obtain the first nanoplastic suspension.

[0040] The first nanoplastic suspension is centrifuged at 4°C and 20,000 to 30,000 rpm for 10 to 20 minutes to obtain a precipitate. A hydrochloric acid solution with a pH value of 2 is added to the precipitate, and the crystalline iron salt on the surface of the plastic is removed by repeated acid washing. The precipitate after acid washing is ultrasonically dispersed in an aqueous solution again to obtain a second nanoplastic suspension, and the pH value of the second nanoplastic suspension is adjusted to neutral (pH value is about 7) to terminate the catalytic oxidation disintegration reaction.

[0041] (4) Take a certain amount of the second nanoplastic suspension into a small beaker, and cover the small beaker with tin foil to form a light-proof condition. Add fluorescein isothiocyanate (FITC) to the small beaker, stir evenly to fully dissolve the fluorescein isothiocyanate, and react at room temperature in a light-proof condition for 24 hours to obtain a reaction solution. The concentration of FITC in the second nanoplastic suspension is 1 mg / L.

[0042] The reaction solution was placed in a 1000Da dialysis bag and dialyzed for 3 days to remove unreacted FITC. The dialysate in the dialysis bag was taken and freeze-dried in vacuum to obtain an irregular nanoplastic standard product, which was recorded as PE@Fe3O4-FITC.

[0043] Figure 1 The PE@Fe3O4-FITC prepared in this example is a scanning electron microscope image. The particle size of the irregular nanoplastic standard product prepared by the method provided by the present invention is mainly between 100 and 200 nm. The concentration of the product is 7.57×10 12 particles / mL, the average sphericity value of the product was 0.52±0.09, and the average aspect ratio was 0.67±0.10. Figure 2 The fluorescence imaging diagram of PE@Fe3O4-FITC is shown in FIG. 1 , where the upper diagram is a dark field and the lower diagram is a bright field, indicating that the PE@Fe3O4-FITC prepared in this embodiment can show fluorescence and be used for tracing.

[0044] Example 2

[0045] This embodiment provides a method for preparing traceable and recyclable irregular nanoplastics using polybutylene adipate terephthalate (PBAT) as a plastic masterbatch. The specific method is as follows:

[0046] (1) Prepare SiO2-coated nanomagnetic powder, the preparation method is consistent with step (1) of Example 1.

[0047] (2) In order to prevent the hydrolysis and carbonization of the plastic masterbatch caused by the moisture generated by melting at high temperature, PBAT and calcium peroxide powder (particle size of 200 mesh) were first dried in a vacuum drying oven at 60°C for 24 hours. The dried PBAT, calcium peroxide, and SiO2-coated nanomagnetic powder were added to the feed port of the twin-screw extruder. The mass ratio of PBAT, calcium peroxide, and SiO2-coated nanomagnetic powder was 1000:5:1.

[0048] The die diameter of the twin screw is 20 mm, and the aspect ratio of the screw is 40:1. The preset temperature of the twin screw extruder is set to 180°C, 190°C, and 200°C from feeding to discharging, the die head temperature is set to 190°C, and the speed is set to 75-100r / min. After melt blending in the twin screw extruder, the plastic pellets are extruded. The plastic pellets are placed in a vacuum drying oven at 60°C and dried for 3 hours.

[0049] The dried plastic pellets were placed in a flat vulcanizer, and the plastic pellets were rolled into films. The rolling heating temperature was set to 120° C. to obtain a plastic film with a thickness of 50 μm.

[0050] (3) After the plastic film obtained in step (2) was subjected to UV aging for 15 days, 0.1414 g of the plastic film was added to a ferrous chloride solution having a concentration of 45.83 mg / L to form a reaction system, and a catalytic oxidation disintegration reaction was performed. Referring to the optimal addition ratio of the Fenton reaction catalyst to the oxidant, the n(Fe 2+ ): n(CaO2) = 1:2. The pH value of the reaction system is controlled to be 1-2 to avoid the formation of trivalent iron salt precipitation to interfere with the catalytic oxidation disintegration reaction. The catalytic oxidation disintegration reaction time is 4 hours to obtain the first nanoplastic suspension.

[0051] The first nanoplastic suspension is centrifuged at 4°C and 20,000 to 30,000 rpm for 10 to 20 minutes to obtain a precipitate. A hydrochloric acid solution with a pH value of 2 is added to the precipitate, and the crystalline iron salt on the surface of the plastic is removed by repeated acid washing. The precipitate after acid washing is ultrasonically dispersed in an aqueous solution again to obtain a second nanoplastic suspension, and the pH value of the second nanoplastic suspension is adjusted to neutral (pH value is about 7) to terminate the catalytic oxidation disintegration reaction.

[0052] (4) Take a certain amount of the second nanoplastic suspension into a small beaker, and cover the small beaker with tin foil to form a light-proof condition. Add fluorescein isothiocyanate (FITC) to the small beaker, stir evenly to fully dissolve the fluorescein isothiocyanate, and react at room temperature in a light-proof condition for 24 hours to obtain a reaction solution. The concentration of FITC in the second nanoplastic suspension is 1 mg / L.

[0053] The reaction solution was dialyzed in a 1000Da dialysis bag for 3 days to remove unreacted FITC, and the dialysate in the dialysis bag was taken and freeze-dried in vacuum to obtain an irregular nanoplastic standard product, which was recorded as PBAT@Fe3O4-FITC.

[0054] Figure 3 The PBAT@Fe3O4-FITC prepared in this example is a scanning electron microscope image. The irregular nanoplastic standard product prepared by the method provided by the present invention has a particle size of 50 to 200 nm. The concentration of the product is 3.34×10 15 particles / mL, the average sphericity value of the product was 0.27±0.11, and the average aspect ratio was 0.72±0.12. Figure 4 The fluorescence imaging diagram of PBAT@Fe3O4-FITC is shown in FIG. 1 , where the upper diagram is a dark field and the lower diagram is a bright field, indicating that the PBAT@Fe3O4-FITC prepared in this embodiment can show fluorescence and be used for tracing.

[0055] Example 3

[0056] This embodiment provides a method for preparing traceable and recyclable irregular nanoplastics using polybutylene succinate (PBS) as a plastic masterbatch. The specific method is as follows:

[0057] (1) Prepare SiO2-coated nanomagnetic powder, the preparation method is the same as that in Example 1.

[0058] (2) In order to prevent the hydrolysis and carbonization of plastic masterbatch caused by the water generated by melting at high temperature, PBS and calcium peroxide powder (particle size of 200 mesh) were first dried in a vacuum drying oven at 60°C for 24 hours. The dried PBS, calcium peroxide, and SiO2-coated nanomagnetic powder were added to the feed port of the twin-screw extruder. The mass ratio of PBS, calcium peroxide, and SiO2-coated nanomagnetic powder was 1000:5:1.

[0059] The die diameter of the twin screw is 20 mm, and the aspect ratio of the screw is 40:1. The preset temperature of the twin screw extruder is set to 180°C, 190°C, and 200°C from feeding to discharging, the die head temperature is set to 190°C, and the speed is set to 75-100r / min. After melt blending in the twin screw extruder, the plastic pellets are extruded. The plastic pellets are placed in a vacuum drying oven at 60°C and dried for 3 hours.

[0060] The dried plastic pellets were placed in a flat vulcanizer, and the plastic pellets were rolled into films. The rolling heating temperature was set to 120° C. to obtain a plastic film with a thickness of 80 μm.

[0061] (3) After the plastic film obtained in step (2) was subjected to UV aging for 15 days, 0.2586 g of the plastic film was added to a ferrous chloride solution with a concentration of 84.91 mg / L to form a reaction system, and a catalytic oxidation disintegration reaction was performed. Referring to the optimal addition ratio of the Fenton reaction catalyst to the oxidant, the n(Fe 2+ ): n(CaO2) = 1:2. The pH value of the reaction system is controlled to be 1-2 to avoid the formation of trivalent iron salt precipitation to interfere with the catalytic oxidation disintegration reaction. The catalytic oxidation disintegration reaction time is 4 hours to obtain the first nanoplastic suspension.

[0062] The first nanoplastic suspension is centrifuged at 4°C and 20,000 to 30,000 rpm for 10 to 20 minutes to obtain a precipitate. A hydrochloric acid solution with a pH value of 2 is added to the precipitate, and the crystalline iron salt on the surface of the plastic is removed by repeated acid washing. The precipitate after acid washing is ultrasonically dispersed in an aqueous solution again to obtain a second nanoplastic suspension, and the pH value of the second nanoplastic suspension is adjusted to neutral (pH value is about 7) to terminate the catalytic oxidation disintegration reaction.

[0063] (4) Take a certain amount of the second nanoplastic suspension into a small beaker, and cover the small beaker with tin foil to form a light-proof condition. Add fluorescein isothiocyanate (FITC) to the small beaker, stir evenly to fully dissolve the fluorescein isothiocyanate, and react at room temperature in a light-proof condition for 24 hours to obtain a reaction solution. The concentration of FITC in the second nanoplastic suspension is 1 mg / L.

[0064] The reaction solution was placed in a 1000Da dialysis bag and dialyzed for 3 days to remove unreacted FITC. The dialysate in the dialysis bag was taken and freeze-dried in vacuum to obtain an irregular nanoplastic standard product, which was recorded as PBS@Fe3O4-FITC.

[0065] Figure 5 The PBS@Fe3O4-FITC prepared in this example is a scanning electron microscope image. The particle size of the irregular nanoplastic standard product prepared by the method provided by the present invention is mainly between 100 and 200 nm, and the concentration of the standard product is 1.04×10 13 particles / mL, the average sphericity value of the product was 0.29±0.08, and the average aspect ratio was 0.68±0.09. Figure 6 The fluorescence imaging diagram of PBS@Fe3O4-FITC is shown in FIG. 1 , where the upper diagram is a dark field and the lower diagram is a bright field, indicating that the PBS@Fe3O4-FITC prepared in this embodiment can show fluorescence and be used for tracing.

[0066] The fluorescence effect can make it easier to identify the prepared irregular nanoplastic standards when conducting environmental behavior testing and studying chemical effects, eliminating the interference of other particles. In addition, the incorporation of nanomagnetic powder @SiO2 makes nanoplastics easier to recycle, which can facilitate the recycling of environmental testing samples. After recycling, nanoplastics can be used for field monitoring and laboratory research on toxicity, accumulation, weathering, etc.

[0067] Fluorescein isothiocyanate (FITC) can be stored for many years in a cool, dark and dry place. It has good dispersibility, low dye leakage and good photostability. It can be used to detect or track the interaction between conjugates and other biological molecules. The isothiocyanate group in FITC reacts with the hydroxyl group on the plastic to obtain a stable fluorescent plastic. Compared with other fluorescent molecular dyes, it is superior in efficiency, stability and molecular binding force.

[0068] According to the results of Examples 1 to 3, compared with the prior art, the method provided by the present invention can obtain irregular nanoplastic standard products with the desired particle size in a short time. The nanoplastics prepared by internal strong oxidative disintegration are mostly irregular in shape, which is closer to the nanoplastics in the actual environment. Compared with the spherical regular nanoplastic standard products, the products prepared by this method are more representative.

[0069] The above-described embodiment is only a preferred solution of the present invention, but it is not intended to limit the present invention. A person skilled in the relevant technical field may make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, any technical solution obtained by equivalent replacement or equivalent transformation falls within the protection scope of the present invention.

Claims

1. A method for preparing traceable and recyclable irregular nanoplastics by internal strong oxidative disintegration, characterized in that: The specific steps are as follows: S1: Melt and blend the dried plastic masterbatch, oxidant and SiO2-coated nano magnetic powder, extrude the plastic pellets, and then roll-press them into a film to obtain a plastic film; S2: after ultraviolet aging, the plastic film obtained in step S1 is placed in a reducing agent solution to form a reaction system, and a catalytic oxidation disintegration reaction is performed to obtain a first nanoplastic suspension; after centrifuging the first nanoplastic suspension, a precipitate is retained, an acid solution is added to the precipitate, and the precipitate is repeatedly acid-washed to remove the iron salt; the precipitate after acid washing is ultrasonically dispersed in an aqueous solution again to obtain a second nanoplastic suspension, and the pH value of the second nanoplastic suspension is adjusted to neutral to terminate the catalytic oxidation disintegration reaction; S3: adding fluorescein isothiocyanate to the second nanoplastic suspension obtained in step S2, stirring evenly to fully dissolve the fluorescein isothiocyanate, reacting at room temperature and in the dark to obtain a reaction solution; placing the reaction solution in a dialysis bag for dialyzing to remove unreacted fluorescein isothiocyanate, taking the dialysate in the dialysis bag, and performing vacuum freeze-drying to obtain the irregular nanoplastic.

2. The method for preparing traceable and recyclable irregular nanoplastics by internal strong oxidative disintegration according to claim 1, characterized in that: The plastic masterbatch in step S1 is made of biodegradable polybutylene succinate (PBS), polybutylene adipate-terephthalate (PBAT), polylactic acid (PLA) or polycaprolactone (PCL), or traditional plastics such as polyethylene (PE), polystyrene (PS), polyvinyl chloride (PVC) or polypropylene (PP).

3. The method for preparing traceable and recyclable irregular nanoplastics by internal strong oxidative disintegration according to claim 1, characterized in that: In step S1, the plastic masterbatch and the oxidant are dried in a vacuum drying oven at 60° C. for 12 to 24 hours; the plastic pellets are placed in a vacuum drying oven at 60° C. for 3 to 5 hours and then pressed into a film.

4. The method for preparing traceable and recyclable irregular nanoplastics by internal strong oxidative disintegration according to claim 1, characterized in that: The oxidant is calcium peroxide powder, and the particle size of the oxidant is 200 meshes; the mass ratio of the plastic masterbatch, the oxidant and the SiO2-coated nano magnetic powder is 1000:5:

1.

5. The method for preparing traceable and recyclable irregular nanoplastics by internal strong oxidative disintegration according to claim 1, characterized in that: The preparation method of SiO2 coated nano magnetic powder is as follows: The nano magnetic powder is dissolved in anhydrous ethanol, and after ultrasonic dispersion, 25% concentrated ammonia water is added to react for 30 minutes; then tetraethoxysilane is added to continue the reaction for 3 to 4 hours, and a precipitate is obtained by centrifugation; the precipitate is first washed twice with alcohol under magnetic field attraction, and then repeatedly washed three times with distilled water, and the precipitate is dried to obtain SiO2-coated nano magnetic powder; the nano magnetic powder adopts oleic acid-modified ferroferric oxide magnetic nanoparticles, with a concentration of 1 mg / mL, a particle size of 10 nm, and a saturation magnetization intensity of 75emu / g Fe.

6. The method for preparing traceable and recyclable irregular nanoplastics by internal strong oxidative disintegration according to claim 1, characterized in that: In step S1, a twin-screw extruder is used to prepare plastic pellets, and the preset temperatures of the twin-screw extruder are set to 180° C., 190° C., and 200° C. in each section from feeding to discharging, the head temperature is set to 190° C., and the rotation speed is set to 75-100 r / min; in step S1, a flat-plate vulcanizer is used to roll-press the plastic pellets into films, and the rolling heating temperature is set to 120° C. to obtain a plastic film with a thickness of 10-150 μm.

7. The method for preparing traceable and recyclable irregular nanoplastics by internal strong oxidative disintegration according to claim 1, characterized in that: In step S2, the plastic film is aged under ultraviolet light for 1 to 15 days.

8. The method for preparing traceable and recyclable irregular nanoplastics by internal strong oxidative disintegration according to claim 1, characterized in that: The reducing agent solution in step S2 is a ferrous chloride solution with a concentration of 15 to 120 mg / L; the molar ratio of ferrous ions and calcium peroxide in the catalytic oxidation disintegration reaction system is controlled to be 1:2; the acid solution in step S2 is a hydrochloric acid solution with a pH value of 1 to 3.

9. The method for preparing traceable and recyclable irregular nanoplastics by internal strong oxidative disintegration according to claim 1, characterized in that: The pH value of the reaction system in step S2 is 1 to 3 to avoid the formation of trivalent iron salt precipitation interfering with the catalytic oxidation disintegration reaction; the catalytic oxidation disintegration reaction time is 4 to 8 hours; the first nanoplastic suspension is centrifuged at 4°C and 20,000 to 30,000 rpm for 10 to 20 minutes to obtain a precipitate.

10. The method for preparing traceable and recyclable irregular nanoplastics by internal strong oxidative disintegration according to claim 1, characterized in that: In step S3, the concentration of fluorescein isothiocyanate in the second nanoplastic suspension is 0.8-2 mg / L; the reaction solution is placed in a 500-1000 Da dialysis bag for 3-5 days.