Phenolic resin-based friction material as well as preparation method and application thereof

By introducing amino-modified nano-silica and double-bond-modified nano-silica into phenolic resin-based friction materials, the stability of the friction coefficient at high temperatures was improved, solving the problem of large fluctuations in the friction coefficient of nano-modified phenolic resin-based composite materials at high temperatures, and enhancing braking performance and wear resistance.

CN118994841APending Publication Date: 2024-11-22ZHENGZHOU BAIYUN IND

Patent Information

Application Number
CN202411250480.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-06
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Existing nano-modified phenolic resin-based composite materials have unstable friction coefficients at high temperatures, exhibiting significant fluctuations with temperature changes, leading to unstable braking performance.

Method used

Amino-modified and double-bond-modified nano-silica were used as nanomaterials to reduce the free phenol content and improve the heat resistance of phenolic resin by participating in the cross-linking reaction of phenolic resin. Furthermore, nanomaterials with different particle sizes were introduced into the friction material to improve the microscopic flatness of the friction interface.

Benefits of technology

This technology improves the stability of friction performance of friction materials at high temperatures, reduces wear and noise, and meets the braking requirements of commercial vehicles in harsh environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118994841A_ABST
    Figure CN118994841A_ABST
Patent Text Reader

Abstract

The invention relates to a phenolic resin-based friction material as well as a preparation method and application thereof, and belongs to the technical field of brake materials. According to the phenolic resin-based friction material, phenolic resin is used as a main adhesive, nitrile rubber is used as an auxiliary adhesive, a fiber material is cooperatively used as a material framework, artificial graphite, calcined petroleum coke, natural graphite and molybdenum disulfide are used as lubricants, and antimony sulfide, zirconium silicate and aluminum oxide are used as modifiers. And barium sulfate and heavy calcium carbonate are used as filling agents, so that the cable has the characteristics of high temperature resistance, low abrasion, low noise and low dual aggressivity. Wherein the nano material participates in the cross-linking reaction of phenolic resin, so that the content of free phenol can be reduced, the heat resistance of the resin can be improved, the microscopic flatness of a friction interface in the braking process can be effectively improved, and the friction interface of the friction material in the friction process can be repaired; and the contact stability of the friction interface of the friction material in the braking process is effectively improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a phenolic resin-based friction material and a preparation method and application thereof, belonging to the technical field of brake materials. Background Art

[0002] In recent years, commercial vehicle technology has achieved rapid development. New technologies represented by new energy technologies have been widely used in commercial vehicles. At the same time, new requirements have been put forward for commercial vehicle braking systems and key components therein (for example, commercial vehicle friction materials). Compared with fuel vehicles, new energy vehicles have the characteristics of strong power, large output torque, fast acceleration, and low background noise. The friction materials involved in braking have strict requirements in terms of braking torque, high-speed braking stability, braking noise, and high temperature resistance. The original friction materials cannot meet the current use requirements of commercial vehicles, especially under special conditions such as heavy-load operation of commercial vehicles, continuous switching between high and low speeds, and extreme working conditions.

[0003] At present, all friction materials used in commercial vehicles are organic friction materials, which are mainly divided into semi-metallic friction materials, low-metal friction materials and metal-free friction materials. Their common characteristics are that the production process, production equipment and raw material supply system are relatively mature and cost-effective, but their friction coefficient decays more seriously under harsh working conditions such as high speed, heavy load or continuous long-term braking. At high temperatures, the friction coefficient fluctuates greatly and wears greatly, which not only shortens the service life of the friction material, but also poses safety hazards.

[0004] How to reduce the obvious drop in braking torque of commercial vehicle friction materials under harsh environments, improve the braking torque and braking torque stability of friction materials under high temperature conditions, and make commercial vehicle friction materials have better wear resistance and high temperature resistance, is the current research focus of commercial vehicle friction materials.

[0005] At present, the main method to improve the performance of commercial vehicle brake pads is to improve its heat resistance by changing the molecular structure of the main adhesive phenolic resin of commercial vehicle brake pads, which mainly includes:

[0006] 1) Etherify or esterify the phenolic hydroxyl group, or "lock" it by chelating the phenolic hydroxyl group with heavy metals to increase its thermal decomposition temperature; for example, compared with ordinary phenolic resin, the brake pad using boron-modified phenolic resin as a binder has significantly reduced thermal decay at high temperature and high speed, and maintains a good friction coefficient and low wear rate throughout the process;

[0007] 2) By changing the curing temperature, pressure, crosslinking agent type, etc. during the curing process of phenolic resin, the release of low molecular weight compounds during the curing process is reduced to form a better crosslinking state;

[0008] 3) Introduce rigid structural units such as aromatic heterocycles with high temperature resistance to improve the heat resistance of phenolic resin to meet more demanding working conditions. For example, the friction material prepared with polybenzoxazine resin as a binder has higher performance in terms of friction coefficient, temperature rise of friction interface, thermal decay resistance, wear resistance and interface friendliness than the friction material prepared with ordinary phenolic resin as a binder.

[0009] However, so far, the above improvements have not been able to widely, effectively and significantly improve the heat resistance and friction coefficient of automotive friction materials in actual applications. The main reason is that the heat resistance of ordinary phenolic resins is difficult to improve, so the above modification methods of phenolic resins have limited effect on improving the heat resistance of friction materials.

[0010] Nanomaterial modification is rarely used in brake pads, especially commercial vehicle brake pads. Currently, the research on nano-modification of brake pads mainly includes the following aspects:

[0011] 1) Ceramic-based nanomaterials are used as modifiers to improve and enhance the performance of friction materials. However, due to the uneven particle size, difficulty in dispersion and poor bonding with the matrix of ceramic-based nanomaterials, the mechanical toughness of phenolic resin will be greatly affected.

[0012] 2) The phenolic resin in the nano-copper modified friction material is prepared by the in-situ generation method. Compared with the ordinary phenolic resin, its initial decomposition temperature is increased, but not significantly, and the cost is high, which makes it difficult to mass produce and commercialize it.

[0013] 3) The use of aluminum and silicate nano-modified phenolic resins is mainly to improve the thermal stability and strength of phenolic resin-based friction materials, but has limited improvement on heat resistance, complex processes, and is difficult to mass produce and market.

[0014] Chinese patent document CN117511120A discloses a nano-modified phenolic resin-based composite material and its preparation method and application. The patent document uses nano-modified phenolic resin (nano-modifier: one or more of silicon dioxide, amino-modified nano-silicon dioxide, double-bond-modified nano-silicon dioxide and epoxy-modified nano-silicon dioxide), polyimide and nitrile rubber as binders, and uses aramid fiber and / or aramid pulp, glass fiber, steel fiber, potassium titanate whisker, flaky graphite, blocky graphite, natural serpentine nanoparticles, vermiculite, potassium feldspar and barite. The nano-modified phenolic resin-based composite material has excellent heat resistance and wear resistance. However, the friction coefficient of the nano-modified phenolic resin-based composite material prepared by the patent document is unstable at high temperature, and the friction coefficient will fluctuate greatly with temperature, resulting in unstable performance during continuous braking. Summary of the invention

[0015] The purpose of the present invention is to provide a phenolic resin-based friction material, which can solve the problem that the friction coefficient of the current nano-modified phenolic resin-based composite material will fluctuate greatly with temperature changes.

[0016] The second object of the present invention is to provide a method for preparing a phenolic resin-based friction material, which can solve the problem that the friction coefficient of the currently prepared nano-modified phenolic resin-based composite material will fluctuate greatly with temperature.

[0017] The third object of the present invention is to provide a phenolic resin-based friction material for use as a brake material, which can solve the problem that the friction coefficient of the phenolic resin-based friction material currently used as a brake material will fluctuate greatly with temperature changes.

[0018] In order to achieve the above objectives, the technical solution adopted by the phenolic resin-based friction material of the present invention is:

[0019] A phenolic resin-based friction material is made of the following components in parts by mass: 3-5 parts of nanomaterials, 5-7 parts of phenolic resins, 2-3 parts of nitrile rubbers, 26-34 parts of fiber materials, 9-11 parts of artificial graphite, 5-7 parts of calcined petroleum cokes, 4-6 parts of natural graphite, 2-3 parts of molybdenum disulfide, 4-6 parts of antimony sulfide, 4-6 parts of zirconium silicate, 1.5-2.5 parts of aluminum oxide, 5.5-18.5 parts of barium sulfate, and 4-16 parts of heavy calcium carbonate; the nanomaterials are composed of amino-modified nanosilicon dioxide and double-bond-modified nanosilicon dioxide.

[0020] The phenolic resin-based friction material of the present invention uses phenolic resin as the main adhesive, nitrile rubber as the auxiliary adhesive, and fiber materials as the material skeleton, while artificial graphite, calcined petroleum coke, natural graphite and molybdenum disulfide are used as lubricants, antimony sulfide, zirconium silicate and aluminum oxide are used as modifiers, and barium sulfate and heavy calcium carbonate are used as fillers. It has the characteristics of high temperature resistance, low wear, low noise, and low dual attack (according to the SAE J2521 standard commonly used in the automotive industry worldwide, the actual test result shows that the braking noise is below 60dB, and the probability of occurrence is less than 2%). Among them, the nanomaterial can reduce the content of free phenol and improve the heat resistance of the resin by participating in the cross-linking reaction of the phenolic resin; by introducing a certain proportion of nanomaterials into the friction material, the microscopic flatness of the friction interface during the braking process can be effectively improved; by adding nanomaterials of different particle sizes, the friction performance stability of the friction material can be improved, mainly because the nanomaterial can repair the friction interface of the friction material during the friction process, and effectively improve the contact stability of the friction interface of the friction material during the braking process.

[0021] Preferably, the nanomaterial is composed of the following components in parts by mass: 2 to 3 parts of amino-modified nano-silicon dioxide and 1 to 2 parts of double-bond-modified nano-silicon dioxide.

[0022] Preferably, the fiber material is composed of the following components in parts by mass: 3 to 5 parts of carbon fiber, 5 to 7 parts of copper fiber, 9 to 11 parts of steel fiber, and 9 to 11 parts of silicate mineral fiber.

[0023] The technical solution adopted by the preparation method of the phenolic resin-based friction material of the present invention is:

[0024] A method for preparing the phenolic resin-based friction material as described above comprises the following steps: mixing the components, hot pressing and curing to obtain the phenolic resin-based friction material.

[0025] The preparation method of the phenolic resin-based friction material of the present invention can ensure that the phenolic resin and other raw materials are evenly distributed and fully cured by mixing the components and then performing hot pressing molding and curing to shape, thereby improving the friction and heat resistance of the material.

[0026] Preferably, the temperature of hot pressing is 170-200°C and the pressure is 280-360 kg / cm 2 In the present invention, the hot pressing can be performed by an automatic hydraulic press, for example, an automatic hydraulic press with a press tonnage of 600 tons, a heating temperature of 0 to 200° C., and a press power of 65 kW.

[0027] Preferably, the curing method is as follows: the hot-pressed material is heated from room temperature to 138-142°C and kept warm for 1.8-2.2 hours, then heated to 158-162°C and kept warm for 1.8-2.2 hours, then heated to 178-182°C and kept warm for 1.8-2.2 hours, and finally heated to 208-212°C and kept warm for 3.8-4.2 hours.

[0028] Preferably, the time required for heating from room temperature to 138-142°C is 0.8-1.2 hours. In the present invention, curing and shaping can be performed in an electric heating ventilation drying oven, for example, a drying oven with a maximum volume of 4m 2 , electric heating ventilation drying box with heating power of 38kW and heating temperature range of 0~300℃.

[0029] The technical solution adopted by the application of the phenolic resin-based friction material of the present invention as a brake material is:

[0030] An application of the phenolic resin-based friction material as described above as a brake material.

[0031] The phenolic resin-based friction material of the present invention has good heat resistance and high temperature resistance when used as a brake material. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 Schematic diagram of the process of preparing the phenolic resin-based friction material of Example 1 of the present invention;

[0033] Figure 2 This is a schematic diagram of the friction coefficient of the phenolic resin-based friction material of Example 1 of the present invention tested according to GB5763-2008;

[0034] Figure 3 It is a schematic diagram of the friction coefficient of common commercial vehicle friction materials in the experimental examples of the present invention tested according to GB5763-2008;

[0035] Figure 4 This is a schematic diagram of the friction coefficient of the phenolic resin-based friction material of Example 1 in the experimental example of the present invention and the common commercial vehicle friction material tested according to GB5763-2018;

[0036] Figure 5 It is a schematic diagram of the wear amount of the phenolic resin-based friction material of Example 1 in the experimental example of the present invention and the common commercial vehicle friction material tested according to different standards. DETAILED DESCRIPTION

[0037] The technical solution of the present invention is further described below in conjunction with specific embodiments.

[0038] The phenolic resin-based friction material of the present invention is a pioneering invention. The phenolic resin-based friction material of the present invention is made of the following components in parts by mass: 3-5 parts of nanomaterials, 5-7 parts of phenolic resins, 2-3 parts of nitrile rubbers, 26-34 parts of fiber materials, 9-11 parts of artificial graphite, 5-7 parts of calcined petroleum coke, 4-6 parts of natural graphite, 2-3 parts of molybdenum disulfide, 4-6 parts of antimony sulfide, 4-6 parts of zirconium silicate, 1.5-2.5 parts of aluminum oxide, 10-14 parts of barium sulfate, and 8-12 parts of heavy calcium carbonate; the nanomaterials are composed of amino-modified nanosilicon dioxide and double-bond-modified nanosilicon dioxide.

[0039] The phenolic resin-based friction material of the present invention uses phenolic resin as the main adhesive, nitrile rubber as the auxiliary adhesive, and fiber materials as the material skeleton. At the same time, artificial graphite, calcined petroleum coke, natural graphite and molybdenum disulfide are used as lubricants, antimony sulfide, zirconium silicate and aluminum oxide are used as modifiers, and barium sulfate and heavy calcium carbonate are used as fillers. It has the characteristics of high temperature resistance, low wear, low noise, and low dual aggressiveness. Among them, nanomaterials can reduce the content of free phenol and improve the heat resistance of the resin by participating in the cross-linking reaction of phenolic resin; by introducing a certain proportion of nanomaterials into the friction material, the microscopic flatness of the friction interface during the braking process can be effectively improved. By adding nanomaterials of different particle sizes, the friction performance stability of the friction material can be improved. The main reason is that the nanomaterials can repair the friction interface of the friction material during the friction process, and effectively improve the contact stability of the friction interface of the friction material during the braking process.

[0040] In the present invention, the nitrile rubber needs to meet the following conditions: the acrylonitrile content is 32-34%; the Mooney viscosity ML100℃1+4: 45-60;

[0041] The phenolic resin needs to meet the following conditions: free phenol ≤ 1.5%; the polymerization rate at 150°C is 60 to 95s.

[0042] The average length of carbon fiber is 1 to 3 mm, and the average diameter is 10 to 30 μm;

[0043] The average length of copper fibers is 1 to 3 mm, and the average diameter is 0.2 to 0.5 mm;

[0044] The average length of steel fibers is 3-4 mm, and the average diameter is 0.1-0.2 mm;

[0045] The average length of the mineral fibers is 300-500 μm, and the average diameter is 30-80 μm.

[0046] Artificial graphite needs to meet the following conditions: C% ≥ 99%; volatile matter ≤ 0.5%; ash ≤ 0.5%;

[0047] Calcined petroleum coke needs to meet the following conditions: C% ≥ 97%; volatile matter ≤ 1.5%; ash ≤ 1.5%;

[0048] Natural graphite needs to meet the following conditions: C% ≥ 90%; volatile matter ≤ 5%; ash content ≤ 1.5%.

[0049] Molybdenum disulfide needs to meet the following conditions: MoS2 ≥ 99%; 1000 mesh sieve residue % ≤ 1.0%;

[0050] Antimony sulfide needs to meet the following conditions: Sb2O3% ≥ 70%; 200 mesh sieve residue% ≤ 2.0%;

[0051] Zirconium silicate needs to meet the following conditions: ZrO2% ≥ 60%; 1000 mesh sieve residue ≤ 1%;

[0052] Alumina needs to meet the following conditions: Al2O3% ≥ 95%; 325 mesh sieve residue ≤ 1%;

[0053] Barium sulfate needs to meet the following conditions: BaSO4% ≥ 98%; 325 mesh sieve residue ≤ 1%;

[0054] Heavy calcium carbonate needs to meet the following conditions: CaCO3% ≥ 80%; 320 mesh sieve residue ≤ 2.0%.

[0055] The particle size of amino-modified nano-silica is 20 to 40 nm; the particle size of double-bond-modified nano-silica is 30 to 50 nm.

[0056] In the following examples and comparative examples, amino-modified nano-silica is provided by the Nano-Engineering Research Institute of Henan University, and the product model is RNS-A. Double-bond-modified nano-silica is provided by the Nano-Engineering Research Institute of Henan University, and the product model is RNS-D. The manufacturer of phenolic resin is Shengquan Resin, and the product model is PF (free phenol ≤ 1.5%; polymerization rate at 150°C is 60-95s). The manufacturer of nitrile rubber is Nanjing Shengdong Technology Co., Ltd., and the product model is NBR (acrylonitrile content is 32-34%; Mooney viscosity ML100°C 1+4: 45-60). The manufacturer of copper fiber and steel fiber is Nanyang Junlong, and silicate mineral fiber (product model is The manufacturer of LFC101 is Lapulas, the manufacturer of artificial graphite and calcined petroleum coke is Jinwan Special Carbon, the manufacturer of natural graphite is Jixi Huizeyuan Graphite Co., Ltd., the manufacturer of molybdenum disulfide is Luoyang Molybdenum Co., Ltd., the manufacturer of antimony sulfide is Jiujiang Kunsheng Mining Co., Ltd., the manufacturer of zirconium silicate and alumina is Great Wall Aluminum Co., Ltd., the manufacturer of barium sulfate is Yinchen Micro Powder Factory, and the manufacturer of heavy calcium carbonate is Jiaozuo Calcium Source.

[0057] 1. Specific embodiments of the phenolic resin-based friction material and the preparation method thereof of the present invention are as follows:

[0058] Example 1

[0059] The phenolic resin-based friction material of this embodiment is made of the following components in parts by mass: 4 parts of nanomaterials, 6 parts of phenolic resin, 2.5 parts of nitrile rubber, 4 parts of carbon fiber, 6 parts of copper fiber, 10 parts of steel fiber, 10 parts of silicate mineral fiber, 10 parts of artificial graphite, 6 parts of calcined petroleum coke, 5 parts of natural graphite, 2.5 parts of molybdenum disulfide, 5 parts of antimony sulfide, 5 parts of zirconium silicate, 2 parts of aluminum oxide, 12 parts of barium sulfate, and 10 parts of heavy calcium carbonate; the nanomaterial is composed of amino-modified nano-silica and double-bond-modified nano-silica, and the mass fractions of amino-modified nano-silica and double-bond-modified nano-silica are both 2 parts. In this embodiment, the average particle size of the amino-modified nano-silicon dioxide is 30nm, the average particle size of the double-bond-modified nano-silicon dioxide is 40nm; the average length of the carbon fiber is 2mm, the average diameter is 20μm, the average length of the copper fiber is 2mm, the average diameter is 0.3mm, the average length of the steel fiber is 3.5mm, the average diameter is 0.15mm, the average length of the mineral fiber is 400μm, and the average diameter is 50μm; molybdenum disulfide meets the following conditions: MoS2≥99%; 1000 mesh sieve The residue% ≤1.0%; antimony sulfide meets the following conditions: Sb2O3% ≥70%; 200 mesh sieve residue% ≤2.0%; zirconium silicate meets the following conditions: ZrO2% ≥60%; 1000 mesh sieve residue ≤1%; alumina meets the following conditions: Al2O3% ≥95%; 325 mesh sieve residue ≤1%; barium sulfate meets the following conditions: BaSO4% ≥98%; 325 mesh sieve residue ≤1%; heavy calcium carbonate meets the following conditions: CaCO3% ≥80%; 320 mesh sieve residue ≤2.0%.

[0060] The preparation method of the phenolic resin-based friction material of this embodiment is as follows: Figure 1 As shown, the specific steps include:

[0061] (1) The nanomaterial, phenolic resin and nitrile rubber are uniformly stirred at low speed by using a barrel rotary and high-speed flying blade rotary mixer (barrel reduction motor power of 4.0 kW, maximum mixing weight of 100 kg, barrel speed of 0-11 rpm, flying blade group speed of 0-1450 rpm), the stirring time is 5 min, and the temperature is controlled below 80° C. to obtain a resin mixture; then, powdered raw materials (artificial graphite, calcined petroleum coke, natural graphite, molybdenum disulfide, antimony sulfide, zirconium silicate, aluminum oxide, barium sulfate and heavy calcium carbonate) are added to a vertical high-speed mixer (motor power of 30 kW, maximum mixing weight of 100 kg, spindle speed of 950 rpm, flying blade group speed of 1450 rpm), stirred for 5 min, then the resin mixture is added, and stirring is continued for 5 min, and finally, fiber materials (carbon fiber, copper fiber, steel fiber and silicate mineral fiber) are added, and stirring is continued for 5 min to obtain a friction raw material;

[0062] (2) The friction raw material is hot-pressed by an automatic hydraulic press (press tonnage is 600 tons, heating temperature is 0-200°C, power is 65kW) to obtain a hot-pressed material. The hot-pressing temperature is 170-200°C and the pressure is 350kg / cm 2 , the time is 5 to 8 minutes; during the hot pressing process, exhaust is required, the number of exhausts is 5 times, each time the pressure is maintained for 10 seconds and the pause is 5 seconds;

[0063] (3) The hot-pressed material is subjected to a curing heat treatment in an electric heating ventilation drying oven. During the heat treatment, the hot-pressed material is heated from room temperature to 140°C and then kept warm for 1 hour, then heated to 160°C and then kept warm for 2 hours, then heated to 180°C and then kept warm for 2 hours, and finally heated to 210°C and then kept warm for 4 hours; the time required to heat from room temperature to 140°C is 1 hour;

[0064] (4) The material after the solidification and shaping heat treatment is processed by a CNC automatic grinder, including thickness, grooving and chamfering, and finally printed and packaged to obtain the friction material for the brake pad.

[0065] Example 2

[0066] The phenolic resin-based friction material of this embodiment is made of the following components in parts by mass: 3 parts of nanomaterials, 5 parts of phenolic resin, 2 parts of nitrile rubber, 3 parts of carbon fiber, 5 parts of copper fiber, 9 parts of steel fiber, 9 parts of silicate mineral fiber, 9 parts of artificial graphite, 5 parts of calcined petroleum coke, 4 parts of natural graphite, 2 parts of molybdenum disulfide, 4 parts of antimony sulfide, 4 parts of zirconium silicate, 1.5 parts of aluminum oxide, 18.5 parts of barium sulfate, and 16 parts of heavy calcium carbonate; the nanomaterial is composed of amino-modified nano-silica and double-bond-modified nano-silica, and the mass portions of amino-modified nano-silica and double-bond-modified nano-silica are 2 parts and 1 part, respectively. In this embodiment, the average particle size of the amino-modified nano-silicon dioxide is 20nm, the average particle size of the double-bond-modified nano-silicon dioxide is 30nm; the average length of the carbon fiber is 1mm, the average diameter is 10μm, the average length of the copper fiber is 1mm, the average diameter is 0.2mm, the average length of the steel fiber is 3mm, the average diameter is 0.1mm, the average length of the mineral fiber is 300μm, and the average diameter is 30μm; molybdenum disulfide meets the following conditions: MoS2≥99%; 1000 mesh sieve residue The following conditions shall apply to the following materials: Sb2O3% ≥ 70%; 200 mesh sieve residue % ≤ 2.0%; zirconium silicate shall meet the following conditions: ZrO2% ≥ 60%; 1000 mesh sieve residue ≤ 1%; alumina shall meet the following conditions: Al2O3% ≥ 95%; 325 mesh sieve residue ≤ 1%; barium sulfate shall meet the following conditions: BaSO4% ≥ 98%; 325 mesh sieve residue ≤ 1%; heavy calcium carbonate shall meet the following conditions: CaCO3% ≥ 80%; 320 mesh sieve residue ≤ 2.0%.

[0067] The preparation method of the phenolic resin-based friction material of this embodiment specifically includes the following steps:

[0068] (1) The nanomaterial, phenolic resin and nitrile rubber are uniformly stirred at low speed by using a barrel rotary and high-speed flying blade rotary mixer (barrel reduction motor power of 4.0 kW, maximum mixing weight of 100 kg, barrel speed of 0-11 rpm, flying blade group speed of 0-1450 rpm), the stirring time is 5 min, and the temperature is controlled below 80° C. to obtain a resin mixture; then, powdered raw materials (artificial graphite, calcined petroleum coke, natural graphite, molybdenum disulfide, antimony sulfide, zirconium silicate, aluminum oxide, barium sulfate and heavy calcium carbonate) are added to a vertical high-speed mixer (motor power of 30 kW, maximum mixing weight of 100 kg, spindle speed of 950 rpm, flying blade group speed of 1450 rpm), stirred for 5 min, then the resin mixture is added, and stirring is continued for 5 min, and finally, fiber materials (carbon fiber, copper fiber, steel fiber and silicate mineral fiber) are added, and stirring is continued for 5 min to obtain a friction raw material;

[0069] (2) The friction raw material is hot-pressed by an automatic hydraulic press (press tonnage is 600 tons, heating temperature is 0-200°C, power is 65kW) to obtain a hot-pressed material. The hot-pressing temperature is 170-200°C and the pressure is 350kg / cm 2 , the time is 5 to 8 minutes; during the hot pressing process, exhaust is required, the number of exhausts is 5 times, each time the pressure is maintained for 10 seconds and the pause is 5 seconds;

[0070] (3) The hot-pressed material is subjected to a curing heat treatment in an electric heating ventilation drying oven. During the heat treatment, the hot-pressed material is heated from room temperature to 140°C and then kept warm for 1 hour, then heated to 160°C and then kept warm for 2 hours, then heated to 180°C and then kept warm for 2 hours, and finally heated to 210°C and then kept warm for 4 hours; the time required to heat from room temperature to 140°C is 1 hour;

[0071] (4) The material after the solidification and shaping heat treatment is processed by a CNC automatic grinder, including thickness, grooving and chamfering, and finally printed and packaged to obtain the friction material for the brake pad.

[0072] Example 3

[0073] The phenolic resin-based friction material of this embodiment is made of the following components in parts by mass: 5 parts of nanomaterials, 7 parts of phenolic resin, 3 parts of nitrile rubber, 5 parts of carbon fiber, 7 parts of copper fiber, 11 parts of steel fiber, 11 parts of silicate mineral fiber, 11 parts of artificial graphite, 7 parts of calcined petroleum coke, 6 parts of natural graphite, 3 parts of molybdenum disulfide, 6 parts of antimony sulfide, 6 parts of zirconium silicate, 2.5 parts of aluminum oxide, 5.5 parts of barium sulfate, and 4 parts of heavy calcium carbonate; the nanomaterial is composed of amino-modified nano-silica and double-bond-modified nano-silica, and the mass portions of amino-modified nano-silica and double-bond-modified nano-silica are 3 parts and 2 parts, respectively. In this embodiment, the average particle size of the amino-modified nano-silicon dioxide is 40nm, the average particle size of the double-bond-modified nano-silicon dioxide is 50nm; the average length of the carbon fiber is 3mm, the average diameter is 30μm, the average length of the copper fiber is 3mm, the average diameter is 0.5mm, the average length of the steel fiber is 4mm, the average diameter is 0.2mm, the average length of the mineral fiber is 500μm, and the average diameter is 80μm; molybdenum disulfide meets the following conditions: MoS2≥99%; 1000 mesh sieve residue The following conditions shall apply to the following materials: Sb2O3% ≥ 70%; 200 mesh sieve residue % ≤ 2.0%; zirconium silicate shall meet the following conditions: ZrO2% ≥ 60%; 1000 mesh sieve residue ≤ 1%; alumina shall meet the following conditions: Al2O3% ≥ 95%; 325 mesh sieve residue ≤ 1%; barium sulfate shall meet the following conditions: BaSO4% ≥ 98%; 325 mesh sieve residue ≤ 1%; heavy calcium carbonate shall meet the following conditions: CaCO3% ≥ 80%; 320 mesh sieve residue ≤ 2.0%.

[0074] The preparation method of the phenolic resin-based friction material of this embodiment specifically includes the following steps:

[0075] (1) The nanomaterial, phenolic resin and nitrile rubber are uniformly stirred at low speed by using a barrel rotary and high-speed flying blade rotary mixer (barrel reduction motor power of 4.0 kW, maximum mixing weight of 100 kg, barrel speed of 0-11 rpm, flying blade group speed of 0-1450 rpm), the stirring time is 5 min, and the temperature is controlled below 80° C. to obtain a resin mixture; then, powdered raw materials (artificial graphite, calcined petroleum coke, natural graphite, molybdenum disulfide, antimony sulfide, zirconium silicate, aluminum oxide, barium sulfate and heavy calcium carbonate) are added to a vertical high-speed mixer (motor power of 30 kW, maximum mixing weight of 100 kg, spindle speed of 950 rpm, flying blade group speed of 1450 rpm), stirred for 5 min, then the resin mixture is added, and stirring is continued for 5 min, and finally, fiber materials (carbon fiber, copper fiber, steel fiber and silicate mineral fiber) are added, and stirring is continued for 5 min to obtain a friction raw material;

[0076] (2) The friction raw material is hot-pressed by an automatic hydraulic press (press tonnage is 600 tons, heating temperature is 0-200°C, power is 65kW) to obtain a hot-pressed material. The hot-pressing temperature is 170-200°C and the pressure is 350kg / cm 2 , the time is 5 to 8 minutes; during the hot pressing process, exhaust is required, the number of exhausts is 5 times, each time the pressure is maintained for 10 seconds and the pause is 5 seconds;

[0077] (3) The hot-pressed material is subjected to a curing heat treatment in an electric heating ventilation drying oven. During the heat treatment, the hot-pressed material is heated from room temperature to 140°C and then kept warm for 1 hour, then heated to 160°C and then kept warm for 2 hours, then heated to 180°C and then kept warm for 2 hours, and finally heated to 210°C and then kept warm for 4 hours; the time required to heat from room temperature to 140°C is 1 hour;

[0078] (4) The material after the solidification and shaping heat treatment is processed by a CNC automatic grinder, including thickness, grooving and chamfering, and finally printed and packaged to obtain the friction material for the brake pad.

[0079] Comparative Example 1

[0080] The only difference between the phenolic resin-based friction material of this comparative example and the phenolic resin-based friction material of Example 1 is that in the phenolic resin-based friction material of this comparative example, the mass fraction of artificial graphite is 0 parts, the total mass fraction of artificial graphite, calcined petroleum coke and natural graphite is 21 parts, and the mass ratio of calcined petroleum coke to natural graphite is 6:5.

[0081] Comparative Example 2

[0082] The only difference between the phenolic resin-based friction material of this comparative example and the phenolic resin-based friction material of Example 1 is that in the phenolic resin-based friction material of this comparative example, the mass fraction of calcined petroleum coke is 0 parts, the total mass fraction of artificial graphite, calcined petroleum coke and natural graphite is 21 parts, and the mass ratio of artificial graphite to natural graphite is 10:5.

[0083] Comparative Example 3

[0084] The only difference between the phenolic resin-based friction material of this comparative example and the phenolic resin-based friction material of Example 1 is that in the phenolic resin-based friction material of this comparative example, the mass fraction of natural graphite is 0 parts, the total mass fraction of artificial graphite, calcined petroleum coke and natural graphite is 21 parts, and the mass ratio of artificial graphite to calcined petroleum coke is 10:6.

[0085] Comparative Example 4

[0086] The only difference between the phenolic resin-based friction material of this comparative example and the phenolic resin-based friction material of Example 1 is that in the phenolic resin-based friction material of this comparative example, the mass fraction of antimony sulfide is 0 parts, the total mass fraction of antimony sulfide, zirconium silicate and aluminum oxide is 12 parts, and the mass ratio of zirconium silicate to aluminum oxide is 5:2.

[0087] Comparative Example 5

[0088] The only difference between the phenolic resin-based friction material of this comparative example and the phenolic resin-based friction material of Example 1 is that in the phenolic resin-based friction material of this comparative example, the mass fraction of zirconium silicate is 0 parts, the total mass fraction of antimony sulfide, zirconium silicate and aluminum oxide is 12 parts, and the mass ratio of antimony sulfide to aluminum oxide is 5:2.

[0089] Comparative Example 6

[0090] The only difference between the phenolic resin-based friction material of this comparative example and the phenolic resin-based friction material of Example 1 is that in the phenolic resin-based friction material of this comparative example, the mass fraction of aluminum oxide is 0 parts, the total mass fraction of antimony sulfide, zirconium silicate and aluminum oxide is 12 parts, and the mass ratio of antimony sulfide to zirconium silicate is 5:5.

[0091] The component proportions of the phenolic resin-based friction materials of Examples 1-3 are listed in Table 1.

[0092] Table 1 Component ratios of phenolic resin-based friction materials of Examples 1-3

[0093]

[0094] 2. The specific examples of the application of the phenolic resin-based friction material of the present invention as a brake material are as follows:

[0095] Any phenolic resin-based friction material in Examples 1-3 can be used as a brake material.

[0096] Experimental example

[0097] In order to evaluate the high temperature resistance and wear resistance of the phenolic resin-based friction materials of each embodiment and comparative example and the common commercial vehicle friction materials, performance tests were conducted according to the relevant test methods specified in standards GB5763-2018 and GB5763-2008. The test results of the phenolic resin-based friction materials of Example 1 and the common commercial vehicle friction materials are shown in Tables 2-4, Figure 2-5Table 2 shows the friction coefficients of the phenolic resin-based friction material of Example 1 and the common commercial vehicle friction material tested according to GB5763-2008, Table 3 shows the friction coefficients of the phenolic resin-based friction material of Example 1 and the common commercial vehicle friction material tested according to GB5763-2018, and Table 4 shows the wear amounts of the phenolic resin-based friction material of Example 1 and the common commercial vehicle friction material tested according to different standards. Figure 2 Schematic diagram of the friction coefficient of the phenolic resin-based friction material of Example 1 tested according to GB5763-2008, Figure 3 This is a schematic diagram of the friction coefficient of common commercial vehicle friction materials tested according to GB5763-2008. Figure 4 Schematic diagram of the friction coefficient of the phenolic resin-based friction material of Example 1 and the common commercial vehicle friction material tested according to GB5763-2018, Figure 5 It is a schematic diagram of the wear amount of the phenolic resin-based friction material of Example 1 and common commercial vehicle friction materials tested according to different standards.

[0098] Table 2 Friction coefficients of the phenolic resin-based friction material of Example 1 and common commercial vehicle friction materials tested according to GB5763-2008

[0099]

[0100] Table 3 Friction coefficients of the phenolic resin-based friction material of Example 1 and common commercial vehicle friction materials tested according to GB5763-2018

[0101]

[0102] Table 4 Wear amount of the phenolic resin-based friction material of Example 1 and common commercial vehicle friction materials tested according to different standards

[0103]

[0104] From Table 2-4 and Figure 2-5 It can be seen that, compared with common commercial vehicle friction materials on the market, the phenolic resin-based friction material of Example 1 has a higher friction coefficient and a lower wear rate.

[0105] In addition, the friction coefficients of the phenolic resin-based friction materials of Examples 2-3 tested according to GB5763-2008 are shown in Table 5, the friction coefficients of the phenolic resin-based friction materials of Examples 2-3 tested according to GB5763-2018 are shown in Table 6, and the wear amounts of the phenolic resin-based friction materials of Examples 2-3 tested according to different standards are shown in Table 7. The friction coefficients of the phenolic resin-based friction materials of the comparative examples tested according to GB5763-2008 are shown in Table 8, the friction coefficients of the phenolic resin-based friction materials of the comparative examples tested according to GB5763-2018 are shown in Table 9, and the wear amounts of the phenolic resin-based friction materials of the comparative examples tested according to different standards are shown in Table 10.

[0106] Table 5 Friction coefficients of the phenolic resin-based friction materials of Examples 2-3 and common commercial vehicle friction materials tested according to GB5763-2008

[0107]

[0108] Table 6 Friction coefficients of phenolic resin-based friction materials of Examples 2-3 and common commercial vehicle friction materials tested according to GB5763-2018

[0109]

[0110] Table 7 Wear amount of phenolic resin-based friction materials of Examples 2-3 and common commercial vehicle friction materials tested according to different standards

[0111]

[0112] Table 8 Friction coefficients of phenolic resin-based friction materials of comparative examples 1-6 and common commercial vehicle friction materials tested according to GB5763-2008

[0113]

[0114] Table 9 Friction coefficients of phenolic resin-based friction materials of comparative examples 1-6 and common commercial vehicle friction materials tested according to GB5763-2018

[0115]

[0116]

[0117] Table 10 Wear amount of phenolic resin-based friction materials of comparative examples 1-6 and common commercial vehicle friction materials tested according to different standards

[0118]

Claims

1. A phenolic resin-based friction material, It is characterized in that The invention is prepared from the following components in parts by mass: 3-5 parts of nano materials, 5-7 parts of phenolic resin, 2-3 parts of nitrile rubber, 26-34 parts of fiber materials, 9-11 parts of artificial graphite, 5-7 parts of calcined petroleum coke, 4-6 parts of natural graphite, 2-3 parts of molybdenum disulfide, 4-6 parts of antimony sulfide, 4-6 parts of zirconium silicate, 1.5-2.5 parts of aluminum oxide, 5.5-18.5 parts of barium sulfate and 4-16 parts of heavy calcium carbonate; the nano materials are composed of amino-modified nano silicon dioxide and double-bond-modified nano silicon dioxide.

2. The phenolic resin-based friction material according to claim 1, It is characterized in that The nano material is composed of the following components in parts by mass: 2 to 3 parts of amino-modified nano silicon dioxide and 1 to 2 parts of double-bond-modified nano silicon dioxide.

3. The phenolic resin-based friction material according to claim 1 or 2, It is characterized in that The fiber material consists of the following components in parts by mass: 3 to 5 parts of carbon fiber, 5 to 7 parts of copper fiber, 9 to 11 parts of steel fiber and 9 to 11 parts of silicate mineral fiber.

4. A method for preparing a phenolic resin-based friction material as claimed in any one of claims 1 to 3, It is characterized in that The following steps are involved: After the components are mixed evenly, they are hot pressed and cured to obtain a phenolic resin-based friction material.

5. The method for preparing a phenolic resin-based friction material according to claim 4, It is characterized in that The temperature of hot pressing is 170~200℃ and the pressure is 280~360kg / cm 2 , time is 5 to 8 minutes.

6. The method for preparing a phenolic resin-based friction material according to claim 4 or 5, It is characterized in that The curing method is as follows: the hot-pressed material is heated from room temperature to 138-142°C and kept warm for 1.8-2.2 hours, then heated to 158-162°C and kept warm for 1.8-2.2 hours, then heated to 178-182°C and kept warm for 1.8-2.2 hours, and finally heated to 208-212°C and kept warm for 3.8-4.2 hours.

7. The method for preparing a phenolic resin-based friction material according to claim 6, It is characterized in that The time required to heat from room temperature to 138-142°C is 0.8-1.2h.

8. Use of the phenolic resin-based friction material as claimed in any one of claims 1 to 3 as a brake material.

Citation Information

Patent Citations

  • Low-resin-based aramid pulp wear-resistant disc brake pad and preparation method thereof

    CN113124076A

  • Nano-modified phenolic resin-based composite material as well as preparation method and application thereof

    CN117511120A

Cited By

  • Copper-free ceramic brake pad beneficial to electrostatic spraying and preparation method of copper-free ceramic brake pad

    CN120794424A

  • Resin-based friction plate for aluminum ceramic brake disc and preparation method of resin-based friction plate

    CN121086447A

  • Phenolic resin-based friction material as well as preparation method and application thereof

    CN121948870A