Water-based radix asparagi resin emulsion and preparation method thereof
By introducing imide structure and hydrophobic asparagus resin into the aqueous asparagus resin, combined with the emulsification method, the problems of insufficient water resistance and mechanical strength of the aqueous asparagus resin are solved, and better water resistance and heat resistance are achieved. Suitable for asparagus polyurea materials in harsh environments.
Patent Information
- Application Number
- CN202411368846.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-29
- Publication Date
- 2024-12-06
AI Technical Summary
The existing water-based asparagus resins are insufficient in water resistance and mechanical strength, and are not suitable for use in strict environments, and the hydrophilic polyether structure is prone to hydrolysis, resulting in poor heat resistance.
Using an aqueous asparagus resin emulsion, combining hydrophilic asparagus resin and hydrophobic asparagus resin, hydrophilic polyether is introduced through the imide structure to improve the side chain stability of the resin, and form a stable Emulsion, combined with isocyanate curing agent to improve water resistance and mechanical strength.
It significantly improves the water resistance, heat resistance and flexibility of asparagus polyurea materials, and has good stability, and is suitable for applications in harsh environments.
Smart Images

Figure BDA0005067013610000021 
Figure BDA0005067013610000022 
Figure BDA0005067013610000031
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of emulsions and relates to an aqueous asparagus resin emulsion and a preparation method thereof. Background Art
[0002] Asparagine resin, also known as aspartic acid ester resin, is generally obtained by Michael addition reaction of diethyl maleate and polyamine. It can be cured by adding isocyanate curing agent to form asparagine polyurea material, which is widely used in various applications such as coatings, seam beautifiers, protective coatings, etc. The ester group on the side chain of asparagine resin has good solvation effect and internal plasticization effect. Therefore, asparagine resin has the characteristics of high solid content and low viscosity. It has low viscosity without adding diluent and good construction performance. However, it also has the disadvantages of insufficient mechanical strength, easy hydrolysis of ester group and poor heat resistance. It is not suitable for some harsh environmental conditions. For example, asparagine polyurea coatings used for offshore bridge piers require asparagine polyurea to have good hydrolysis resistance.
[0003] Water-based coatings are environmentally friendly and safe, and are becoming a trend. Many researchers have also studied the preparation methods of water-based asparagine resins and disclosed some preparation processes. Generally, the alkyl group (such as ethyl) on the ester group is replaced by a hydrophilic polyether structure through an ester exchange reaction. However, due to the poor hydrolysis resistance of the ester group, the hydrophilic polyether structure falls off after the ester group is hydrolyzed, resulting in a weakening or failure of the hydrophilicity, which affects the use. Summary of the invention
[0004] In the prior art, water-based asparagine resin emulsion is prepared by generally grafting a hydrophilic structure onto an asparagine resin structure to prepare a self-emulsifying resin. However, due to the good hydrophilicity of such resin, the water resistance of the coating after cross-linking and curing will be biased. In order to solve the above technical problems, the present invention provides a water-based asparagine resin emulsion and a preparation method thereof.
[0005] The technical solution of the present invention is as follows:
[0006] An aqueous asparagine resin emulsion, the emulsion containing hydrophilic asparagine resin and hydrophobic asparagine resin;
[0007] The sum of the weight of the hydrophilic asparagine resin and the hydrophobic asparagine resin in the emulsion accounts for 5-60% by weight;
[0008] The water compatibility of the hydrophilic asparagine resin is 100-160 g water / 100 g resin;
[0009] The water compatibility test method is as follows: at 25°C, weigh 100 grams of the resin sample to be tested and place it in a colorless and transparent container, slowly and gradually add an appropriate amount of pure water while stirring, stir evenly, and then measure according to the method specified in GB 1721-2008 "Determination of Appearance and Transparency of Varnish, Clear Oil and Thinner", and record the weight of pure water added when the instrument measurement value reaches 82, which is the water compatibility;
[0010] The structure of the hydrophobic asparagine resin is shown in the following formula (1):
[0011]
[0012] Wherein, Z is selected from a divalent organic structure with an average molecular weight of 50-500 which is inert to react with isocyanate groups at 100° C. after removing two primary amino groups from the first divalent organic amine, and R1, R2, R3 and R4 are independently selected from C1-C4 alkyl groups.
[0013] Preferably, the weight ratio of the hydrophilic asparagine resin to the hydrophobic asparagine resin is 1:3-5:1.
[0014] Preferably, the hydrophilic asparagine resin has a structure as shown in the following formula (2):
[0015] PA-L-CH-L-PA(2)
[0016] Wherein, -CH- is a divalent hydrophilic aspartic acid ester structure, and L is an intermediate structure having a structure as shown in the following formula (3):
[0017]
[0018] Wherein, R5 is a divalent organic structure remaining after removing two isocyanate groups from a diisocyanate compound;
[0019] -PA is a monovalent asparagine resin structure, and -PA does not contain a hydrophilic group.
[0020] More preferably, the structure of -CH- is as shown in the following formula (4) or (5), or a combination of the structures shown in formula (4) and formula (5),
[0021]
[0022] wherein X is selected from a divalent organic structure having an average molecular weight of 50-500 which is inert to react with isocyanate groups at 100° C. after removing two primary amino groups from a second divalent organic amine, R6 and R7 are independently selected from C1-C4 alkyl groups, R8 is selected from a monovalent polyether structure which is remaining after removing primary amino groups from a first single-ended amino polyether, and the solubility of the first single-ended amino polyether in pure water at 25° C. is not less than 10 g / 100 g water,
[0023]
[0024] wherein Y is selected from a divalent organic structure having an average molecular weight of 50-500 which is inert to the isocyanate group at 100°C after removing two primary amino groups from the third divalent organic amine, and R9 and R 10 The monovalent polyether structure is independently selected from the monovalent polyether structure remaining after removing the primary amino group from the second single-ended amino polyether, and the solubility of the second single-ended amino polyether in pure water at 25° C. is not less than 10 g / 100 g water.
[0025] More preferably, the structure of -PA is as shown in the following formula (6):
[0026]
[0027] wherein Q is selected from a divalent organic structure having an average molecular weight of 50-500 which is inert to the isocyanate group at 100° C. after removing two primary amino groups from the fourth divalent organic amine, and R 11 , R 12 , R 13 and R 14 Independently selected from C1-C4 alkyl.
[0028] The method for preparing the aqueous asparagus resin emulsion described in any one of the above embodiments comprises the following steps:
[0029] The first asparagine resin is put into a four-necked flask, a catalyst is added in an amount of 0.1% to 0.5% by weight of the first asparagine resin, the temperature is raised to 90 to 150° C., a single-terminal amino polyether is added, and the reaction is carried out under negative pressure and dealcoholization is maintained until no bubbles are generated, thereby obtaining a first prepolymer;
[0030] The first prepolymer is mixed with a diisocyanate compound and reacted to obtain a second prepolymer terminated with a diisocyanate;
[0031] The second asparagus resin is added to the second prepolymer, mixed evenly, and pure water is added for emulsification, and reacted at 10-60° C. for 0.5-5 hours to obtain the aqueous asparagus resin emulsion.
[0032] Preferably, the molar ratio of the first asparagine resin to the single-terminated amine polyether is 1:1-2.
[0033] Preferably, the structure of the single-terminated amino polyether is as shown in the following formula (7):
[0034] NH2CH2CH2(OCH2CH2) m (OCH2CHCH3) n OR 15 (7)
[0035] Among them, R 15 Selected from H, C1-C8 alkyl, cycloalkyl or C6-C20 substituted cycloalkyl, m≥3, n≥0, mn≥3, m+n≤100.
[0036] Preferably, the molar ratio of the first prepolymer to the diisocyanate compound is 1:2-10.
[0037] Preferably, the molar ratio of the second prepolymer to the second aspart resin is 1:3-20.
[0038] The beneficial effects of the present invention are:
[0039] (1) The present invention introduces a hydrophilic polyether structure into the side chain of the asparagine resin through an imide structure. The imide structure has excellent hydrolysis resistance, heat resistance and other properties and excellent stability. Therefore, the hydrophilic polyether structure can be stably grafted onto the side chain of the asparagine resin.
[0040] (2) In the hydrophilic asparagine resin of the present invention, the side chain contains an imide structure, and at least the terminal group contains an ester group (or the side chain may also contain an ester group). The characteristics of the imide structure and the ester structure are combined, and the hydrolysis resistance and heat resistance of the asparagine resin can be improved while the asparagine resin structure will not have poor flexibility due to excessive rigidity.
[0041] (3) The present invention adopts the method of emulsifying hydrophobic asparagine resin with hydrophilic asparagine resin. The hydrophilicity of the asparagine polyurea material obtained after curing is worse than the hydrophilicity of the hydrophilic asparagine resin used alone. Therefore, the water resistance of the asparagine polyurea obtained after curing will be better. DETAILED DESCRIPTION
[0042] The technical solution of the present invention is further illustrated and described below through specific implementation methods.
[0043] In order to solve the problems of poor water resistance and low mechanical strength of water-based asparagine polyurea in the prior art, on the one hand, the present invention provides an aqueous asparagine resin emulsion, which contains hydrophilic asparagine resin and hydrophobic asparagine resin;
[0044] The sum of the weight of the hydrophilic asparagine resin and the hydrophobic asparagine resin in the emulsion accounts for 5-60% by weight;
[0045] The water compatibility of hydrophilic asparagine resin is 100-160g water / 100g resin;
[0046] The test method of water compatibility is as follows: at 25°C, weigh 100g of the resin sample to be tested and place it in a colorless and transparent container. Slowly add an appropriate amount of pure water while stirring, stir evenly, and then measure according to the method specified in GB 1721-2008 "Determination of Appearance and Transparency of Varnish, Clear Oil and Thinner". The weight of pure water added when the instrument measurement value reaches 82 is the water compatibility.
[0047] The structure of hydrophobic asparagine resin is shown in the following formula (1):
[0048]
[0049] Wherein, Z is selected from a divalent organic structure with an average molecular weight of 50-500 which is inert to react with isocyanate groups at 100° C. after removing two primary amino groups from the first divalent organic amine, and R1, R2, R3 and R4 are independently selected from C1-C4 alkyl groups.
[0050] In the present invention, an imide structure is grafted onto the side chain of the hydrophilic asparagine resin, and a hydrophilic polyether structure is grafted onto the imide structure. The imide structure has good stability and high rigidity, and can prevent the hydrophilic polyether structure from being hydrolyzed or falling off due to poor heat resistance, which affects its hydrophilicity and further causes the stability of the emulsion to deteriorate or fail, and can improve the mechanical strength and heat resistance of the asparagine resin. The hydrophobic asparagine resin contains an ester group, which can bring into play the good properties of the asparagine resin, such as weather resistance, impact resistance, good flexibility and the like.
[0051] The aqueous asparagine resin emulsion of the present invention combines the characteristics of hydrophilic asparagine resin and hydrophobic asparagine resin. The hydrophilic asparagine resin has good emulsification performance, and emulsifies the hydrophobic asparagine resin to form a stable emulsion. The asparagine polyurea obtained after curing with an isocyanate curing agent has good water resistance, heat resistance, flexibility, etc., and has good comprehensive performance. The first divalent organic amine is a hydrophobic divalent organic amine or the divalent organic structure remaining after removing two amino groups is a hydrophobic structure, which can be a divalent organic amine commonly used in asparagine resin, such as 4,4'-diaminodicyclohexylmethane, 3,3'-dimethyl-4,4'-diaminodicyclohexylmethane, 1,4-cyclohexanediamine, etc.
[0052] In the present invention, the weight proportion of the sum of the weight of the hydrophilic asparagine resin and the hydrophobic asparagine resin in the emulsion can be 5%, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, etc. or any value in between, without special restrictions. Preferably, the weight proportion of the sum of the weight of the hydrophilic asparagine resin and the hydrophobic asparagine resin in the emulsion is 20-60%.
[0053] In a preferred embodiment of the present invention, the weight ratio of the hydrophilic asparagine resin to the hydrophobic asparagine resin is 1:3-5:1. For example, the weight ratio of the hydrophilic asparagine resin to the hydrophobic asparagine resin can be any value or any value in between 1:3, 1:2, 1:1, 2:1, 3:1, 4:1, 5:1, etc., without any particular limitation. Considering the water resistance of the asparagine polyurea material obtained after emulsification and curing, the weight ratio of the hydrophilic asparagine resin to the hydrophobic asparagine resin is more preferably 1:3-1:1.
[0054] In a preferred embodiment of the present invention, the hydrophilic asparagine resin has a structure as shown in the following formula (2): PA-L-CH-L-PA (2)
[0055] Wherein, -CH- is a divalent hydrophilic aspartic acid ester structure, L is an intermediate structure connecting the -CH- structure and the -PA structure, and has a structure as shown in the following formula (3):
[0056]
[0057] Wherein, R5 is a divalent organic structure remaining after removing two isocyanate groups from a diisocyanate compound;
[0058] -PA is a monovalent asparagine resin structure, and -PA does not contain a hydrophilic group.
[0059] The above-mentioned -CH- is a divalent hydrophilic aspartic acid ester structure. On the basis of the asparagine resin structure (for example, as shown in the above formula (1)), part or all of the ester groups are converted into imide structures through an imidization reaction, and the hydrophilic polyether chain segment is grafted on the imide structure, which has good stability. -PA is a monovalent asparagine resin structure. For example, the structure can be as shown in the above formula (1). -PA is located at both ends of the hydrophilic asparagine resin, which can adjust the hydrophilicity and hydrophobicity of the hydrophilic asparagine resin, so that the hydrophilic asparagine resin has more stable emulsification properties and can better emulsify the hydrophobic asparagine resin of the present invention. The fact that -PA does not contain a hydrophilic group means that the -PA structure does not contain an ionic group (such as a carboxyl group, a sulfonic acid group, etc.), a hydrophilic polyether structure, and a high-polarity group containing active hydrogen such as a carboxyl group, a hydroxyl group, and an amino group.
[0060] In a more preferred embodiment of the present invention, the structure of -CH- is as shown in the following formula (4) or (5), or a combination of the structures shown in formula (4) and formula (5),
[0061]
[0062] wherein X is selected from a divalent organic structure having an average molecular weight of 50-500 which is inert to react with isocyanate groups at 100°C and which is left after two primary amino groups are removed from the second divalent organic amine; R6 and R7 are independently selected from C1-C4 alkyl groups; R8 is selected from a monovalent polyether structure which is left after primary amino groups are removed from the first single-terminated amino polyether; and the solubility of the first single-terminated amino polyether in pure water at 25°C is not less than 10 g / 100 g water;
[0063]
[0064] wherein Y is selected from a divalent organic structure having an average molecular weight of 50-500 which is inert to the isocyanate group at 100° C. after removing two primary amino groups from the third divalent organic amine; 10 The monovalent polyether structure is independently selected from the monovalent polyether structure remaining after removing the primary amino group from the second single-ended amino polyether, and the solubility of the second single-ended amino polyether in pure water at 25° C. is not less than 10 g / 100 g water.
[0065] In the present invention, the second dibasic organic amine and the third dibasic organic amine may be the same as the first dibasic organic amine, which may be a hydrophobic dibasic organic amine or the divalent organic structure remaining after removing two amino groups is a hydrophobic structure, and may be dibasic organic amines commonly used in asparagus resin, such as 4,4'-diaminodicyclohexylmethane, 3,3'-dimethyl-4,4'-diaminodicyclohexylmethane, 1,4-cyclohexanediamine, etc.
[0066] In the structure of -CH-, the ester group is located at the side chain of the hydrophilic asparagine resin. After the imidization reaction, part or all of the ester group is converted to an imide structure, and the hydrophilic polyether segment is directly connected to the N atom of the imide, with good stability, not easy to hydrolyze, and high heat resistance. Moreover, since the imide structure of the rigid structure is located at the side chain of the hydrophilic asparagine resin structure, the rigidity of the hydrophilic resin structure is less affected, but the heat resistance, water resistance, etc. of the asparagine resin can be significantly improved. At the same time, in combination with the hydrophobic asparagine resin, the asparagine polyurea obtained after the emulsion of the present invention is added with a curing agent for curing has good flexibility, mechanical strength, water resistance, heat resistance, etc.
[0067] In a more preferred embodiment of the present invention, the structure of -PA is as shown in the following formula (6):
[0068]
[0069] wherein Q is selected from a divalent organic structure having an average molecular weight of 50-500 which is inert to the isocyanate group at 100° C. after removing two primary amino groups from the fourth divalent organic amine, and R 11 , R 12 , R 13 and R 14 Independently selected from C1-C4 alkyl.
[0070] In the present invention, the fourth binary organic amine, such as the first binary organic amine, the second binary organic amine or the third binary organic amine, is a hydrophobic binary organic amine or the divalent organic structure remaining after removing two amino groups is a hydrophobic structure, which can be a commonly used binary organic amine of asparagine, such as 4,4'-diaminodicyclohexylmethane, 3,3'-dimethyl-4,4'-diaminodicyclohexylmethane, 1,4-cyclohexanediamine, etc. The asparagine structure is introduced into the two ends of the hydrophilic asparagine, the hydrophilic and hydrophobic properties of the hydrophilic asparagine can be adjusted, and the solvation and internal plasticization of the ester group can also be brought into play, so as to avoid the flexibility deviation of the asparagine polyurea obtained. And due to the emulsification of the hydrophilic asparagine, the hydrophobic asparagine is emulsified and wrapped by the hydrophilic asparagine, and the ester group is less exposed to the outside, avoiding direct contact with water, delaying the hydrolysis of the ester group, and improving hydrolysis resistance.
[0071] On the other hand, the present invention also provides a method for preparing the aqueous asparagus resin emulsion described in any one of the above embodiments, comprising the following steps:
[0072] The first asparagine resin is put into a four-necked flask, a catalyst is added in an amount of 0.1% to 0.5% by weight of the first asparagine resin, the temperature is raised to 90 to 150° C., a single-terminal amino polyether is added, and the reaction is carried out under negative pressure and dealcoholization is maintained until no bubbles are generated, thereby obtaining a first prepolymer;
[0073] The first prepolymer is mixed with a diisocyanate compound and reacted to obtain a second prepolymer terminated with a diisocyanate;
[0074] The second asparagus resin is added to the second prepolymer, mixed evenly, and pure water is added for emulsification. The mixture is reacted at 10-60° C. for 0.5-5 hours to obtain an aqueous asparagus resin emulsion.
[0075] In the present invention, the emulsion of the present invention can be obtained by the reaction of the above three steps, and can be carried out in the same reactor, so the production efficiency is high. The catalyst used can be C8-C8 fatty acid (such as lauric acid, stearic acid, etc.), benzotriazole, 1-hydroxybenzotriazole, etc.
[0076] In the present invention, the first asparagine resin and the single-terminal amino polyether react, and the ester group on the side chain of the first asparagine resin can be partially or completely converted into an imide structure, and a hydrophilic polyether segment is introduced into the side chain of the asparagine resin to give the asparagine resin good hydrophilicity. In a preferred embodiment of the present invention, the molar ratio of the first asparagine resin and the single-terminal amino polyether is 1:1-2. By adjusting the molar ratio of the first asparagine resin and the single-terminal amino polyether, the ratio of the ester group converted into the imide group and the ratio of the introduced hydrophilic polyether segment can be adjusted. For example, the molar ratio can be any value in 1:1, 1:1.1, 1:1.2, 1:1.3, 1:1.4, 1:1.5, 1:1.6, 1:1.7, 1:1.8, 1:1.9, 1:2, etc. or any value therebetween, without special restrictions.
[0077] In a preferred embodiment of the present invention, the structure of the single-terminated amino polyether is shown in the following formula (7):
[0078] NH2CH2CH2(OCH2CH2) m (OCH2CHCH3) n OR 15 (7)
[0079] Among them, R 15 Selected from H, C1-C8 alkyl, cycloalkyl or C6-C20 substituted cycloalkyl, m≥3, n≥0, mn≥3, m+n≤100.
[0080] In the present invention, the above-mentioned single-terminated amino polyether can be directly obtained from the market, such as ZM-1100 of Zibo Zhengda Polyurethane Co., Ltd., CAM-2070 of Yangzhou Chenhua New Materials Co., Ltd., or single-terminated amino polyethylene glycol, such as methoxy polyethylene glycol amine, number average molecular weight 400, 600, 800, 1000, etc. Using single-terminated amino polyether, the terminal amino group can react with the ester group to form an imide structure and introduce the polyether structure into the hydrophilic secondary amino resin of the present invention. In the present invention, R4 and R5 can be the same or different.
[0081] m and n represent the average degree of polymerization of -OCH2CH2- and -OCH2CHCH3-, respectively. If the values of m and n are too high, or the value of m+n is too high, the reactivity of the terminal amino group will be reduced, which may affect the reaction efficiency and reaction degree of the imide reaction.
[0082] In a preferred embodiment of the present invention, the molar ratio of the first prepolymer to the diisocyanate compound is 1:2-10. Using the above technical solution, the two -NH- groups in the first polymer will be converted into NCO groups. If the diisocyanate compound is excessive, the excess diisocyanate compound can be removed by methods such as reduced pressure distillation. For example, the molar ratio of the first prepolymer to the diisocyanate compound can be any value of 1:2, 1:2.2, 1:2.5, 1:3, 1:3.2, 1:3.5, 1:4, 1:4.5, 1:5, 1:6, 1:7, 1:8, 1:9, 1:10, etc., without special restrictions. More preferably, from the perspective of raw material utilization, the molar ratio of the first prepolymer to the diisocyanate compound can be 1:2-3. The diisocyanate compound is selected from aliphatic diisocyanates, which has better weather resistance and other properties. In a preferred embodiment of the present invention, the diisocyanate compound is selected from one or a combination of two or more of pentamethylene diisocyanate (PDI), hexamethylene diisocyanate (HMDI), 1,4-cyclohexyl diisocyanate, 2-methyl-1,4-cyclohexyl diisocyanate, isophorone diisocyanate (IPDI) and 4,4'-dicyclohexylmethane diisocyanate (H12MDI).
[0083] In a preferred embodiment of the present invention, the molar ratio of the second prepolymer to the second asparagine resin is 1:3-20. By adopting the above technical solution, both ends of the second prepolymer can be grafted with asparagine resin structures, and the excess second asparagine resin can be directly used as the hydrophobic asparagine resin in the emulsion. For example, the molar ratio of the second prepolymer to the second asparagine resin can be 1:3, 1:3.5, 1:4, 1:4.5, 1:5, 1:5.5, 1:6, 1:6.5, 1:7, 1:7.5, 1:8, 1:8.5, 1:9, 1:9.5, 1:10, 1:11, 1:12, 1:13, 1:14, 1:15, 1:16, 1:17, 1:18, 1:19, 1:20, etc., or any value in between, without special restrictions.
[0084] In the present invention, the first asparagine resin and the second asparagine resin are both conventional asparagine resins, which can be obtained by Michael addition reaction of diethyl maleate and a diamine compound (4,4'-diaminodicyclohexylmethane, 3,3'-dimethyl-4,4'-diaminodicyclohexylmethane, etc.), or can be directly purchased on the market, such as F420 resin, F520 resin, F220 resin, F421 resin, etc. of Feiyang Junyan Company, Desmophen NH 1420, NH 1520, etc. of Covestro Company.
[0085] The technical solution of the present invention is further described and illustrated according to various embodiments below. Unless otherwise specified, the parts described in the following embodiments are parts by weight.
[0086] Example 1
[0087] 1 mol of F420 resin and 0.2% of 1-hydroxybenzotriazole by weight of the F420 resin are added to a reaction container, the temperature is raised to 120° C., 1 mol of amino-terminated polyether ZM-1100 is added until reflux occurs in the reaction system, nitrogen is introduced to remove the generated ethanol until no bubbles are generated in the reaction system, and a first prepolymer is obtained; 2 mol of isophorone diisocyanate IPDI is continued to be added to the above reaction container, stirred at room temperature for 3 hours, heated to 60° C. and reacted for 1 hour to obtain a second prepolymer; 5 mol of F420 resin is continued to be added to the above reaction container, pure water is gradually added at a stirring speed of 1200 rpm to make a solid content of 40%, the speed is reduced to 600 rpm and stirred for 30 minutes after the addition, and the reaction is continued at 30° C. for 2 hours to obtain an aqueous asparagus resin emulsion.
[0088] Example 2
[0089] The difference between this embodiment and embodiment 1 is that the amino-terminated polyether ZM-1100 is adjusted from 1 mol to 1.5 mol. The other steps remain unchanged.
[0090] Example 3
[0091] The difference between this embodiment and embodiment 1 is that the amount of amino-terminated polyether ZM-1100 is adjusted from 1 mol to 2 mol. The other steps remain unchanged.
[0092] Example 4
[0093] The difference between this embodiment and embodiment 2 is that 5 mol of F420 resin is adjusted to 8 mol of F420 resin. The other steps remain unchanged.
[0094] Example 5
[0095] The difference between this embodiment and embodiment 2 is that 5 mol of F420 resin is adjusted to 18 mol of F420 resin. The other steps remain unchanged.
[0096] Example 6
[0097] The difference between this embodiment and embodiment 4 is that 18 mol of F420 resin is adjusted to 18 mol of F520 resin. The other steps remain unchanged.
[0098] Comparative Example 1
[0099] The hydrophilic polyaspartic acid ester resin and F420 resin were prepared by the method of Example 1 in the prior art CN111303368A and mixed in a weight ratio of 1:1. Pure water was gradually added at a stirring speed of 1200 rpm to make a solid content of 40%. After the addition, the speed was lowered to 600 rpm and stirred for 30 minutes to obtain an aqueous asparagine resin emulsion.
[0100] Comparative Example 2
[0101] Add 2 mol F420 resin and 0.2% by weight of F420 resin 1-hydroxybenzotriazole into a reaction container, heat to 120°C, add 1 mol of terminal amino polyether ZM-1100, until reflux occurs in the reaction system, introduce nitrogen to remove the generated ethanol until no bubbles are generated in the reaction system, cool to room temperature, gradually add pure water at a stirring speed of 1200 rpm to make a solid content of 40%, reduce the speed to 600 rpm and stir for 30 minutes after the addition, to obtain an aqueous asparagus resin emulsion.
[0102] Performance Testing
[0103] Storage stability of emulsion: Take 100g of the emulsion to be tested and add it into a 200ml transparent plastic bottle, seal it, and place it at 25℃. Observe the time when abnormalities such as precipitation, stratification, and oil floating appear, which is the storage time.
[0104] The emulsion to be tested and the water-based isocyanate curing agent Huntsman 9236 were mixed evenly at a secondary amine to isocyanate molar ratio of 1:1.05 to obtain a coating composition, which was formed into a film on a clean glass surface, heated and cured, with a film thickness of 0.3 mm, and placed at 25°C and 55% humidity for 24 hours. The tensile strength, heat deformation temperature, flexibility and water resistance of the film were tested.
[0105] Tensile strength: tested using an electronic tensile testing machine.
[0106] Heat deformation temperature: measured according to the method of GB / T1634-2019.
[0107] Flexibility: measured according to the method of GB / T 1731-2020.
[0108] Water resistance: Tested according to the method of GB / T1733-1993, the substrate is clean tinplate, and the paint film is observed every 1 hour to see if there are any problems such as bubbling, warping, and falling off. The time when the paint film shows the above problems is the water resistance time. The longer the water resistance time, the better the water resistance.
[0109] The results are shown in Table 1 below.
[0110] Table 1
[0111]
[0112]
[0113] Example 7
[0114] 1 mol F420 resin and 0.3% of 1-hydroxybenzotriazole by weight of the F420 resin were added to a reaction container, the temperature was raised to 125° C., 1.3 mol of amino-terminated polyether CAM-2070 was added until reflux occurred in the reaction system, nitrogen was introduced to remove the generated ethanol until no bubbles were generated in the reaction system, and a first prepolymer was obtained; 2.5 mol H12MDI was continuously added to the above reaction container, stirred at room temperature for 3 hours, the temperature was raised to 160° C., the pressure was reduced to below -0.099 MPa to remove low-boiling substances, and a second prepolymer was obtained; 10 mol F420 resin was continuously added to the above reaction container, pure water was gradually added at a stirring speed of 1300 rpm to make a solid content of 35%, after the addition, the speed was reduced to 600 rpm and stirred for 30 minutes, and the reaction was continued at 30° C. for 3 hours to obtain an aqueous asparagus resin emulsion.
[0115] Example 8
[0116] The difference between this example and example 7 is that the amino-terminated polyether CAM-2070 is replaced by an equal mole of methoxy-terminated amino-terminated polyethylene glycol (average degree of polymerization 25). The other steps remain unchanged.
[0117] Example 9
[0118] The difference between this example and example 7 is that the amino-terminated polyether CAM-2070 is replaced by an equal mole of isooctyl-terminated amino-terminated polyethylene glycol (average degree of polymerization 25). The other steps remain unchanged.
[0119] The performance test results are shown in Table 2 below.
[0120] Table 2
[0121]
[0122]
[0123] Combining the data in Table 1 and Table 2, it can be seen that the water-based asparagus resin emulsion of the present invention has good storage properties, tensile strength, heat deformation temperature and flexibility, and good water resistance.
[0124] As described above, the basic principles, main features and advantages of the present invention are shown and described. Those skilled in the art should understand that the present invention is not limited by the above embodiments, which are only preferred embodiments of the present invention and cannot be used to limit the scope of the present invention. That is, equivalent changes and modifications made according to the scope of the present invention and the content of the specification should still be within the scope of the present invention. The scope of protection required by the present invention is defined by the attached claims and their equivalents.
Claims
1. An aqueous asparagus resin emulsion, characterized in that The emulsion contains hydrophilic asparagine resin and hydrophobic asparagine resin; The sum of the weight of the hydrophilic asparagine resin and the hydrophobic asparagine resin in the emulsion accounts for 5-60% by weight; The water compatibility of the hydrophilic asparagine resin is 100-160 g water / 100 g resin; The water compatibility test method is as follows: at 25°C, weigh 100 grams of the resin sample to be tested and place it in a colorless and transparent container, slowly and gradually add an appropriate amount of pure water while stirring, stir evenly, and then measure according to the method specified in GB 1721-2008 "Determination of Appearance and Transparency of Varnish, Clear Oil and Thinner", and record the weight of pure water added when the instrument measurement value reaches 82, which is the water compatibility; The structure of the hydrophobic asparagine resin is shown in the following formula (1): Wherein, Z is selected from a divalent organic structure with an average molecular weight of 50-500 which is inert to react with isocyanate groups at 100° C. after removing two primary amino groups from the first divalent organic amine, and R1, R2, R3 and R4 are independently selected from C1-C4 alkyl groups.
2. The aqueous asparagus resin emulsion according to claim 1, characterized in that The weight ratio of the hydrophilic asparagine resin to the hydrophobic asparagine resin is 1:3-5:
1.
3. The aqueous asparagus resin emulsion according to claim 1, characterized in that The hydrophilic asparagine resin has a structure as shown in the following formula (2): PA-L-CH-L-PA(2) Wherein, -CH- is a divalent hydrophilic aspartic acid ester structure, and L is an intermediate structure having a structure as shown in the following formula (3): Wherein, R5 is a divalent organic structure remaining after removing two isocyanate groups from a diisocyanate compound; -PA is a monovalent asparagine resin structure, and -PA does not contain a hydrophilic group.
4. The aqueous asparagus resin emulsion according to claim 3, characterized in that The structure of the -CH- is as shown in the following formula (4) or (5), or a combination of the structures shown in formula (4) and formula (5), wherein X is selected from a divalent organic structure having an average molecular weight of 50-500 which is inert to react with isocyanate groups at 100° C. after removing two primary amino groups from a second divalent organic amine, R6 and R7 are independently selected from C1-C4 alkyl groups, R8 is selected from a monovalent polyether structure which is remaining after removing primary amino groups from a first single-ended amino polyether, and the solubility of the first single-ended amino polyether in pure water at 25° C. is not less than 10 g / 100 g water, wherein Y is selected from a divalent organic structure having an average molecular weight of 50-500 which is inert to the isocyanate group at 100°C after removing two primary amino groups from the third divalent organic amine, and R9 and R 10 The monovalent polyether structure is independently selected from the monovalent polyether structure remaining after removing the primary amino group from the second single-ended amino polyether, and the solubility of the second single-ended amino polyether in pure water at 25° C. is not less than 10 g / 100 g water.
5. The aqueous asparagus resin emulsion according to claim 3, characterized in that The structure of -PA is as shown in the following formula (6): wherein Q is selected from a divalent organic structure having an average molecular weight of 50-500 which is inert to the isocyanate group at 100° C. after removing two primary amino groups from the fourth divalent organic amine, and R 11 , R 12 , R 13 and R 14 Independently selected from C1-C4 alkyl.
6. The method for preparing the aqueous asparagus resin emulsion according to any one of claims 1 to 5, characterized in that: The following steps are involved: The first asparagine resin is put into a four-necked flask, a catalyst is added in an amount of 0.1% to 0.5% by weight of the first asparagine resin, the temperature is raised to 90 to 150° C., a single-terminal amino polyether is added, and the reaction is carried out under negative pressure and dealcoholization is maintained until no bubbles are generated, thereby obtaining a first prepolymer; The first prepolymer is mixed with a diisocyanate compound and reacted to obtain a second prepolymer terminated with a diisocyanate; The second asparagus resin is added to the second prepolymer, mixed evenly, and pure water is added for emulsification, and reacted at 10-60° C. for 0.5-5 hours to obtain the aqueous asparagus resin emulsion.
7. The method for preparing the aqueous asparagus resin emulsion according to claim 6, characterized in that: The molar ratio of the first asparagine resin to the single-terminated amine-based polyether is 1:1-2.
8. The method for preparing the aqueous asparagus resin emulsion according to claim 6, characterized in that: The structure of the single-terminated amino polyether is shown in the following formula (7): NH2CH2CH2(OCH2CH2) m (OCH2CHCH3) n OR 15 (7) Among them, R 15 Selected from H, C1-C8 alkyl, cycloalkyl or C6-C20 substituted cycloalkyl, m≥3, n≥0, mn≥3, m+n≤100.
9. The method for preparing the aqueous asparagus resin emulsion according to claim 6, characterized in that: The molar ratio of the first prepolymer to the diisocyanate compound is 1:2-10.
10. The method for preparing the aqueous asparagus resin emulsion according to claim 6, characterized in that: The molar ratio of the second prepolymer to the second aspart resin is 1:3-20.