Polypropylene master batch containing low-content additive and high-filling-rate calcium carbonate and preparation method of polypropylene master batch
By heat treatment and modification of calcium carbonate powder, combined with low content of additives, a high filling rate polypropylene masterbatch was prepared, which solved the performance problems caused by the high content of additives in the prior art and achieved calcium carbonate The good compatibility and high filling rate of particles with polypropylene resin reduce production costs.
Patent Information
- Application Number
- CN202411090224.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-11-22
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Coupling agents and lubricants with high proportion and heterogeneity in the prior art lead to problems such as precipitation, migration, and discoloration during the preparation of polypropylene masterbatch, which increases costs and affects the performance of the product, and it is difficult to achieve carbonic acid with high filling rate. Good compatibility between calcium particles and polypropylene resin.
通过对碳酸钙粉体进行第一次和第二次热处理,并与改性剂混合,随后与聚丙烯、铝酸酯偶联剂和聚乙烯蜡进行混合和挤出切粒,制备低含量添加剂高填充率的聚丙烯母粒,采用饱和脂肪酸或硬脂酸盐作为包覆剂,提高碳酸钙颗粒与聚丙烯树脂的相容性。
The excellent compatibility and high filling rate between calcium carbonate particles and polypropylene resin are achieved, the use of additives is reduced, the dispersion and melting index of masterbatches are improved, the production cost is reduced, and the processing efficiency is improved.
Smart Images

Figure CN118994778A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of filling masterbatches, and in particular to a polypropylene masterbatch with low additive content and high calcium carbonate filling rate and a preparation method thereof. Background Art
[0002] In the production process of polypropylene products, it is generally necessary to add a certain amount of non-metallic powder for filling and modification, which plays a role in reducing costs and improving performance. Ultrafine calcium carbonate is the most widely used type of non-metallic powder. By adding calcium carbonate, the amount of polypropylene resin can be reduced, the cost can be reduced, and the impact resistance and dimensional stability of polypropylene can be improved, so that polypropylene can obtain better processing performance.
[0003] In order to obtain better addition effects and prevent dust pollution during addition, ultrafine calcium carbonate needs to be prepared into filler masterbatch for addition. Since the surface polarity of calcium carbonate particles is strong and polypropylene is a non-polar material, a certain amount of coupling agent, lubricant and other additives need to be added when preparing polypropylene-based calcium carbonate filler masterbatch, especially high-filling masterbatch, to improve the compatibility and dispersibility of calcium carbonate particles and polypropylene resin, and improve the processing efficiency of masterbatch. According to the fineness and filling rate of calcium carbonate powder, the ratio of coupling agent to lubricant varies from 6 to 10%, and the quality of the ingredients of coupling agent and lubricant is also different. Auxiliary agents with high ratio and different ingredients are not only not conducive to the design of downstream application formula, but also cause precipitation, migration and discoloration, and also increase the cost of masterbatch. Specifically, the coupling agent generally added in the preparation process of filling masterbatch is aluminate or titanate coupling agent. The solvent in the coupling agent is generally a small molecule alkane, which will precipitate during the application process and affect the appearance and performance of the product; lubricants are generally polyethylene wax, paraffin, fatty acid salts and other substances. These substances have low surface energy and high small molecule content, which will not only have negative behaviors such as precipitation and migration, but also affect the printing and thermal bonding properties of the final product due to its low surface energy.
[0004] Therefore, it is of great practical significance to develop a polypropylene masterbatch with low additive content and high calcium carbonate filling rate. Summary of the invention
[0005] The purpose of the present invention is to provide a polypropylene masterbatch with low additive content and high calcium carbonate filling rate and a preparation method thereof in order to overcome the deficiencies of the prior art.
[0006] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0007] The present invention provides a method for preparing polypropylene masterbatch with low additive content and high calcium carbonate filling rate, comprising the following steps:
[0008] 1) subjecting the calcium carbonate powder to a first heat treatment, and then mixing it with a modifier and subjecting it to a second heat treatment to obtain modified calcium carbonate powder;
[0009] 2) mixing modified calcium carbonate powder, polypropylene, aluminate coupling agent and polyethylene wax to obtain a mixture;
[0010] 3) extruding and pelletizing the mixture in sequence to obtain polypropylene masterbatch with low additive content and high calcium carbonate filling rate;
[0011] In step 1), the temperatures of the first heat treatment and the second heat treatment are independently 120-130°C.
[0012] Preferably, in step 1), the rotation speed of the first heat treatment is 600-1000 r / min, and the time of the first heat treatment is 10-30 min; the mixing temperature is 120-130° C., the mixing time is 8-15 min, and the mixing rotation speed is 600-1000 r / min; and the time of the second heat treatment is 10-30 min.
[0013] Preferably, the particle size of the calcium carbonate powder in step 1) is 3 to 6 μm; the mass of the modifier is 0.6 to 1.0% of the mass of the calcium carbonate powder.
[0014] Preferably, the modifier is a saturated fatty acid or a stearate, the saturated fatty acid is stearic acid, lauric acid or caprylic acid, and the stearate is calcium stearate or zinc stearate.
[0015] Preferably, in step 2), the mass ratio of the modified calcium carbonate powder, polypropylene, aluminate coupling agent and polyethylene wax is 90-95:4-8:0.5-1:1-1.5; and the molecular weight of the polyethylene wax is 2000-5000.
[0016] Preferably, the aluminate coupling agent is isopropyl distearoyloxyaluminate.
[0017] Preferably, the mixing temperature in step 2) is 115-140° C., and the mixing time is 10-20 min.
[0018] Preferably, during the extrusion process in step 3), the temperature of the processing zone is 150-170° C., the temperature of the outlet die head is 165-185° C.; and the pelletizing is water ring pelletizing or water-cooled strand pelletizing.
[0019] The present invention also provides a polypropylene masterbatch with low additive content and high calcium carbonate filling rate prepared by the preparation method.
[0020] The beneficial effects of the present invention include the following:
[0021] 1) The present invention performs a pre-coating treatment on calcium carbonate powder, and obtains a good coating effect on calcium carbonate particles by adding a saturated fatty acid or stearate with a mass content of less than 1%, thereby ensuring that the calcium carbonate particles have excellent compatibility with the polypropylene resin, and improving the dispersibility of the calcium carbonate particles in the resin, which not only greatly reduces the addition of lubricants during the processing process, but also improves the calcium carbonate filling rate, effectively controls the moisture content of the filling masterbatch, and obtains a high-filling masterbatch with high calcium carbonate content, smooth surface, high melt index, low moisture content and good dispersibility.
[0022] 2) The present invention performs two heat treatments before and after the modifier is coated on the calcium carbonate powder. The purpose of the heat treatment before coating is to enhance the activity of the surface of the calcium carbonate particles, improve the interaction between calcium carbonate and the modifier, and improve the coating effect. The heat treatment after coating is to further enhance the bonding force between the curing modifier and the surface of the calcium carbonate particles to ensure the coating efficiency.
[0023] 3) The present invention uses a saturated fatty acid or stearate with internal lubrication as a coating agent to modify the calcium carbonate powder, so that the compatibility of the calcium carbonate particles with the polypropylene resin is better, and a low amount of additives is added to prepare a high-filling masterbatch. The filling amount of calcium carbonate in the filling masterbatch of the present invention reaches more than 92%, the amount of additives added is less than 3%, and the preparation process is simple, shortening the processing flow of the polypropylene material, improving the processing efficiency, increasing the output, and reducing the production cost. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 is the contact angle diagram of the polypropylene masterbatch of Example 1;
[0025] Figure 2 is the contact angle diagram of the polypropylene masterbatch of Example 2;
[0026] Figure 3 is the contact angle diagram of the polypropylene masterbatch of Example 3;
[0027] Figure 4 This is the contact angle diagram of the polypropylene masterbatch of Comparative Example 1;
[0028] Figure 5 This is the contact angle diagram of the polypropylene masterbatch of Comparative Example 2;
[0029] Figure 6 This is the contact angle diagram of the polypropylene masterbatch of Comparative Example 3;
[0030] Figure 7 This is a contact angle diagram of the polypropylene masterbatch of Comparative Example 4;
[0031] Figure 8 This is a photo of the polypropylene masterbatch of Example 1;
[0032] Fig. 9This is a photo of the polypropylene masterbatch of Comparative Example 1. DETAILED DESCRIPTION
[0033] The present invention provides a method for preparing polypropylene masterbatch with low additive content and high calcium carbonate filling rate, comprising the following steps:
[0034] 1) subjecting the calcium carbonate powder to a first heat treatment, and then mixing it with a modifier and subjecting it to a second heat treatment to obtain modified calcium carbonate powder;
[0035] 2) mixing modified calcium carbonate powder, polypropylene, aluminate coupling agent and polyethylene wax to obtain a mixture;
[0036] 3) extruding and pelletizing the mixture in sequence to obtain polypropylene masterbatch with low additive content and high calcium carbonate filling rate;
[0037] In step 1), the temperatures of the first heat treatment and the second heat treatment are independently 120-130°C.
[0038] In the present invention, the temperatures of the first heat treatment and the second heat treatment in step 1) are independently preferably 122-128°C, and more preferably 124-125°C.
[0039] In the present invention, the rotation speed of the first heat treatment in step 1) is preferably 600-1000r / min, more preferably 700-900r / min, more preferably 800-850r / min; the time of the first heat treatment is preferably 10-30min, more preferably 15-25min, more preferably 18-20min; the mixing temperature is preferably 120-130°C, more preferably 122-128°C, more preferably 124-125°C; the mixing time is preferably 8-15min, more preferably 10-13min, more preferably 11-12min; the mixing rotation speed is preferably 600-1000r / min, more preferably 700-900r / min, more preferably 800-850r / min; the time of the second heat treatment is preferably 10-30min, more preferably 15-25min, more preferably 20-22min.
[0040] In the present invention, the particle size of the calcium carbonate powder in step 1) is preferably 3-6 μm, more preferably 3.5-5 μm, and more preferably 3.7-4 μm; the mass of the modifier is preferably 0.6-1.0% of the mass of the calcium carbonate powder, more preferably 0.7-0.9%, and more preferably 0.8%.
[0041] In the present invention, the modifier is preferably a saturated fatty acid or a stearate, the saturated fatty acid is preferably stearic acid, lauric acid or caprylic acid, and the stearate is preferably calcium stearate or zinc stearate.
[0042] In the present invention, the activation degree of the modified calcium carbonate powder is ≥98% or the contact angle of the modified calcium carbonate powder is ≥130°.
[0043] In the present invention, the mass ratio of the modified calcium carbonate powder, polypropylene, aluminate coupling agent and polyethylene wax in step 2) is preferably 90-95:4-8:0.5-1:1-1.5, more preferably 92-94:5-7:0.6-0.9:1.1-1.4, more preferably 92.4-93:6:0.7-0.8:1.2-1.3; the molecular weight of the polyethylene wax is preferably 2000-5000, more preferably 2500-4000, more preferably 3000-3500.
[0044] In the present invention, the aluminate coupling agent is preferably isopropyl distearoyloxyaluminate.
[0045] In the present invention, the polypropylene is preferably polypropylene B4808, polypropylene J641 or polypropylene J600.
[0046] In the present invention, the mixing temperature in step 2) is preferably 115-140°C, more preferably 120-135°C, and more preferably 125-130°C; the mixing time is preferably 10-20 min, more preferably 12-18 min, and more preferably 14-15 min.
[0047] In the present invention, during the extrusion process of step 3), the temperature of the processing zone is preferably 150-170°C, further preferably 155-165°C, and more preferably 160°C; the temperature of the outlet die head is preferably 165-185°C, further preferably 170-180°C, and more preferably 175-178°C; and the pelletizing is preferably water ring pelletizing or water-cooled strand pelletizing.
[0048] The present invention also provides a polypropylene masterbatch with low additive content and high calcium carbonate filling rate prepared by the preparation method.
[0049] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.
[0050] In the embodiments and comparative examples, the model of the high-speed stirrer is SHR-300L, the model of the high-speed mixer is SHR-300L, the rotation speed is 820 r / min; and the aperture of the vibrating screen is 5 mm.
[0051] Example 1
[0052] The temperature of the high-speed mixer is set to 125°C. After the high-speed mixer reaches the set temperature, calcium carbonate powder with a particle size of 4 μm is added into the high-speed mixer, and the mixture is stirred at a speed of 850 r / min for mutual friction for 18 minutes. Then, zinc stearate accounting for 0.8% of the mass of the calcium carbonate powder is added, and the mixture is stirred at a speed of 850 r / min for 10 minutes at 125°C. Finally, the stirring of the high-speed mixer is turned off, and the material is heat treated at 125°C and static for 22 minutes to obtain modified calcium carbonate powder.
[0053] Add modified calcium carbonate powder, polypropylene B4808, isopropyl distearoyloxyaluminate and polyethylene wax with a molecular weight of 3000 into a high-speed mixer, the mass ratio of modified calcium carbonate powder, polypropylene, isopropyl distearoyloxyaluminate and polyethylene wax is 92.4:6:0.6:1 (the total mass of the materials is 100 kg), the processing temperature of the high-speed mixer is 125°C, and the mixing time is 15 min to obtain a mixture.
[0054] The mixture was added into a single screw extruder. The temperature of the processing zone of the extruder was 160°C and the temperature of the outlet die head was 175°C. The extruded material was water-ring pelletized and the particles were screened out with a vibrating screen to obtain a polypropylene masterbatch with a low additive content and a high calcium carbonate filling rate.
[0055] Example 2
[0056] The temperature of the high-speed mixer is set to 125°C. After the high-speed mixer reaches the set temperature, calcium carbonate powder with a particle size of 4 μm is added into the high-speed mixer, and the mixture is stirred at a speed of 850 r / min for mutual friction for 18 minutes. Then, zinc stearate accounting for 0.8% of the mass of the calcium carbonate powder is added, and the mixture is stirred at a speed of 850 r / min for 10 minutes at 125°C. Finally, the stirring of the high-speed mixer is turned off, and the material is heat treated at 125°C and static for 22 minutes to obtain modified calcium carbonate powder.
[0057] Add modified calcium carbonate powder, polypropylene B4808, isopropyl distearoyloxyaluminate and polyethylene wax with a molecular weight of 3200 into a high-speed mixer, the mass ratio of modified calcium carbonate powder, polypropylene, isopropyl distearoyloxyaluminate and polyethylene wax is 93:5.3:0.7:1 (the total mass of the materials is 100 kg), the processing temperature of the high-speed mixer is 125°C, and the mixing time is 15 min to obtain a mixture.
[0058] The mixture was added into a single screw extruder. The temperature of the processing zone of the extruder was 160°C and the temperature of the outlet die head was 175°C. The extruded material was water-ring pelletized and the particles were screened out with a vibrating screen to obtain a polypropylene masterbatch with a low additive content and a high calcium carbonate filling rate.
[0059] Example 3
[0060] The temperature of the high-speed mixer is set to 125°C. After the high-speed mixer reaches the set temperature, calcium carbonate powder with a particle size of 5 μm is added into the high-speed mixer, and the mixture is stirred at a high speed of 900 r / min for mutual friction for 20 minutes. Then, zinc stearate accounting for 0.9% of the mass of the calcium carbonate powder is added, and the mixture is stirred at 125°C for 10 minutes at a speed of 900 r / min. Finally, the stirring of the high-speed mixer is turned off, and the material is heat treated at 125°C in a static state for 25 minutes to obtain modified calcium carbonate powder.
[0061] Add modified calcium carbonate powder, polypropylene B4808, isopropyl distearoyloxyaluminate and polyethylene wax with a molecular weight of 3500 into a high-speed mixer, the mass ratio of modified calcium carbonate powder, polypropylene, isopropyl distearoyloxyaluminate and polyethylene wax is 92.4:6:0.6:1 (the total mass of the materials is 100 kg), the processing temperature of the high-speed mixer is 125°C, and the mixing time is 16 min to obtain a mixture.
[0062] The mixture was added into a single screw extruder. The temperature of the processing zone of the extruder was 165°C and the temperature of the outlet die head was 170°C. The extruded material was water-ring pelletized and the particles were screened out with a vibrating screen to obtain a polypropylene masterbatch with a low additive content and a high calcium carbonate filling rate.
[0063] Example 4
[0064] The temperature of the high-speed mixer is set to 128°C. After the high-speed mixer reaches the set temperature, calcium carbonate powder with a particle size of 3.5 μm is added into the high-speed mixer, and the mixture is stirred at a high speed of 800 r / min for mutual friction for 25 minutes. Then, stearic acid accounting for 1.2% of the mass of the calcium carbonate powder is added, and the mixture is stirred at a speed of 800 r / min at 128°C for 13 minutes. Finally, the stirring of the high-speed mixer is turned off, and the material is heat treated at 128°C in a static state for 15 minutes to obtain modified calcium carbonate powder.
[0065] Add modified calcium carbonate powder, polypropylene J641, isopropyl distearoyloxyaluminate and polyethylene wax with a molecular weight of 4000 into a high-speed mixer, the mass ratio of modified calcium carbonate powder, polypropylene, isopropyl distearoyloxyaluminate and polyethylene wax is 91:7:0.8:1.2 (the total mass of the materials is 100 kg), the processing temperature of the high-speed mixer is 130°C, and the mixing time is 12 min to obtain a mixture.
[0066] The mixture was added into a single screw extruder. The temperature of the processing zone of the extruder was 155°C and the temperature of the outlet die head was 180°C. The extruded material was water-cooled and pelletized. The particles were screened out with a vibrating screen to obtain a polypropylene masterbatch with a low additive content and a high calcium carbonate filling rate.
[0067] Comparative Example 1
[0068] Calcium carbonate powder with a particle size of 4 μm, polypropylene B4808, isopropyl distearoyloxyaluminate and polyethylene wax with a molecular weight of 3000 are added into a high-speed mixer, the mass ratio of calcium carbonate powder, polypropylene, isopropyl distearoyloxyaluminate and polyethylene wax is 92.4:6:0.6:1 (the total mass of the materials is 100 kg), the processing temperature of the high-speed mixer is 125°C, and the mixing time is 15 min to obtain a mixture.
[0069] The mixture was added into a single screw extruder. The temperature of the processing zone of the extruder was 160°C and the temperature of the outlet die head was 175°C. The extruded material was water-ring pelletized. The particles were screened out with a vibrating screen to obtain fine particles to obtain polypropylene masterbatch.
[0070] Comparative Example 2
[0071] Calcium carbonate powder with a particle size of 4 μm, polypropylene B4808, isopropyl distearoyloxyaluminate and polyethylene wax with a molecular weight of 3000 are added into a high-speed mixer, the mass ratio of calcium carbonate powder, polypropylene, isopropyl distearoyloxyaluminate and polyethylene wax is 87:8:2.2:2.8 (the total mass of the materials is 100 kg), the processing temperature of the high-speed mixer is 125°C, and the mixing time is 20 min to obtain a mixture.
[0072] The mixture was added into a single screw extruder. The temperature of the processing zone of the extruder was 160°C and the temperature of the outlet die head was 175°C. The extruded material was water-ring pelletized. The particles were screened out with a vibrating screen to obtain fine particles to obtain polypropylene masterbatch.
[0073] Comparative Example 3
[0074] The temperature of the high-speed mixer is set to 125°C. After the high-speed mixer reaches the set temperature, calcium carbonate powder with a particle size of 4 μm is added into the high-speed mixer. At the same time, zinc stearate accounting for 0.8% of the mass of the calcium carbonate powder is added. The mixture is stirred at 125°C at a speed of 850 r / min for 30 minutes. Finally, the stirring of the high-speed mixer is turned off, and the material is heat treated at 125°C in a static state for 22 minutes to obtain modified calcium carbonate powder.
[0075] Add modified calcium carbonate powder, polypropylene B4808, isopropyl distearoyloxyaluminate and polyethylene wax with a molecular weight of 3000 into a high-speed mixer, the mass ratio of modified calcium carbonate powder, polypropylene, isopropyl distearoyloxyaluminate and polyethylene wax is 92.4:6:0.6:1 (the total mass of the materials is 100 kg), the processing temperature of the high-speed mixer is 125°C, and the mixing time is 15 min to obtain a mixture.
[0076] The mixture was added into a single screw extruder. The temperature of the processing zone of the extruder was 160°C and the temperature of the outlet die head was 175°C. The extruded material was water-ring pelletized and the particles were screened out with a vibrating screen to obtain a polypropylene masterbatch with a low additive content and a high calcium carbonate filling rate.
[0077] Comparative Example 4
[0078] The temperature of the high-speed mixer is set to 125°C. After the high-speed mixer reaches the set temperature, calcium carbonate powder with a particle size of 4 μm is added into the high-speed mixer, and the mixture is stirred at a speed of 850 r / min for mutual friction for 18 minutes. Then, zinc stearate accounting for 0.8% of the mass of the calcium carbonate powder is added, and the mixture is stirred at a speed of 850 r / min for 10 minutes at 125°C to obtain modified calcium carbonate powder.
[0079] Add modified calcium carbonate powder, polypropylene B4808, isopropyl distearoyloxyaluminate and polyethylene wax with a molecular weight of 3000 into a high-speed mixer, the mass ratio of modified calcium carbonate powder, polypropylene, isopropyl distearoyloxyaluminate and polyethylene wax is 92.4:6:0.6:1 (the total mass of the materials is 100 kg), the processing temperature of the high-speed mixer is 125°C, and the mixing time is 15 min to obtain a mixture.
[0080] The mixture was added into a single screw extruder. The temperature of the processing zone of the extruder was 160°C and the temperature of the outlet die head was 175°C. The extruded material was water-ring pelletized and the particles were screened out with a vibrating screen to obtain a polypropylene masterbatch with a low additive content and a high calcium carbonate filling rate.
[0081] The properties of the (modified) calcium carbonate powder and polypropylene masterbatch of Examples 1 to 4 and Comparative Examples 1 to 4 were tested, the oil absorption value and contact angle of the (modified) calcium carbonate powder, the ash content and melt index of the polypropylene masterbatch were tested, the smoothness of the surface of the polypropylene masterbatch was checked by visual inspection, and the content of fine particle fragments (fine particle fragments are fragments less than 5 mm, most of which are particles of 1 to 3 mm) in the masterbatch after pelletizing was detected. The test results are shown in Table 1.
[0082] Table 1 Performance test results of modified calcium carbonate powder and polypropylene masterbatch
[0083]
[0084] The present invention adopts processes such as two heat treatments to pretreat calcium carbonate powder in the preparation of filling masterbatch, adopts a lower amount of auxiliary agent added to carry out surface coating of the filler calcium carbonate powder, effectively improves the compatibility of the filling powder with polypropylene resin, reduces the amount of auxiliary agent added in the preparation process of the filling masterbatch, significantly improves the filling rate of the filler calcium carbonate powder, and reduces the production cost.
[0085] By comparing the embodiment with comparative example 1, it can be found that the filling masterbatch prepared by using pretreated calcium carbonate has a higher melt index, better surface smoothness, and a lower content of fine particles in the masterbatch. By comparing the embodiment with comparative example 2, it can be seen that when the calcium carbonate filling amount is reduced and the addition amount of polypropylene resin, aluminate coupling agent, PE wax and other additives is increased, the obtained filling masterbatch has a lower melt index and poorer surface smoothness. By comparing the embodiment with comparative examples 3 and 4, it can be found that when the modified calcium carbonate is not subjected to the front and rear heat treatment process, the obtained modified calcium carbonate has a higher oil absorption value and a smaller contact angle. When the same proportion of calcium carbonate is used for filling, the obtained filling masterbatch has a lower melt index, more fine particles in the prepared masterbatch, and a rough surface.
[0086] The contact angle pictures of the polypropylene masterbatch of Examples 1 to 3 and Comparative Examples 1 to 4 are as follows: Figures 1 to 7 shown.
[0087] The polypropylene masterbatches prepared in Examples 1 to 4 were mixed with polypropylene resin (the mass ratio of polypropylene masterbatches to polypropylene resin was 30:70) and then added to a small laboratory film blowing machine for film blowing (film thickness was 0.05 mm). The number of white spots per square meter of film was detected, and the dispersibility of calcium carbonate powder in the polypropylene masterbatch was evaluated (white spots were not allowed within one square meter, and the presence of white spots indicated poor dispersibility). It can be seen from the results that no white spots appeared within one square meter in the films of Examples 1 to 4, and the dispersibility of calcium carbonate powder in the polypropylene masterbatch was good. The photos of the polypropylene masterbatches of Example 1 and Comparative Example 1 are shown below. Figure 8 and Fig. 9 shown.
[0088] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing polypropylene masterbatch with low additive content and high calcium carbonate filling rate, It is characterized in that The following steps are included: 1) subjecting the calcium carbonate powder to a first heat treatment, and then mixing it with a modifier and subjecting it to a second heat treatment to obtain modified calcium carbonate powder; 2) mixing modified calcium carbonate powder, polypropylene, aluminate coupling agent and polyethylene wax to obtain a mixture; 3) extruding and pelletizing the mixture in sequence to obtain polypropylene masterbatch with low additive content and high calcium carbonate filling rate; In step 1), the temperatures of the first heat treatment and the second heat treatment are independently 120-130°C.
2. The preparation method according to claim 1, It is characterized in that Step 1) The rotation speed of the first heat treatment is 600-1000 r / min, and the time of the first heat treatment is 10-30 min; the mixing temperature is 120-130° C., the mixing time is 8-15 min, and the mixing rotation speed is 600-1000 r / min; the time of the second heat treatment is 10-30 min.
3. The preparation method according to claim 1 or 2, It is characterized in that Step 1) The particle size of the calcium carbonate powder is 3 to 6 μm; the mass of the modifier is 0.6 to 1.0% of the mass of the calcium carbonate powder.
4. The preparation method according to claim 3, It is characterized in that The modifier is a saturated fatty acid or a stearate, the saturated fatty acid is stearic acid, lauric acid or caprylic acid, and the stearate is calcium stearate or zinc stearate.
5. The preparation method according to claim 1 or 4, It is characterized in that Step 2) The mass ratio of the modified calcium carbonate powder, polypropylene, aluminate coupling agent and polyethylene wax is 90-95:4-8:0.5-1:1-1.5; the molecular weight of the polyethylene wax is 2000-5000.
6. The preparation method according to claim 5, It is characterized in that The aluminate coupling agent is isopropyl distearoyloxy aluminate.
7. The preparation method according to claim 5, It is characterized in that Step 2) The mixing temperature is 115-140° C. and the mixing time is 10-20 min.
8. The preparation method according to claim 6 or 7, It is characterized in that During the extrusion process of step 3), the temperature of the processing zone is 150-170° C., and the temperature of the outlet die head is 165-185° C.; and the pelletizing is water ring pelletizing or water-cooled strand pelletizing.
9. Polypropylene masterbatch with low additive content and high calcium carbonate filling rate prepared by the preparation method according to any one of claims 1 to 8.
Citation Information
Patent Citations
Highly-filled calcium carbonate masterbatch for non-woven fabrics and preparation method thereof
CN101914239A
Calcium carbonate filler master batch for polypropylene and polyethylene and preparation process thereof
CN103360680A
Filling masterbatch and preparation method thereof
CN105400064A
Ultra-fine calcium carbonate modified and filled master batch preparation method and product thereof
CN105462061A
Polypropylene filling masterbatch and preparation method thereof
CN106543558A