Composition as well as preparation method and application thereof
By using a combination of polyisocyanates, specific polymers, polyols, silane compounds and water-soluble chelating agents in the aqueous polyurethane polyurea dispersion, the problem of easy hydrolysis of the aqueous polyurethane polyurea dispersion under environmental conditions is solved, and the problem of water-based polyurethane polyurea dispersion is improved. Hydrolysis resistance and thermal stability, suitable for coatings, adhesives and inks.
Patent Information
- Application Number
- CN202310573633.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-19
- Publication Date
- 2024-11-22
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Water-based polyurethane polyurea dispersion is easily hydrolyzed when stored under environmental conditions, resulting in a degradation of its application performance, affecting the adhesion, dirt resistance, scratch resistance, impact resistance, sealant and adhesive coating of coating properties, heat resistance and hydrolysis resistance.
The aqueous polyurethane polyurea dispersion is prepared by specific reaction and treatment methods using a composition containing polyisocyanates, polymers, polyols, silane compounds, hydrophilic compounds and water-soluble chelating agents that meet specific structures, thereby increasing its hydrolysis resistance. and thermal stability and reduce viscosity.
It improves the low-temperature performance, hydrolysis resistance, and hydrolysis resistance of the aqueous polyurethane polyurea dispersion after heat storage, taking into account low viscosity and is suitable for industrial production.
Smart Images

Figure CN118995018A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a composition, the preparation and application of the composition, in particular to the application in the field of coatings, adhesives or inks, and articles prepared, coated, bonded, sealed or printed using the composition. Background Art
[0002] Waterborne polyurethane polyurea dispersions can be widely used in the fields of coatings, adhesives, sealants and printing inks. Compared with traditional solvent-based polyurethanes, it has the advantages of being environmentally friendly, non-flammable and non-explosive, safe to store and having a high solid content. However, compared with solvent-based polyurethanes, waterborne polyurethane polyurea dispersions contain excess water by definition, which can hydrolyze the hydrolyzable groups when stored under ambient conditions. At the same time, the metal ions present in the system (such as metal ions introduced in the catalyst used for the synthesis of polyurethane or precursors) will also promote the hydrolysis of the hydrolyzable groups on the waterborne polyurethane polyurea dispersion, thereby reducing its application performance. Specifically, in the field of coating products, it will affect the adhesion, dirt resistance, scratch resistance, impact resistance, elongation at break and water washability of the coating, and in the field of sealant and adhesive products, it will affect the brushability, heat resistance and hydrolysis resistance of the sealant and adhesive.
[0003] Patents such as DE 19954500, DE 4410557 or EP 792908 propose to introduce carboxylate into polyurethane polyurea dispersion and then compound it with carbodiimide to improve the adhesive property, wherein the carboxylate is obtained by adding dimethylol propionic acid into polyurethane polyurea. The above-mentioned reactive carboxyl group has low reactivity with carbodiimide.
[0004] CN 108250390 B describes that a self-crosslinkable aqueous polyurethane dispersion is obtained by adding a non-hindered bifunctional silane and introducing a terminal polyethoxy chain segment as a hydrophilic agent.
[0005] CN 109081897 A describes that a self-crosslinkable aqueous polyurethane dispersion is obtained by adding non-sterically hindered difunctional, monofunctional or bifunctional silane and introducing a terminal polyethoxy chain segment as a hydrophilic agent.
[0006] CN 113136160 A describes that a water-soluble chelating agent is added to form a stable compound by complexing with metal ions in the system so that the compound no longer promotes the hydrolysis of polyurethane; the water resistance and heat resistance of waterborne polyurethane are increased by introducing a non-sterically hindered bifunctional silane (KH792); and a small amount of monofunctional polyether with hydrophilic end groups is added to replace part of the hydrophilic groups of sulfonates to reduce the content of sulfonate groups, thereby preparing a waterborne polyurethane adhesive with excellent stability.
[0007] EP 3026071 A1 describes a process for preparing aqueous polyurethane dispersions which are obtained from a mixture comprising at least one readily crystallizable polyester polyol and at least one polyether polyol, the polyether polyol being a polyalkylene glycol homopolymer or copolymer containing ethylene oxide units.
[0008] WO 2016135162 A1 describes a method for preparing an aqueous peptide-functionalized polyurethane dispersion (PUD) that can be used as an adhesive, especially for metal surfaces, wherein the dispersion is made by reacting a maleimide-terminated polyurethane prepolymer with one or more peptides. The amino acid side chains in the peptide and the maleimide groups undergo a coupling reaction, and the adsorption properties of the peptide are utilized to improve its adsorption quality on the substrate surface. The reaction mixture contains at least a polyether polyol and a polyester polyol, the polyether polyol can be a polyalkylene glycol homopolymer or copolymer, and the polyester polyol can be a crystalline / semi-crystalline polyol.
[0009] US 10640702 BB describes a method for preparing and using coated particles for use as proppants in hydraulic fracturing to optimize capital costs and equipment costs and improve production efficiency. The coated particles are composed of substrate particles with a particle size not exceeding 3 mesh and a coating comprising a crystalline or semi-crystalline polyester / polyurethane having a decrystallization temperature of at least 35°C and modified by aminosilane. The crystalline or semi-crystalline polyester / polyurethane may contain a monofunctional or difunctional polyether polyol polymerized by ethylene oxide or copolymerized by ethylene oxide and propylene oxide.
[0010] WO 2018 / 158278 A1 describes an aqueous polyurethane polyurea dispersion comprising a soluble chelating agent salt. Summary of the invention
[0011] The object of the present invention is to provide a composition, the preparation and application of the composition, especially the application in the field of coatings, adhesives or inks, and the products prepared, coated, bonded, sealed or printed using the composition.
[0012] The composition according to the present invention comprises:
[0013] (a) a polyurethane polyurea polymer, wherein the polyurethane polyurea polymer is obtained by reacting a system comprising the following components:
[0014] (a1) a polyisocyanate;
[0015] (a2) a polymer conforming to formula I:
[0016]
[0017] Where n is 10-75, R1 is an alkyl group containing 1 to 10 carbon atoms, and R2 is a structure containing at least two isocyanate-reactive groups;
[0018] (a3) a polyol different from component a2), said polyol having a hydroxyl functionality of 1.5 to 4;
[0019] (a4) a silane compound comprising an isocyanate-reactive group and at least two methoxy and / or ethoxy groups attached to a silicon atom;
[0020] (a5) a hydrophilic compound different from (a2) containing 2 to 3 isocyanate-reactive groups; and
[0021] (a6) optionally a compound containing 1 to 3 amino groups and / or hydroxyl groups;
[0022] The amount of the polymer conforming to the structure of formula I is 0.7 wt%-9 wt%, and the amount of the silane compound is 0.14 wt%-0.6 wt%, relative to the total weight of the polyurethane polyurea polymer;
[0023] (b) at least one water-soluble chelating agent selected from ethylenediaminetetraacetate, tartrate, citrate, pyrophosphate, tripolyphosphate, hexametaphosphate, gluconate and / or a mixture of at least two thereof; and
[0024] (c) Water.
[0025] According to one aspect of the present invention, a method for preparing the composition provided by the present invention is provided, comprising the following steps: mixing the polyurethane polyurea polymer (a) or the components for preparing the polyurethane polyurea polymer, a chelating agent (b) and water (c) in any manner.
[0026] According to another aspect of the present invention, a coating, an adhesive or an ink comprising the composition provided by the present invention is provided.
[0027] According to another aspect of the present invention, there is provided use of the composition provided by the present invention for preparing a coating product, a bonding product or a printing product.
[0028] According to another aspect of the present invention, there is provided an article containing a substrate prepared, coated, bonded, sealed or printed according to the composition provided by the present invention.
[0029] The methoxy and / or ethoxy silane in the polyurethane polyurea in the composition of the present invention can undergo hydrolysis and subsequent condensation, so that the composition has good hydrolysis resistance; the side group soft segment generated by the polymer conforming to the structure of formula I of the polyurethane polyurea is more inclined to separate from the polyurethane hard segment, so that the polyurethane soft segment is softer and more active, thereby hindering the close arrangement of molecules, reducing the chance of mutual entanglement of its macromolecular groups, making it difficult to form a polymer cluster structure, so that the composition has good low-temperature stability; the chelating agent salt in the composition of the present invention can reduce the double electric layer force between particles, thereby greatly reducing the viscosity of the composition.
[0030] Therefore, the composition of the present invention has excellent low-temperature performance, good hydrolysis resistance and hydrolysis resistance after heat storage, and can also take into account low viscosity and is easy for industrial production. DETAILED DESCRIPTION
[0031] The present invention provides a composition comprising:
[0032] (a) a polyurethane polyurea polymer, wherein the polyurethane polyurea polymer is obtained by reacting a system comprising the following components:
[0033] (a1) a polyisocyanate;
[0034] (a2) a polymer conforming to formula I:
[0035]
[0036] Where n is 10-75, R 1 is an alkyl group containing 1 to 10 carbon atoms, and R2 is a structure containing at least two isocyanate-reactive groups;
[0037] (a3) a polyol different from component a2), said polyol having a hydroxyl functionality of 1.5 to 4;
[0038] (a4) a silane compound comprising an isocyanate-reactive group and at least two methoxy and / or ethoxy groups attached to a silicon atom;
[0039] (a5) a hydrophilic compound different from (a2) containing 2 to 3 isocyanate-reactive groups; and
[0040] (a6) optionally a compound containing 1 to 3 amino groups and / or hydroxyl groups;
[0041] The amount of the polymer conforming to the structure of formula I is 0.7 wt%-9 wt%, and the amount of the silane compound is 0.14 wt%-0.6 wt%, relative to the total weight of the polyurethane polyurea polymer;
[0042] (b) at least one water-soluble chelating agent selected from ethylenediaminetetraacetate, tartrate, citrate, pyrophosphate, tripolyphosphate, hexametaphosphate, gluconate and / or a mixture of at least two thereof; and
[0043] (c) Water.
[0044] The invention also provides the preparation and application of the composition, especially the application in the field of coatings, adhesives or inks, and products obtained by coating, bonding, sealing or printing with the composition.
[0045] The term "solidification" as used herein refers to the process in which a liquid substance changes from a liquid state to a solid state under normal temperature conditions.
[0046] The term "coating" as used herein refers to a substance that can be coated on the surface of an object using different construction techniques to form a solid coating that is firmly adhered, has a certain strength, and is continuous.
[0047] The term "adhesive" used in this article refers to a chemical substance that can be coated on the surface of an object using different construction techniques to form a coating on the object itself or on the surface of one object to another object, and to bond the object itself or on the surface of one object to another object. It is also used as a synonym for adhesive and / or sealant and / or bonding agent.
[0048] As used herein, the term "polyurethane polyurea" refers to polyurethane and / or polyurethane urea and / or polyurea.
[0049] As used herein, the term "aqueous polyurethane polyurea dispersion" refers to an aqueous polyurethane dispersion and / or an aqueous polyurethane urea dispersion and / or an aqueous polyurea dispersion.
[0050] The content of polyurethane polyurea in the aqueous polyurethane polyurea dispersion described herein is equivalent to the solid component content of the aqueous polyurethane polyurea dispersion.
[0051] The term "solid component" used herein refers to a solid fraction or an effective component.
[0052] The term "isocyanate-reactive compound" as used herein refers to a component containing a group reactive toward an isocyanate group, i.e., a component containing a group having a Zerevitinov-active hydrogen, the definition of which is given in Rompp's Chemical Dictionary (Rommp Chemie Lexikon), 10th ed., Georg Thieme Verlag Stuttgart, 1996. Generally, a group having a Zerevitinov-active hydrogen is understood in the art to mean a hydroxyl group (OH), an amino group (NH x ) and thiol group (SH).
[0053] The term "isocyanate-reactive group" as used herein refers to a group reactive toward an isocyanate group, i.e., a group containing a Zerevitinov-active hydrogen, the definition of which is given in Rompp's Chemical Dictionary (Rommp Chemie Lexikon), 10th ed., Georg Thieme Verlag Stuttgart, 1996. Generally, a group containing a Zerevitinov-active hydrogen is understood in the art to refer to a hydroxyl group (OH), an amino group (NH x ) and thiol group (SH).
[0054] Component a) Polyurethane polyurea polymer
[0055] Component a1) Polyisocyanate
[0056] The isocyanate functionality of the polyisocyanate is preferably not less than 2, more preferably 2-4, most preferably 2.
[0057] The polyisocyanate of component a1) preferably has at least two isocyanate groups, more preferably one or more of the following: aliphatic polyisocyanates, cycloaliphatic polyisocyanates, aromatic polyisocyanates, araliphatic polyisocyanates, and their derivatives having iminooxadiazinedione, isocyanurate, uretdione, carbamate, allophanate, biuret, urea, oxadiazinetriae, oxazolidinone, acylurea and / or carbodiimide groups.
[0058] The polyisocyanate of component a1) is further preferably an isocyanate conforming to the following general formula: Y(NCO)2, wherein Y is selected from: a divalent aliphatic hydrocarbon group containing 4 to 12 carbon atoms, a divalent alicyclic hydrocarbon group containing 6 to 15 carbon atoms, a divalent aromatic hydrocarbon group containing 6 to 15 carbon atoms or a divalent aromatic aliphatic hydrocarbon group containing 7 to 15 carbon atoms.
[0059] The polyisocyanate of component a1) is also preferably one or more of the following: tetramethylene diisocyanate, pentamethylene diisocyanate, hexamethylene diisocyanate, dodecamethylene diisocyanate, 1,4-cyclohexane diisocyanate, isophorone diisocyanate, 4,4′-dicyclohexylmethane diisocyanate, 4,4′-dicyclohexylpropane diisocyanate, 1,4-phenylene diisocyanate, 2,4-toluene diisocyanate, 2,6-toluene diisocyanate, 4,4′-diphenylmethane diisocyanate, 2,2′- and 2,4′-diphenylmethane diisocyanate, tetramethylxylyl diisocyanate and p-xylylene diisocyanate.
[0060] The polyisocyanate of component a1) is preferably selected from the group consisting of hexamethylene diisocyanate, isophorone diisocyanate, a mixture of hexamethylene diisocyanate and isophorone diisocyanate, or a mixture of hexamethylene diisocyanate and 4,4′-dicyclohexylmethane diisocyanate.
[0061] The polyisocyanate of component a1) is most preferably a mixture of hexamethylene diisocyanate and isophorone diisocyanate, or a mixture of hexamethylene diisocyanate and 4,4'-dicyclohexylmethane diisocyanate.
[0062] The amount of the component a1) is preferably 5% to 40% by weight, most preferably 8% to 20% by weight, relative to the total weight of the polyurethane polyurea polymer.
[0063] Component a2) a polymer conforming to formula I
[0064] In the formula I, n is 10-75, which may be an integer or not, preferably 10-40, more preferably 10-30.
[0065] The at least two isocyanate-reactive groups of R2 are preferably selected from at least two amino groups, at least two hydroxyl groups, or at least one amino group and at least one hydroxyl group.
[0066] The polymer conforming to the structure of formula I is preferably one or more of the following: a polymer conforming to the structure of formula II and a polymer conforming to the structure of formula III,
[0067]
[0068] Wherein, in formula II, a is 10-75, which may be an integer or not, and b is 0-50, which may be an integer or not; in formula III, x is 10-75, which may be an integer or not, and y is 1-50, which may be an integer or not.
[0069] The number average molecular weight of the polymer of component a2) conforming to the structure of formula I is preferably 500 g / mol-4000 g / mol, most preferably 600 g / mol-1500 g / mol, and the number average molecular weight is tested according to gel chromatography, using tetrahydrofuran as the mobile phase, and the molecular weight is calculated based on polystyrene as the standard, and components with a molecular weight of 200 or more are selected for calculation and measured with a differential refractometer.
[0070] The functionality of the polymer of component a2) conforming to formula I is preferably 2.
[0071] The amount of the component a2) polymer conforming to the structure of formula I is preferably 0.7 wt% to 9 wt%, most preferably 0.7 wt% to 4 wt%, relative to the total weight of the waterborne polyurethane polyurea polymer.
[0072] Component a3) is a polyol different from component a2)
[0073] The polyol of component a3) which is different from component a2) is preferably one or more of the following: diols with a number average molecular weight of 62-15000 and polyols with a number average molecular weight of 62-15000, further preferably one or more of the following: diols with a number average molecular weight of 62-5000 and triols with a number average molecular weight of 92-5000, most preferably one or more of the following: polyester polyols with a number average molecular weight of 500-2500 containing 1.5-3 hydroxyl groups, 2500 polycarbonate polyol containing 1.5-3 hydroxyl groups, number average molecular weight of 200-2500 polyether polyol containing 1.5-3 hydroxyl groups, number average molecular weight of 250-2500 polylactone polyol containing 1.5-3 hydroxyl groups and small molecule alcohol, the number average molecular weight is tested according to gel chromatography, tetrahydrofuran is used as the mobile phase, and the molecular weight is calculated based on polystyrene as the standard, and components with a molecular weight of 200 or higher are selected for calculation and measured with a differential refractometer.
[0074] The polyether polyol having a number average molecular weight of 200-2500 and containing 1.5-3 hydroxyl groups is preferably a polytetrahydrofuran polyol having a number average molecular weight of 200-2500 and containing 1.5-3 hydroxyl groups.
[0075] The melting enthalpy of the polyol of component a3) which is different from component a2) is preferably not less than 15 J / g, further preferably 25 J / g-100 J / g, most preferably 40 J / g-80 J / g, obtained by the first temperature increase curve of DSC from 20°C to 100°C according to method A in DIN 65467, with a sample load of 10-20 mg and a heating rate of 20 K / min.
[0076] The amount of component a3) is preferably 5% to 94% by weight, most preferably 70% to 90% by weight, relative to the total weight of the composition.
[0077] Component a4) Silane compound
[0078] The component a4) is a silane compound containing one isocyanate-reactive group and at least two methoxy and / or ethoxy groups attached to a silicon atom; the isocyanate-reactive group is preferably a primary or secondary amino group.
[0079] The component a4) silane compound is preferably one or more of the following: bis(3-triethoxysilylpropyl)amine, bis(3-trimethoxysilylpropyl)amine, (3-aminopropyl)trimethoxysilane, (3-aminopropyl)triethoxysilane, 3-aminopropyl(diethoxy)methylsilane and 3-aminopropylmethyldimethoxysilane; more preferably one or more of the following: bis(3-triethoxysilylpropyl)amine, bis(3-trimethoxysilylpropyl)amine, (3-aminopropyl)trimethoxysilane, (3-aminopropyl)triethoxysilane, 3-aminopropyl(diethoxy)methylsilane and 3-aminopropylmethyldimethoxysilane.
[0080] Furthermore, the corresponding aspartic acid esters (Formula IV) which can be synthesized from the abovementioned amino-functional silanes and esters of unsaturated dicarboxylic acids, such as maleic acid, can be used.
[0081]
[0082] wherein X is the same or different and is methoxy, ethoxy, methyl or ethyl, provided that at least two groups are methoxy and / or ethoxy; wherein Q is alkyl, preferably n-propyl, and Z is alkoxy, preferably methoxy or ethoxy.
[0083] Further preferred compounds are diethyl N-(3-triethoxysilylpropyl)aspartate, diethyl N-(3-trimethoxysilylpropyl)aspartate and diethyl N-(3-dimethoxymethylsilylpropyl)aspartate.
[0084] The component a4) is most preferably one or more of the following: (3-aminopropyl)trimethoxysilane, (3-aminopropyl)triethoxysilane and 3-aminopropylmethyldimethoxysilane.
[0085] The amount of the component a4) silane compound is preferably 0.14% to 0.6% by weight, most preferably 0.18% to 0.4% by weight, relative to the total weight of the composition.
[0086] Component a5) a hydrophilic compound containing 2 to 3 isocyanate-reactive groups
[0087] The hydrophilic group of the hydrophilic compound preferably comprises one or more of the following: an ionic group, a potentially ionic group and a non-ionic group.
[0088] The hydrophilic compound containing 2 to 3 isocyanate-reactive groups of component a5) is preferably one or more of the following: N-(2-aminoethyl)-2-aminoethane sulfonate, dimethylol propionate and (N-(2-aminoethyl)-2-aminoethane carboxylate.
[0089] The amount of component a5) is preferably 0.2% to 50% by weight, most preferably 1% to 5% by weight, relative to the total weight of the composition.
[0090] Component a6) Compounds containing 1 to 3 amino and / or hydroxyl groups
[0091] The component a6) compound containing 1 to 3 amino groups and / or hydroxyl groups may contain 1 to 3 amino groups or 1 to 3 hydroxyl groups or a combination of amino groups and hydroxyl groups.
[0092] The compound containing 1 to 3 amino groups and / or hydroxyl groups of component a6) preferably contains at least one amino group; further preferably one or more of the following: aliphatic monoamines, alicyclic monoamines, aliphatic primary and / or secondary diamines, hydrazides, aliphatic primary and / or secondary triamines, aliphatic primary and / or secondary amino alcohols, alicyclic primary and / or secondary diamines, alicyclic primary and / or secondary triamines, alicyclic primary and / or secondary amino alcohols; most preferably one or more of the following: isophoronediamine, N-(2-hydroxyethyl)ethylenediamine and diethanolamine.
[0093] The amount of component a6) is preferably not more than 10% by weight, most preferably from 0.5% to 3% by weight, relative to the total weight of the composition.
[0094] Component b) Chelating agent
[0095] The component b) chelating agent is preferably one or more of the following: ethylenediaminetetraacetate, tartrate, citrate, pyrophosphate, tripolyphosphate, hexametaphosphate and gluconate.
[0096] The amount of component b) is preferably 0.05% to 0.5% by weight, most preferably 0.1% to 0.2% by weight, relative to the total weight of the composition.
[0097] Preferably, the chelating agent b) is characterized in that its concentration is 4.3×10 -7 The pH value of the aqueous solution of 1 mol / g at a temperature of 23°C is in the range of 3-11, preferably in the range of 4-10, and most preferably in the range of 5-8.
[0098] Preparation method of composition
[0099] Preferably, the polyurethane polyurea polymer (a) and water (c) form an aqueous polyurethane polyurea dispersion, and then the chelating agent (b) is introduced to obtain the composition.
[0100] The chelating agent can be added in the form of a solid or an aqueous solution, preferably in the form of an aqueous solution of the chelating agent, which is more conducive to the dispersion of the chelating agent.
[0101] The water-soluble salt of the chelating agent can be added directly or formed in the composition by acid-base neutralization. The acid-base neutralization can be complete or incomplete neutralization, preferably complete neutralization.
[0102] The chelating agent can be added during the chain extension or neutralization process of preparing the polyurethane polyurea polymer, or after the chain extension, or during or after the polyurethane polymer is dispersed in water, or during or after the distillation of the polyurethane polymer.
[0103] The acid can be a free acid that can react with the base to form a chelating agent water-soluble salt. The free acid is preferably one or more of the following: aminocarboxylic acid, hydroxycarboxylic acid, inorganic polyphosphoric acid, hydroxyaminocarboxylic acid, organic polyphosphonic acid and polycarboxylic acid.
[0104] The aminocarboxylic acid is preferably one or more of the following: ethylenediaminetetraacetic acid and aminotriacetic acid.
[0105] The hydroxycarboxylic acid is preferably one or more of the following: tartaric acid, citric acid and gluconic acid.
[0106] The inorganic polyphosphoric acid is preferably one or more of the following: tripolyphosphoric acid, hexametaphosphoric acid and pyrophosphoric acid.
[0107] The hydroxyaminocarboxylic acid is preferably one or more of the following: hydroxyethylethylenediaminetriacetic acid and dihydroxyethylglycine.
[0108] The water in the composition can be introduced before the polyurethane polyurea polymer is formed, can be introduced during the polyurethane polyurea polymer formation process, or can be introduced after the polyurethane polyurea polymer is formed. The water is preferably introduced after the polyurethane polyurea polymer is formed.
[0109] The water and polyurethane polyurea polymer are mixed to form an aqueous polyurethane polyurea dispersion.
[0110] The amount of the organic solvent in the aqueous polyurethane polyurea dispersion is preferably less than 1% by weight relative to the total weight of the aqueous polyurethane polyurea dispersion.
[0111] The solid content of the aqueous polyurethane polyurea dispersion is preferably 15 wt %-70 wt %, further preferably 30 wt %-60 wt %, and most preferably 45 wt %-55 wt %, relative to the total weight of the aqueous polyurethane polyurea dispersion. The solid content is measured using a HS153 moisture meter from Mettler Toledo according to DIN-EN ISO3251:2019, with a heating temperature of 120° C., and the test endpoint is determined when the sample weight loss is less than 1 mg / 140 seconds.
[0112] The pH value of the aqueous polyurethane polyurea dispersion is preferably 4-11, most preferably 5-10, and the pH value is measured at 23° C. using a PB-10 pH meter from Sartorius, Germany.
[0113] The average particle size of the aqueous polyurethane polyurea dispersion is preferably 20 nm to 750 nm, more preferably 50 nm to 450 nm, and most preferably 100 nm to 250 nm. The average particle size is measured by laser correlation (laser particle size analyzer) using a ZEN 1600 tester from Malvern, UK. 13321:1996 Test method: Add 1 drop (about 0.05g) of sample to 50ml of ultrapure water, and test the diluted sample at 23.0±0.1℃; Material: polystyrene latex (RI: 1.590; Absorbance: 0.010), Dispersant: Water (Temperature: 23.0℃; Viscosity: 0.9308cP; RI: 0.330), Equilibration time: 60 seconds, Use disposable colorimetric cup DTS0012, Positioning method: Automatic attenuation selection, Find the best position: Yes, Analysis model: General (normal resolution), Measurement angle: 173° backscattering (NIBS default), Number of runs: 3 times, Run duration: 10 seconds, Number of measurements: 10 times.
[0114] The viscosity of the aqueous polyurethane polyurea dispersion is preferably 300 mPa·s-6000 mPa·s, and the viscosity is measured at 23° C. using a DV-II+Pro. rotational viscometer from Brookfield according to ISO 2555:2018, rotor type: s62-64, rotation speed: 30 RPM, and test temperature: 23° C.
[0115] The aqueous polyurethane polyurea dispersion can be prepared using methods commonly used in the art, such as emulsification dispersion, prepolymer mixing, acetone method, melt emulsification, ketimine solid phase dispersion, and related derivative methods. The above methods are summarized in Methoden der Organischen Chemie (Houben-Weyl, sup. 4th edition, volume E20 / Part 2, page 1682, Georg Thieme Verlag, Stuttgart, 1987). Among them, melt emulsification and acetone methods are better choices, and acetone method is most preferred.
[0116] Preferably, the method for preparing the aqueous polyurethane polyurea dispersion comprises the following steps: i. reacting some or all of component a1) a polyisocyanate, component a2) a polymer conforming to the structure of formula I, and component a3) a polyol different from component a2) to obtain a prepolymer;
[0117] ii. reacting the prepolymer, component a4) a silane compound, component a5) a hydrophilic compound containing 2 to 3 isocyanate-reactive groups, and optionally component a6) a compound containing 1 to 3 amino groups and / or hydroxyl groups to obtain the polyurethane polyurea;
[0118] iii. before, during or after step ii, component c) is introduced into a water dispersion; in a preferred embodiment, component c) water is slowly added while stirring, and the reaction is allowed to proceed at 20 to 60°C, preferably 40 to 60°C, most preferably 40 to 55°C, and stirred for 10-30 minutes; and
[0119] iv. Adding component b) a chelating agent to obtain the aqueous polyurethane polyurea dispersion.
[0120] In the step i, components a2) and a3) are preferably added to a reactor and heated to 30-80° C., preferably 50-70° C., under stirring. When the water content of the mixture in step i is less than 0.5%, preferably less than 0.2% (calculated by weight added to the reactor), component a1) is added under stirring and an exothermic reaction is allowed to proceed at 50-140° C., preferably 60-110° C., most preferably 80-90° C., until the theoretically calculated reaction endpoint is reached.
[0121] In the step ii, component a5) and optional component a6) are preferably dissolved in water, and component a4) is dissolved in acetone, and added to the prepolymer respectively while stirring, and an exothermic reaction is allowed to proceed at 20-60°C, preferably 40-60°C, most preferably 40-55°C, for 30 minutes to obtain polyurethane polyurea.
[0122] The step iv is preferably performed by slowly adding component b) at 20-40°C, preferably 20-30°C, while stirring.
[0123] The preparation method may further comprise a step v. introducing an organic solvent miscible with water but inert to isocyanate groups during or after step i, and removing the organic solvent from the aqueous polyurethane polyurea dispersion.
[0124] The organic solvent is preferably a solvent that is miscible with water but inert to isocyanate groups, and is further preferably one or more of the following: acetone, butanone, propylene glycol dimethyl ether, other ethers not containing hydroxyl functional groups, and esters not containing hydroxyl functional groups; most preferably one or more of the following: acetone and butanone.
[0125] The organic solvent preferably does not contain N-methyl or N-ethyl pyrrolidone compounds.
[0126] The organic solvent is preferably partially or completely removed by distillation, the distillation temperature is preferably 10° C. to 100° C., and the distillation time is preferably 1 hour to 12 hours.
[0127] The distillation temperature is most preferably 25°C-60°C.
[0128] The distillation time is most preferably 2 hours to 7 hours.
[0129] The distillation pressure is preferably 500 mbar-50 mbar, most preferably 200 mbar-60 mbar.
[0130] In order to accelerate the reaction rate of step i, a catalyst commonly used in the preparation of prepolymers can be used, such as triethylamine, 1,4-diazabicyclo-[2,2,2]-octane, bismuth salts of sebacic acid or neodecanoic acid, tin dioctoate, tin (II) chloride or dibutyltin dilaurate, most preferably tin (II) chloride and bismuth neodecanoate.
[0131] The catalyst can be placed in the reactor simultaneously with the components in step i, or can be added afterwards.
[0132] The degree of conversion of the components of step i can be obtained by measuring the NCO content in the components. To this end, the sample can be simultaneously subjected to spectral measurement, such as infrared or near-infrared spectroscopy, and refractive index measurement or chemical analysis, such as titration.
[0133] The prepolymer may be in a solid state or a liquid state at room temperature.
[0134] The component a1) polyisocyanate and the component a2) polymer conforming to the structure of formula I can be added at one time or in multiple times, and can be the same components or different components as those added previously.
[0135] The organic solvent present in the polyurethane polymer can be removed by distillation. The organic solvent can be removed during the formation of the polyurethane polymer or after the polyurethane polymer is formed.
[0136] Coatings, adhesives or inks
[0137] The coating, adhesive or ink preferably further comprises an additive. The additive is preferably one or more of the following: emulsifier, light stabilizer, antioxidant, bactericide, filler, anti-settling agent, defoamer, wetting agent, flow regulator, reactive diluent, plasticizer, neutralizer, catalyst, auxiliary solvent, thickener, pigment, dye, matting agent and tackifier. The additive can be added during and / or after the production of the polyurethane polyurea dispersion.
[0138] The selection of the additives and the dosage used are known in principle to the person skilled in the art and can be easily determined.
[0139] The aqueous polyurethane polyurea dispersions of the invention can also be mixed and used together with other aqueous or solvent-containing oligomers or polymers, such as aqueous or solvent-containing polyesters, polyurethanes, polyurethane-polyacrylates, polyacrylates, polyethers, polyester-polyacrylates, alkyd resins, addition polymers, polyamides / imides or polyepoxides. The compatibility of such mixtures must be tested in each case using simple preliminary tests.
[0140] The aqueous polyurethane polyurea dispersion of the present invention may also be mixed with other compounds containing functional groups such as carboxyl groups, hydroxyl groups and / or blocked isocyanate groups and used together.
[0141] The coating, adhesive or ink of the present invention is obtained by processing according to methods known to those skilled in the art.
[0142] Coated products, bonded products or printed products
[0143] The substrate is preferably one or more of the following: wood, metal, glass, fiber, textile, artificial leather, genuine leather, paper, plastic, rubber, foam, ceramic and various polymer coatings, most preferably one or more of the following: textile, plastic, ceramic, metal, genuine leather, artificial leather and various polymer coatings.
[0144] The coating may be applying the coating, adhesive or ink to the entire surface of the substrate or only to one or more parts of the surface of the substrate.
[0145] The application may be by brushing, dipping, spraying, rolling, knife coating, flow coating, pouring or printing. BRIEF DESCRIPTION OF THE DRAWINGS
[0146] The present invention will be described and explained in more detail below in conjunction with the accompanying drawings, in which:
[0147] Figure 1 It is a schematic diagram of spline bonding.
[0148] Figure 2 It is a schematic diagram of the hydrolysis resistance test of the specimen.
[0149] Figure 3 This is a schematic diagram of dry film cracking and non-cracking in low-temperature film-forming test.
[0150] Example
[0151] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by those skilled in the art to which the invention belongs. When the definition of a term in this specification conflicts with the meaning commonly understood by those skilled in the art to which the invention belongs, the definition described in this article shall prevail.
[0152] Unless otherwise indicated, all numerical values expressing quantities of ingredients, reaction conditions, and so forth used in the specification and claims are to be understood as modified by the term “about.” Accordingly, unless indicated to the contrary, the numerical parameters set forth herein are approximations that can vary depending upon the desired properties desired to be obtained.
[0153] As used herein, "and / or" means one or all of the mentioned elements.
[0154] As used herein, “including” and “comprising” encompasses the case where only the stated elements are present as well as the case where there are other elements other than the stated elements.
[0155] Unless otherwise indicated, "a", "an", "an" and "the" used in this specification are intended to include "at least one" or "one or more". For example, "a component" means one or more components, so more than one component may be considered and may be employed or used in the implementation of the embodiment.
[0156] All percentages in the present invention are by weight, unless otherwise specified.
[0157] The analytical measurements of the present invention were all carried out at 23±2°C unless otherwise stated.
[0158] Test method for solid component content (solid content) of waterborne polyurethane polyurea dispersion: Use Mettler Toledo's HS153 moisture analyzer according to DIN-EN ISO 3251:2019, the heating temperature is 120°C, and the test endpoint is determined when the sample weight loss is less than 1 mg / 140 seconds. Test method for average particle size of waterborne polyurethane polyurea dispersion: measured by laser correlation (laser particle size analyzer) using ZEN 1600 tester of Malvern Company, UK; adding 1 drop (about 0.05 g) of sample to 50 ml of ultrapure water according to ISO13321:1996 test method, and testing the diluted sample at 23.0±0.1°C; material: polystyrene latex (RI: 1.590; absorbance: 0.010), dispersant: water (temperature: 23.0°C; viscosity: 0.9308 cP; RI: 0.330), equilibrium time: 60 seconds, using disposable colorimetric cup DTS0012, positioning method: automatic attenuation selection, finding the best position: yes, analysis model: general (normal resolution), measurement angle: 173° backscattering (NIBS default value), number of runs: 3 times, run duration: 10 seconds, number of measurements: 10 times.
[0159] Test method for pH value of aqueous polyurethane polyurea dispersion: measured at 23°C using a PB-10 pH meter from Sartorius, Germany, according to DIN ISO 976:2016-12.
[0160] Method for determining the pH value of the chelating agent aqueous solution: According to DIN ISO 976:2016-12, the PB-10 pH meter of Sartorius, Germany, was used at 4.3×10 -7 Concentrations in mol / g are measured at 23°C.
[0161] Test method for viscosity of aqueous polyurethane polyurea dispersion: using Brookfield's DV-II+Pro. rotational viscometer, measured at 23°C according to ISO 2555:2018, rotor type: s 62-64, rotation speed: 30RPM, test temperature: 23°C.
[0162] The isocyanate group (NCO) content is determined by volume in accordance with DIN-EN ISO 11909:2007.
[0163] Materials and reagents
[0164] Polyester I: semi-crystalline, difunctional polyester polyol based on adipic acid and 1,4-butanediol, number average molecular weight Mn 2250 g / mol, hydroxyl value 50 mg KOH / g, glass transition temperature -61°C, melting temperature 49°C, melting enthalpy 80 J / g.
[0165] Polyester II: a semicrystalline, difunctional polyester polyol based on adipic acid, 1,6-hexanediol and neopentyl glycol (the molar ratio of 1,6-hexanediol to neopentyl glycol is 3:2), with a number average molecular weight Mn 1700 g / mol, a hydroxyl value of 66 mg KOH / g, a glass transition temperature of -63°C, a melting temperature of 26°C, and a melting enthalpy of 55 J / g.
[0166] Polyether I: Ymer N120, a difunctional polyether containing side chain methoxy polyethylene oxide chains, with a number average molecular weight of 1000 g / mol, available from Perstorp Chemitec AB (SE).
[0167] Polyether II: Ymer N180, a difunctional polyether containing side chain methoxy polyethylene oxide chains, with a number average molecular weight of 600 g / mol, available from Perstorp Chemitec AB (SE).
[0168] Polyether III: MPEG 750, monofunctional polyethoxy ether, number average molecular weight 750 g / mol, available from Shanghai Dongda Chemical Co., Ltd.
[0169] Isocyanate I: H, hexamethylene diisocyanate, available from Covestro AG, Germany.
[0170] Isocyanate II: I, isophorone diisocyanate, can be purchased from Covestro AG, Germany.
[0171] Silane I: PC1200, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane, available from Sysbo Silicone.
[0172] Silane II: PC1210, N-β-(aminoethyl)-γ-aminopropyltriethoxysilane, available from Sysbo Silicone.
[0173] Silane III: PC1130, 3-aminopropylmethyldimethoxysilane, available from Sysbo Silicone.
[0174] Silane IV: PC1100, (3-aminopropyl)triethoxysilane, available from Sysbo Silicone.
[0175] Silane V: PC1110, (3-aminopropyl)trimethoxysilane, available from Sysbo Silicone.
[0176] Lucramul 1820 liquid: emulsifier, fatty alcohol poly (ethylene glycol / propylene glycol) ether, supplied in the form of 15%-20% aqueous solution, available from Levaco GmbH, Germany.
[0177] Tetrasodium ethylenediaminetetraacetate: analytical grade, available from Sinopharm Chemical Reagent Co., Ltd. (pH = 10.4, 4.3 × 10 -7 mol / g aqueous solution)
[0178] Sodium citrate: analytical grade, available from Sinopharm Chemical Reagent Co., Ltd. (pH = 8.0, 4.3 × 10 - 7 mol / g aqueous solution)
[0179] Tetrasodium pyrophosphate: analytical grade, available from Sinopharm Chemical Reagent Co., Ltd. (pH = 9.9, 4.3×10 -7 mol / g aqueous solution)
[0180] Disodium pyrophosphate: analytical grade, available from Sinopharm Chemical Reagent Co., Ltd. (pH = 5.3, 4.3 × 10 -7 mol / g aqueous solution) Sodium salt of N-(2-aminoethyl)-2-aminoethanesulfonic acid: Vestamin A 95, 49% concentration in water, available from Evonik, Germany.
[0181] Diethanolamine: analytical grade specification, available from Sinopharm Chemical Reagent Co., Ltd.
[0182] Hydroxyethylethylenediamine: analytical grade specification, available from Sinopharm Chemical Reagent Co., Ltd.
[0183] Isophorone diamine: analytical grade specification, can be purchased from Sinopharm Chemical Reagent Co., Ltd.
[0184] Borchigel Gel L75N: thickener, clear liquid, 25% concentration, available from Borchers.
[0185] DESMODUR 2802: Aliphatic polycarbodiimide, beige liquid, solid content 40%, Covestro AG, Germany.
[0186] Preparation of composition
[0187] If the raw materials in the following examples are aqueous emulsions or aqueous solutions, the weights include water.
[0188] Composition 1
[0189] 548.4 g of polyester I and 5 g of polyether I were dehydrated at 110° C. and 80 mbar for 1 hour, and 2.3 g of 1,4-butanediol was added and cooled while stirring. 56.65 g of isocyanate I and 7.51 g of isocyanate II were added at 60° C. and stirred at 80-90° C. until an isocyanate content of 1.3% was reached. Then, the mixture was dissolved in 930 g of acetone and cooled to 50° C. to obtain a reaction solution. 11.5 g of sodium salt of N-(2-aminoethyl)-2-aminoethanesulfonic acid, 1.14 g of isophoronediamine, a solution formed by dissolving 2.0 g of hydroxyethylethylenediamine in 50 g of water, and a solution formed by dissolving 2.17 g of silane IV in 21.7 g of acetone were added to the acetone solution in which the prepolymer was dissolved and stirred vigorously. The mixture was stirred for 30 minutes and then dispersed by adding 570 g of water. Acetone was separated by distillation for 3.5 hours. After the acetone content was less than 1.0 wt %, 40 g of Lucramul 1820 liquid and 12.5 g of a 5% aqueous solution of sodium citrate were added respectively to obtain a composition having a solid component content of 50.6 wt % and an average particle size of 162 nm in the dispersed phase, a pH of 6.7, and a viscosity of 318 mPa·s.
[0190] Composition 2
[0191] 548.4 g of polyester I and 5 g of polyether I were dehydrated at 110° C. and 80 mbar for 1 hour, and 2.3 g of 1,4-butanediol was added and cooled while stirring. 56.65 g of isocyanate I and 7.51 g of isocyanate II were added at 60° C. and stirred at 80-90° C. until an isocyanate content of 1.3% was reached. Then, it was dissolved in 930 g of acetone and cooled to 50° C. to obtain a reaction solution. 11.5 g of sodium salt of N-(2-aminoethyl)-2-aminoethanesulfonic acid, 1.14 g of isophoronediamine, a solution formed by dissolving 2.0 g of hydroxyethylethylenediamine in 50 g of water, and a solution formed by dissolving 1.60 g of silane III in 16.0 g of acetone were added to the acetone solution in which the prepolymer was dissolved and stirred vigorously. Stirred for 30 minutes, and then the mixture was dispersed by adding 570 g of water. Acetone was separated by distillation for 3.5 hours. After the acetone content was less than 1.0 wt %, 40 g of Lucramul 1820 liquid and 12.5 g of a 5% aqueous solution of tetrasodium ethylenediaminetetraacetate were added respectively to obtain a composition having a solid component content of 50.3 wt % and an average particle size of 162 nm in the dispersed phase, a pH value of 6.7, and a viscosity of 416 mPa·s.
[0192] Composition 3
[0193] 534.4 g of polyester I and 12.5 g of polyether I were dehydrated at 110° C. and 80 mbar for 1 hour, and 2.3 g of 1,4-butanediol was added and cooled while stirring. 56.38 g of isocyanate I and 7.9 g of isocyanate II were added at 60° C. and stirred at 80-90° C. until an isocyanate content of 1.3% was reached. Then, the mixture was dissolved in 930 g of acetone and cooled to 50° C. to obtain a reaction solution. 11.6 g of sodium salt of N-(2-aminoethyl)-2-aminoethanesulfonic acid, a solution formed by dissolving 1.9 g of hydroxyethylethylenediamine in 50 g of water, and a solution formed by dissolving 1.25 g of silane V in 12.5 g of acetone were added to the acetone solution containing the prepolymer and stirred vigorously. Stirred for 30 min, and then the mixture was dispersed by adding 570 g of water. Acetone was separated by distillation for 5 hours. After the acetone content was less than 1.0 wt %, 40 g of Lucramul 1820 liquid and 12.5 g of a 5% aqueous solution of tetrasodium pyrophosphate were added respectively to obtain a composition having a solid component content of 50 wt % and an average particle size of 163 nm in the dispersed phase, a pH of 6.7, and a viscosity of 1218 mPa·s.
[0194] Composition 4
[0195] 503.4 g of polyester I and 25 g of polyether I were dehydrated at 110° C. and 80 mbar for 1 hour, and 2.3 g of 1,4-butanediol was added and cooled while stirring. 60.62 g of isocyanate I and 8.04 g of isocyanate II were added at 60° C. and stirred at 80-90° C. until an isocyanate content of 1.7% was reached. Then, the mixture was dissolved in 930 g of acetone and cooled to 50° C. to obtain a reaction solution. 12.0 g of sodium salt of N-(2-aminoethyl)-2-aminoethanesulfonic acid, 1.03 g of diethanolamine, a solution formed by dissolving 3.28 g of hydroxyethylethylenediamine in 50 g of water, and a solution formed by dissolving 1.75 g of silane V in 17.5 g of acetone were added to the acetone solution containing the prepolymer and stirred vigorously. The mixture was stirred for 30 min and then dispersed by adding 570 g of water. Acetone was separated by distillation for 7 hours. After the acetone content was less than 1.0 wt %, 40 g of Lucramul 1820 liquid and 12.5 g of a 5% aqueous solution of tetrasodium pyrophosphate were added respectively to obtain a composition having a solid component content of 49 wt % and an average particle size of 164 nm in the dispersed phase, a pH of 6.6, and a viscosity of 5432 mPa·s.
[0196] Composition 5
[0197] 542.8 g of polyester I and 4.5 g of polyether II were dehydrated at 110° C. and 80 mbar for 1 hour, and 2.3 g of 1,4-butanediol was added and cooled while stirring. 59.56 g of isocyanate I and 3.78 g of isocyanate II were added at 60° C. and stirred at 80-90° C. until an isocyanate content of 1.3% was reached. Then, the mixture was dissolved in 930 g of acetone and cooled to 50° C. to obtain a reaction solution. 11.5 g of sodium salt of N-(2-aminoethyl)-2-aminoethanesulfonic acid, a solution formed by dissolving 2.3 g of hydroxyethylethylenediamine in 50 g of water, and a solution formed by dissolving 1.25 g of silane V in 12.5 g of acetone were added to the acetone solution containing the prepolymer and stirred vigorously. Stirred for 30 min, and then the mixture was dispersed by adding 570 g of water. Acetone was separated by distillation for 3.5 hours. After the acetone content was less than 1.0 wt %, 40 g of Lucramul 1820 liquid and 12.5 g of a 5% aqueous solution of tetrasodium pyrophosphate were added respectively to obtain a composition having a solid component content of 50.2 wt % and an average particle size of 174 nm in the dispersed phase, a pH of 6.7, and a viscosity of 375 mPa·s.
[0198] Composition 6
[0199] The main composition was the same as composition 5, but disodium pyrophosphate was added in the last step instead of tetrasodium pyrophosphate. A composition was obtained having a solid component content of 50.0 wt % and an average particle size of 158 nm in the dispersed phase, a pH of 6.4, and a viscosity of 520 mPa·s.
[0200] Comparative composition 1
[0201] 548.4 g of polyester I and 5 g of polyether I were dehydrated at 110° C. and 80 mbar for 1 hour, and 2.3 g of 1,4-butanediol was added and cooled while stirring. 56.65 g of isocyanate I and 7.51 g of isocyanate II were added at 60° C. and stirred at 80-90° C. until an isocyanate content of 1.3% was reached. Then, the mixture was dissolved in 930 g of acetone and cooled to 50° C. to obtain a reaction solution. 11.5 g of sodium salt of N-(2-aminoethyl)-2-aminoethanesulfonic acid, a solution formed by dissolving 2.7 g of hydroxyethylethylenediamine in 50 g of water, and a solution formed by dissolving 2.17 g of silane IV in 21.7 g of acetone were added to the acetone solution containing the prepolymer and stirred vigorously. Stirred for 30 min, and then the mixture was dispersed by adding 570 g of water. Acetone was separated by distillation for 3.5 hours. After the acetone content was less than 1.0 wt %, 40 g of Lucramul 1820 liquid was added to obtain a comparative composition having a solid component content of 50.1 wt % and an average particle size of 162 nm in the dispersed phase, a pH of 6.8, and a viscosity of 1152 mPa·s.
[0202] Comparative composition 2
[0203] 548.4 g of polyester I and 5 g of polyether I were dehydrated at 110° C. and 80 mbar for 1 hour, and 2.3 g of 1,4-butanediol was added and cooled while stirring. 56.65 g of isocyanate I and 7.51 g of isocyanate II were added at 60° C. and stirred at 80-90° C. until an isocyanate content of 1.3% was reached. Then, the mixture was dissolved in 930 g of acetone and cooled to 50° C. to obtain a reaction solution. 11.5 g of sodium salt of N-(2-aminoethyl)-2-aminoethanesulfonic acid, a solution formed by dissolving 2.7 g of hydroxyethylethylenediamine in 50 g of water, and a solution formed by dissolving 1.60 g of silane III in 16.0 g of acetone were added to the acetone solution containing the prepolymer and stirred vigorously. Stirred for 30 minutes, and then the mixture was dispersed by adding 570 g of water. Acetone was separated by distillation for 3.5 hours. After the acetone content was less than 1.0 wt %, 40 g of Lucramul 1820 liquid was added to obtain a comparative composition having a solid component content of 49.7 wt % and an average particle size of 162 nm in the dispersed phase, a pH of 6.7, and a viscosity of 1280 mPa·s.
[0204] Comparative composition 3
[0205] 534.4 g of polyester I and 12.5 g of polyether I were dehydrated at 110° C. and 80 mbar for 1 hour, and 2.3 g of 1,4-butanediol was added and cooled while stirring. 56.38 g of isocyanate I and 7.9 g of isocyanate II were added at 60° C. and stirred at 80-90° C. until an isocyanate content of 1.3% was reached. Then, the mixture was dissolved in 930 g of acetone and cooled to 50° C. to obtain a reaction solution. 11.6 g of sodium salt of N-(2-aminoethyl)-2-aminoethanesulfonic acid, a solution formed by dissolving 1.9 g of hydroxyethylethylenediamine in 50 g of water, and a solution formed by dissolving 1.25 g of silane V in 12.5 g of acetone were added to the acetone solution containing the prepolymer and stirred vigorously. Stirred for 30 min, and then the mixture was dispersed by adding 570 g of water. Acetone was separated by distillation for 5 hours. After the acetone content was less than 1.0 wt %, 40 g of Lucramul 1820 liquid was added to obtain a comparative composition having a solid component content of 50 wt % and an average particle size of 163 nm in the dispersed phase, a pH of 6.6, and a viscosity of 2800 mPa·s.
[0206] Comparative composition 4
[0207] 503.4 g of polyester I and 25 g of polyether I were dehydrated at 110° C. and 80 mbar for 1 hour, and 2.3 g of 1,4-butanediol was added and cooled while stirring. 60.62 g of isocyanate I and 8.04 g of isocyanate II were added at 60° C. and stirred at 80-90° C. until an isocyanate content of 1.7% was reached. Then, the mixture was dissolved in 930 g of acetone and cooled to 50° C. to obtain a reaction solution. 12.0 g of sodium salt of N-(2-aminoethyl)-2-aminoethanesulfonic acid, a solution formed by dissolving 3.75 g of hydroxyethylethylenediamine in 50 g of water, and a solution formed by dissolving 1.75 g of silane V in 17.5 g of acetone were added to the acetone solution containing the prepolymer and stirred vigorously. The mixture was stirred for 30 min and then dispersed by adding 570 g of water. Acetone was separated by distillation for 7 hours. After the acetone content was less than 1.0 wt %, 40 g of Lucramul 1820 liquid was added to obtain a comparative composition having a solid component content of 49 wt % and an average particle size of 164 nm in the dispersed phase, a pH of 6.8, and a viscosity of 10400 mPa·s.
[0208] Comparative composition 5
[0209] 506.3 g of polyester I was dehydrated at 110° C. and 80 mbar for 1 hour, and 2.3 g of 1,4-butanediol was added and cooled while stirring. 58.87 g of isocyanate I and 3.27 g of isocyanate II were added at 60° C. and stirred at 80-90° C. until an isocyanate content of 1.7% was reached. Then, it was dissolved in 930 g of acetone and cooled to 50° C. to obtain a reaction solution. 12.6 g of sodium salt of N-(2-aminoethyl)-2-aminoethanesulfonic acid, a solution formed by dissolving 3.41 g of hydroxyethylethylenediamine in 50 g of water, and a solution formed by dissolving 1.17 g of silane V in 11.7 g of acetone were added to the acetone solution in which the prepolymer was dissolved and stirred vigorously. Stirred for 30 minutes, and then the mixture was dispersed by adding 570 g of water. Acetone was separated by distillation for 3.5 hours. After the acetone content was less than 1.0 wt %, 33.3 g of Lucramul 1820 liquid and 11.6 g of a 5% aqueous solution of tetrasodium pyrophosphate were added respectively to obtain a comparative composition having a solid content of 50.3 wt % and an average particle size of 179 nm in the dispersed phase, a pH of 6.7, and a viscosity of 312 mPa·s.
[0210] Comparative composition 6
[0211] 543.4 g of polyester I and 1.9 g of polyether I were dehydrated at 110° C. and 80 mbar for 1 hour and then cooled. 61.5 g of isocyanate I and 5.11 g of isocyanate II were added at 60° C. and stirred at 80-90° C. until an isocyanate content of 1.8% was reached. Then, the mixture was dissolved in 930 g of acetone and cooled to 50° C. to obtain a reaction solution. 12.0 g of sodium salt of N-(2-aminoethyl)-2-aminoethanesulfonic acid, 7.08 g of isophoronediamine, a solution formed by dissolving 2.0 g of hydroxyethylethylenediamine in 78.92 g of water, and a solution formed by dissolving 1.86 g of silane V in 18.6 g of acetone were added to the acetone solution containing the prepolymer while stirring vigorously. Stirring was continued for 30 min, and then the mixture was dispersed by adding 542 g of water. Acetone was separated by distillation for 3 hours. After the acetone content was less than 1.0 wt %, 40 g of Lucramul 1820 liquid and 12.5 g of a 5% aqueous solution of tetrasodium pyrophosphate were added respectively to obtain a comparative composition having a solid component content of 52.5 wt % and an average particle size of 224 nm in the dispersed phase, a pH of 6.6, and a viscosity of 85 mPa·s.
[0212] Comparative composition 7
[0213] 547.2 g of polyester I and 3.9 g of polyether I were dehydrated at 110° C. and 80 mbar for 1 hour, and 0.8 g of 1,4-butanediol was added and cooled while stirring. 59.1 g of isocyanate I and 5.94 g of isocyanate II were added at 60° C. and stirred at 80-90° C. until an isocyanate content of 1.67% was reached. Then, the mixture was dissolved in 930 g of acetone and cooled to 50° C. to obtain a reaction solution. 12.0 g of sodium salt of N-(2-aminoethyl)-2-aminoethanesulfonic acid, 2.98 g of isophoronediamine, a solution formed by dissolving 1.0 g of hydroxyethylethylenediamine in 50 g of water, and a solution formed by dissolving 1.70 g of silane V in 17.0 g of acetone were added to the acetone solution in which the prepolymer was dissolved and stirred vigorously. The mixture was stirred for 30 minutes and then dispersed by adding 542 g of water. Acetone was separated by distillation for 3 hours. After the acetone content was less than 1.0 wt %, 40 g of Lucramul 1820 liquid and 12.5 g of a 5% aqueous solution of tetrasodium pyrophosphate were added respectively to obtain a comparative composition having a solid component content of 49.6 wt % and an average particle size of 181 nm in the dispersed phase, a pH of 6.5, and a viscosity of 85 mPa·s.
[0214] Comparative composition 8
[0215] 462.9 g of polyester I and 62.9 g of polyether I were dehydrated at 110° C. and 80 mbar for 1 hour, and 2.3 g of 1,4-butanediol was added and cooled while stirring. 62.41 g of isocyanate I and 13.6 g of isocyanate II were added at 60° C. and stirred at 80-90° C. until an isocyanate content of 1.9% was reached. Then, the mixture was dissolved in 930 g of acetone and cooled to 50° C. to obtain a reaction solution. 13.7 g of sodium salt of N-(2-aminoethyl)-2-aminoethanesulfonic acid, 7.44 g of isophoronediamine, a solution formed by dissolving 1.0 g of hydroxyethylethylenediamine in 50 g of water, and a solution formed by dissolving 1.23 g of silane II in 12.3 g of acetone were added to the acetone solution in which the prepolymer was dissolved and stirred vigorously. The mixture was stirred for 30 minutes and then dispersed by adding 1060 g of water. Acetone was separated by distillation for 7 hours. After the acetone content was less than 1.0 wt %, 40 g of Lucramul 1820 liquid and 12.5 g of a 5% aqueous solution of tetrasodium pyrophosphate were added respectively to obtain a comparative composition having a solid component content of 37.6 wt % and an average particle size of 155 nm in the dispersed phase, a pH value of 7.3, and a viscosity of 8416 mPa·s.
[0216] Comparative composition 9
[0217] 506.8 g of polyester I, 18.9 g of polyester II and 18.7 g of polyether I were dehydrated at 110° C. and 80 mbar for 1 hour, and 2.3 g of 1,4-butanediol was added and cooled while stirring. 65.17 g of isocyanate I and 4.17 g of isocyanate II were added at 60° C., and stirred at 80-90° C. until an isocyanate content of 1.7% was reached. Then, it was dissolved in 890 g of acetone and cooled to 50° C. to obtain a reaction solution. A solution of 13.2 g of sodium salt of N-(2-aminoethyl)-2-aminoethanesulfonic acid, 5.05 g of isophoronediamine, and 1.6 g of hydroxyethylethylenediamine dissolved in 60 g of water was added to the acetone solution in which the prepolymer was dissolved while stirring vigorously. Stirring was continued for 30 minutes, and then the mixture was dispersed by adding 550 g of water. Acetone was separated by distillation for 4 hours. After the acetone content was less than 1.0 wt %, 40 g of Lucramul 1820 liquid and 12.5 g of a 5% aqueous solution of tetrasodium pyrophosphate were added respectively to obtain a comparative composition having a solid component content of 50.8 wt % and an average particle size of 175 nm in the dispersed phase, a pH of 6.7, and a viscosity of 712 mPa·s.
[0218] Comparative composition 10
[0219] 542.8 g of polyester I and 7.5 g of polyether I were dehydrated at 110° C. and 80 mbar for 1 hour, and 2.3 g of 1,4-butanediol was added and cooled while stirring. 62.35 g of isocyanate I was added at 60° C. and stirred at 80-90° C. until an isocyanate content of 1.9% was reached. Then it was dissolved in 930 g of acetone and cooled to 50° C. to obtain a reaction solution. 11.47 g of sodium salt of N-(2-aminoethyl)-2-aminoethanesulfonic acid, a solution formed by dissolving 2.95 g of hydroxyethylethylenediamine in 50 g of water, and a solution formed by dissolving 0.77 g of silane III in 7.7 g of acetone were added to the acetone solution containing the prepolymer and stirred vigorously. Stirred for 30 minutes, and then the mixture was dispersed by adding 570 g of water. Acetone was separated by distillation for 4 hours. After the acetone content was less than 1.0 wt %, 40 g of Lucramul 1820 liquid and 12.5 g of a 5% aqueous solution of tetrasodium pyrophosphate were added respectively to obtain a comparative composition having a solid component content of 50.3 wt % and an average particle size of 165 nm in the dispersed phase, a pH value of 7.1, and a viscosity of 640 mPa·s.
[0220] Comparative composition 11
[0221] 421.9 g of polyester I, 170 g of polyester II and 11.36 g of polyether I were dehydrated at 110° C. and 80 mbar for 1 hour, then cooled, 71.25 g of isocyanate I was added at 60° C., and stirred at 80-90° C. until the isocyanate content reached 1.4%. Then, it was dissolved in 1100 g of acetone and cooled to 50° C. to obtain a reaction solution. 9.64 g of sodium salt of N-(2-aminoethyl)-2-aminoethanesulfonic acid, a solution formed by dissolving 4.2 g of isophorone diamine and 1.0 g of hydroxyethylethylenediamine in 50 g of water, and a solution formed by dissolving 4.83 g of silane V in 48.3 g of acetone were added to the acetone solution containing the prepolymer while stirring vigorously. Stirring was continued for 30 minutes, and then the mixture was dispersed by adding 534 g of water. Acetone was separated by distillation for 3.5 hours. After the acetone content was less than 1.0 wt %, 40 g of Lucramul 1820 liquid and 13.8 g of a 5% aqueous solution of tetrasodium pyrophosphate were added respectively to obtain a comparative composition having a solid component content of 55.6 wt % and an average particle size of 235 nm in the dispersed phase, a pH of 7.0, and a viscosity of 190 mPa.s.
[0222] Comparative composition 12
[0223] 542.8 g of polyester I and 12.6 g of polyether III were dehydrated at 110° C. and 80 mbar for 1 hour, and 2.3 g of 1,4-butanediol was added and cooled while stirring. 62.35 g of isocyanate I was added at 60° C. and stirred at 80-90° C. until an isocyanate content of 1.3% was reached. Then, it was dissolved in 930 g of acetone and cooled to 50° C. to obtain a reaction solution. 11.47 g of sodium salt of N-(2-aminoethyl)-2-aminoethanesulfonic acid, a solution formed by dissolving 2.81 g of hydroxyethylethylenediamine in 50 g of water, and a solution formed by dissolving 1.26 g of silane V in 12.6 g of acetone were added to the acetone solution in which the prepolymer was dissolved, respectively, while stirring vigorously. Stirring was continued for 30 min, and then the mixture was dispersed by adding 570 g of water. Acetone was separated by distillation for 6 hours. After the acetone content was less than 1.0 wt %, 40 g of Lucramul 1820 liquid and 12.5 g of a 5% aqueous solution of tetrasodium pyrophosphate were added respectively to obtain a comparative composition having a solid component content of 50.5 wt % and an average particle size of 134 nm in the dispersed phase, a pH of 6.7, and a viscosity of 2403 mPa·s.
[0224] Comparative composition 13
[0225] 542.8 g of polyester I and 12.6 g of polyether III were dehydrated at 110° C. and 80 mbar for 1 hour, and 2.3 g of 1,4-butanediol was added and cooled while stirring. 62.35 g of isocyanate I was added at 60° C. and stirred at 80-90° C. until an isocyanate content of 1.3% was reached. Then it was dissolved in 930 g of acetone and cooled to 50° C. to obtain a reaction solution. 11.47 g of sodium salt of N-(2-aminoethyl)-2-aminoethanesulfonic acid, a solution formed by dissolving 2.81 g of hydroxyethylethylenediamine in 50 g of water, and a solution formed by dissolving 1.54 g of silane IV in 15.4 g of acetone were added to the acetone solution in which the prepolymer was dissolved and stirred vigorously. Stirred for 30 minutes, and then the mixture was dispersed by adding 570 g of water. Acetone was separated by distillation for 5 hours. After the acetone content was less than 1.0 wt %, 40 g of Lucramul 1820 liquid and 12.5 g of a 5% aqueous solution of tetrasodium pyrophosphate were added respectively to obtain a comparative composition having a solid component content of 50.5 wt % and an average particle size of 162 nm in the dispersed phase, a pH of 6.9, and a viscosity of 1200 mPa·s.
[0226] Comparative composition 14
[0227] 548.4 g of polyester I and 5 g of polyether I were dehydrated at 110° C. and 80 mbar for 1 hour, and 2.3 g of 1,4-butanediol was added and cooled while stirring. 62.35 g of isocyanate I was added at 60° C. and stirred at 80-90° C. until an isocyanate content of 1.3% was reached. Then it was dissolved in 930 g of acetone and cooled to 50° C. to obtain a reaction solution. 11.47 g of sodium salt of N-(2-aminoethyl)-2-aminoethanesulfonic acid, 1.87 g of hydroxyethylethylenediamine, 1.26 g of diethanolamine dissolved in 50 g of water, and 1.17 g of silane I dissolved in 11.7 g of acetone were added to the acetone solution containing the prepolymer while stirring vigorously. Stirring was continued for 30 min, and then the mixture was dispersed by adding 570 g of water. Acetone was separated by distillation for 4 hours. After the acetone content was less than 1.0 wt %, 40 g of Lucramul 1820 liquid and 12.5 g of a 5% aqueous solution of tetrasodium pyrophosphate were added respectively to obtain a comparative composition having a solid component content of 49.7 wt % and an average particle size of 152 nm in the dispersed phase, a pH of 6.9, and a viscosity of 542 mPa·s.
[0228] Preparation methods of adhesives of Examples and Comparative Examples
[0229] According to the components shown in Table 1 and Table 2, 1.0 g of DESMODUR 2802 and 0.7 g of BorchiL Gel L75N were sequentially added to 100 g of the composition (the composition was previously left to mature at room temperature for 7 days) at 600 rpm while stirring, and then stirred at 1200 rpm for 10 to 15 minutes to mix well, and the viscosity was adjusted to 5000 mPa·s to 10000 mPa·s for use.
[0230] Hydrolysis resistance test
[0231] After mechanically polishing the substrate 1 (black rubber) and the substrate 2 (black rubber) with a length of 120 mm and a width of 20 mm, a rubber treatment agent (a rubber treatment agent obtained by dissolving trichloroisocyanuric acid (B powder) in ethyl acetate) was applied, and after drying, the adhesive of the present invention was applied to the substrate 1 and the substrate 2 using a brush, with the adhesive application area of 100 mm*20 mm. The substrate 1 and the substrate 2 were heated at 60°C for 3 minutes to dry and heat-activate the adhesive, and then the substrate 1 and the substrate 2 were bonded together for 10 seconds at a pressure of 4 bar, as shown in FIG. Figure 1 After the test strips were stored at room temperature (22±2°C, 50±5%RH) for 72 hours, a 1 kg weight was loaded on one end of the substrate. Figure 2As shown, the time required for the test strip to be completely detached is placed in an oven at 70°C and 95% humidity. If the time required for the test strip to be completely detached is not less than 6 hours, the hydrolysis resistance is qualified; if the time required for the test strip to be completely detached is less than 6 hours, the hydrolysis resistance is unqualified.
[0232] Hydrolysis resistance test of adhesive after storage at 40°C for two weeks
[0233] The test method is the same as the above hydrolysis resistance test, except that the adhesive is aged in an oven at 40°C for two weeks before the hydrolysis resistance test, and then taken out for the hydrolysis resistance test.
[0234] Low temperature film forming test
[0235] The compositions of the examples and comparative examples were left to stand and mature for 7 days at room temperature, and then a 200 micron wet film was scraped on a PP plate with a film scraper at room temperature (22±2°C, 50±5%RH), and the PP plate was immediately placed in a low-temperature oven at 10°C for at least 8 hours to be completely dried. The dry film was taken out to check whether it was cracked. If the dry film was not cracked, the low-temperature film-forming property was qualified, and if the dry film was cracked, the low-temperature film-forming property was unqualified.
[0236] Table 1 shows the evaluation results of hydrolysis resistance, hydrolysis resistance after heat storage and low temperature film forming property of the adhesives of Examples 1-5 of the present invention and Comparative Examples 1-4. Table 2 shows the evaluation results of hydrolysis resistance and low temperature film forming property of the adhesives of Comparative Examples 5-14 of the present invention.
[0237] Table 1 Evaluation of the adhesives of Examples 1-5 and Comparative Examples 1-4
[0238]
[0239] Note: The amounts of the compositions of the examples and comparative examples in Table 1 are all 100 g.
[0240] Table 2 Evaluation of the adhesives of comparative examples 5-14
[0241]
[0242] Note: The amounts of the compositions of the comparative examples in Table 2 are all 100 g.
[0243] The adhesive comprising the composition of Examples 1 to 5 of the present patent application has good hydrolysis resistance, hydrolysis resistance after heat storage and low-temperature film forming property.
[0244] Comparing Examples 1-4 and Comparative Examples 1-4, when the composition does not include a chelating agent, the adhesive including the composition has poor hydrolysis resistance after heat storage.
[0245] Comparative Examples 1-4 and Comparative Examples 5-7, when the composition does not contain a polymer conforming to Formula I or contains a polymer conforming to Formula I in an amount of 0.3 wt % and 0.6 wt %, the adhesive containing the composition cannot take into account both hydrolysis resistance and low temperature film-forming properties.
[0246] Comparing Examples 1-4 and Comparative Examples 9-11, when the composition did not include the silane compound or included the silane compound in an amount of 0.12 wt % and 0.7 wt %, the adhesive including the composition had poor hydrolysis resistance.
[0247] It can be seen from Comparative Example 8 that when the amount of the polymer conforming to the structure of Formula I included in the composition is 10 wt %, the hydrolysis resistance of the adhesive including the composition is poor.
[0248] It can be seen from Comparative Examples 12-13 that when the composition includes a monofunctional polyether polyol, the adhesive including the composition has poor hydrolysis resistance.
[0249] Comparing Comparative Example 14 with Examples 2-3, when the composition only includes a difunctional silane compound and does not include a monofunctional silane compound, the hydrolysis resistance of the adhesive including the composition is very poor.
[0250] It is easy for a person skilled in the art to know that the present invention is not limited to the above-mentioned specific details, and the present invention can be implemented in other specific forms without departing from the spirit or main characteristics of the present invention. Therefore, the embodiments described should be regarded as illustrative rather than restrictive from any point of view, so that the scope of the present invention is indicated by the claims rather than the above description; and therefore any changes, as long as they fall within the meaning and scope of the equivalents of the claims, should be regarded as belonging to the present invention.
Claims
1. A composition comprising: (a) a polyurethane polyurea polymer, wherein the polyurethane polyurea polymer is obtained by reacting a system comprising the following components: (a1) a polyisocyanate; (a2) a polymer conforming to formula I: in, n is 10-75, R 1 is an alkyl group containing 1 to 10 carbon atoms, R 2 is a structure containing at least two isocyanate-reactive groups; (a3) a polyol different from component a2), said polyol having a hydroxyl functionality of 1.5 to 4; (a4) a silane compound comprising an isocyanate-reactive group and at least two methoxy and / or ethoxy groups attached to a silicon atom; (a5) a hydrophilic compound different from (a2) containing 2 to 3 isocyanate-reactive groups; and (a6) optionally a compound containing 1 to 3 amino groups and / or hydroxyl groups; The amount of the polymer conforming to the structure of formula I is 0.7 wt%-9 wt%, and the amount of the silane compound is 0.14 wt%-0.6 wt%, relative to the total weight of the polyurethane polyurea polymer; (b) a water-soluble chelating agent selected from the group consisting of edetate, tartrate, citrate, pyrophosphate, tripolyphosphate, hexametaphosphate and gluconate; and (c) Water.
2. The composition according to claim 1, It is characterized in that The polyisocyanate of component a1) has at least two isocyanate groups; further preferred isocyanates conforming to the following general formula: Y(NCO) 2 , wherein Y is selected from: a divalent aliphatic hydrocarbon group containing 4 to 12 carbon atoms, a divalent alicyclic hydrocarbon group containing 6 to 15 carbon atoms, a divalent aromatic hydrocarbon group containing 6 to 15 carbon atoms, or a divalent aromatic aliphatic hydrocarbon group containing 7 to 15 carbon atoms; and preferably one or more of the following: tetramethylene diisocyanate, pentamethylene diisocyanate, hexamethylene diisocyanate, dodecamethylene diisocyanate, 1,4-cyclohexane diisocyanate, isophorone diisocyanate, 4,4′-dicyclohexylmethane diisocyanate, 4, 4′-dicyclohexylpropane diisocyanate, 1,4-phenylene diisocyanate, 2,4-toluene diisocyanate, 2,6-toluene diisocyanate, 4,4′-diphenylmethane diisocyanate, 2,2′- and 2,4′-diphenylmethane diisocyanate, tetramethylxylyl diisocyanate and p-xylylene diisocyanate, most preferably a mixture of hexamethylene diisocyanate and isophorone diisocyanate, or a mixture of hexamethylene diisocyanate and 4,4′-dicyclohexylmethane diisocyanate.
3. The composition according to claim 1 or 2, It is characterized in that The at least two isocyanate-reactive groups of R2 are selected from at least two amino groups, at least two hydroxyl groups, or at least one amino group and at least one hydroxyl group.
4. A composition according to any one of claims 1 to 3, It is characterized in that The polymer conforming to the structure of formula I is one or more of the following: a polymer conforming to the structure of formula II and a polymer conforming to the structure of formula III, Wherein, in formula II, a is 10-75, and b is 0-50; in formula III, x is 10-75, and y is 1-50.
5. A composition according to any one of claims 1 to 4, It is characterized in that The number average molecular weight of the polymer of component a2) conforming to the structure of formula I is 500 g / mol-4000 g / mol, and the number average molecular weight is tested according to gel chromatography, using tetrahydrofuran as the mobile phase, and the molecular weight is calculated based on polystyrene as the standard, and components with a molecular weight of 200 or higher are selected for calculation and measured with a differential refractometer.
6. A composition according to any one of claims 1 to 5, It is characterized in that The functionality of the polymer of component a2) conforming to the structure of formula I is 2.
7. A composition according to any one of claims 1 to 6, It is characterized in that The polyol of component a3) which is different from component a2) is one or more of the following: diols with a number average molecular weight of 62-15000 and polyols with a number average molecular weight of 62-15000, more preferably one or more of the following: diols with a number average molecular weight of 62-5000 and triols with a number average molecular weight of 92-5000, most preferably one or more of the following: polyester polyols with a number average molecular weight of 500-2500 containing 1.5-3 hydroxyl groups, 500 containing 1.5-3 hydroxyl groups of polycarbonate polyol, number average molecular weight of 200-2500 containing 1.5-3 hydroxyl groups of polyether polyol, number average molecular weight of 250-2500 containing 1.5-3 hydroxyl groups of polylactone polyol and small molecule alcohol, the number average molecular weight is tested according to gel chromatography, tetrahydrofuran is used as the mobile phase, and the molecular weight is calculated based on polystyrene as the standard, and the components with a molecular weight of 200 or more are selected for calculation and measured with a differential refractometer.
8. A composition according to any one of claims 1 to 7, It is characterized in that The melting enthalpy of the polyol of component a3) which is different from component a2) is not less than 15 J / g, most preferably 25 J / g-100 J / g, obtained by DSC from 20°C to 100°C according to method A in DIN 65467, with a sample load of 10-20 mg and a heating rate of 20 K / min.
9. A composition according to any one of claims 1 to 8, It is characterized in that The silane compound of component a4) contains at least one amino group.
10. The composition according to any one of claims 1 to 9, It is characterized in that The component a4) silane compound is one or more of the following: N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane, N-β-(aminoethyl)-γ-aminopropyltriethoxysilane, N-(β-aminoethyl)-γ-aminopropylmethyldimethoxysilane, bis(3-triethoxysilylpropyl)amine, bis(3-trimethoxysilylpropyl)amine, (3-aminopropyl)trimethoxysilane, (3-aminopropyl)triethoxysilane, 3-aminopropyl(diethoxy)methylsilane and 3-aminopropylmethyldimethoxysilane; preferably Select one or more of the following: N-(β-aminoethyl)-γ-aminopropylmethyldimethoxysilane, bis(3-triethoxysilylpropyl)amine, bis(3-trimethoxysilylpropyl)amine, (3-aminopropyl)trimethoxysilane, (3-aminopropyl)triethoxysilane, 3-aminopropyl(diethoxy)methylsilane and 3-aminopropylmethyldimethoxysilane; most preferably one or more of the following: (3-aminopropyl)trimethoxysilane, (3-aminopropyl)triethoxysilane and 3-aminopropylmethyldimethoxysilane.
11. The composition according to any one of claims 1 to 10, It is characterized in that The component a5) hydrophilic compound containing 2 to 3 isocyanate-reactive groups is one or more of the following: N-(2-aminoethyl)-2-aminoethane sulfonate, dimethylol propionate and N-(2-aminoethyl)-2-aminoethane carboxylate.
12. A composition according to any one of claims 1 to 11, It is characterized in that The chelating agent b) is characterized in that its concentration is 4.3×10 -7 The pH value of the aqueous solution of 1 mol / g at a temperature of 23°C is in the range of 3-11, preferably in the range of 4-10, and most preferably in the range of 5-8.
13. A composition according to any one of claims 1 to 12, It is characterized in that The compound containing 1 to 3 amino and / or hydroxyl groups of component a6) is one or more of the following: aliphatic and / or alicyclic primary and / or secondary monoamines or diamines or triamines or amino alcohols, most preferably one or more of the following: isophoronediamine, N-(2-hydroxyethyl)ethylenediamine and diethanolamine.
14. A composition according to any one of claims 1 to 13, It is characterized in that The amount of the component a1) is 5% to 40% by weight, most preferably 8% to 20% by weight, relative to the total weight of the polyurethane polyurea.
15. The composition according to any one of claims 1 to 14, It is characterized in that The amount of the component a2) is 0.7% to 4% by weight, relative to the total weight of the polyurethane polyurea.
16. A composition according to any one of claims 1 to 15, It is characterized in that The amount of the component a3) is 5% to 94% by weight, most preferably 70% to 90% by weight, relative to the total weight of the polyurethane polyurea.
17. A composition according to any one of claims 1 to 16, It is characterized in that The amount of the component a4) is 0.18% to 0.4% by weight, relative to the total weight of the polyurethane polyurea.
18. A composition according to any one of claims 1 to 17, It is characterized in that The amount of the component a5) is 0.2% to 50% by weight, most preferably 1% to 5% by weight, relative to the total weight of the polyurethane polyurea.
19. The composition according to any one of claims 1 to 18, It is characterized in that The amount of component b) is 0.05 wt% to 0.5 wt%, most preferably 0.1 wt% to 0.2 wt%, relative to the total weight of the polyurethane polyurea.
20. The composition according to any one of claims 1 to 19, It is characterized in that The amount of the component a6) compound containing 1 to 3 amino groups and / or hydroxyl groups does not exceed 10% by weight, most preferably 0.5% to 3% by weight, relative to the total weight of the polyurethane polyurea.
21. A method for preparing the composition according to any one of claims 1 to 20, comprising the following steps: mixing the polyurethane polyurea polymer (a) or the components for preparing the polyurethane polyurea polymer, a chelating agent (b) and water (c) in any manner.
22. The preparation method according to claim 21, It is characterized in that The polyurethane polyurea polymer (a) and water (c) form an aqueous polyurethane polyurea dispersion, and then the chelating agent (c) is introduced to obtain the composition.
23. The preparation method according to claim 21 or 22, It is characterized in that The chelating agent (c) is added in the form of an aqueous solution.
24. A coating, adhesive or ink comprising the composition according to any one of claims 1 to 20.
25. The coating, adhesive or ink of claim 24, It is characterized in that The invention further comprises an additive, which is one or more of the following: an emulsifier, a light stabilizer, an antioxidant, a bactericide, a filler, an anti-settling agent, a defoaming agent, a wetting agent, a flow regulator, a reactive diluent, a plasticizer, a neutralizer, a catalyst, an auxiliary solvent, a thickener, a pigment, a dye, a matting agent and a tackifier.
26. Use of the composition according to any one of claims 1 to 20 for preparing a coated product, a bonded product or a printed product.
27. An article comprising a substrate prepared, coated, bonded, sealed or printed with the composition of any one of claims 1 to 20.